Solid electrolyte material and battery using same
By using solid electrolyte materials with Li, M, A and X with low Young's modulus, the electrode structure factor and ion conductivity are improved, the problem of high battery resistance is solved, and stable work in a temperature-changing environment is achieved .
Patent Information
- Application Number
- CN202280093020.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-11
- Filing Date
- 2022-11-14
- Publication Date
- 2024-11-15
AI Technical Summary
It is difficult for the existing solid electrolyte materials to efficiently exert the ion conductivity of the material itself when forming electrodes, resulting in a low electrode structure factor, which in turn increases the resistance of the battery.
A solid electrolyte material containing Li, M, A and X is used, where M is an element in Nb, Ta and Zr, A is an element in O and S, X is an element in F, Cl, Br and I, with low Young's modulus at 23 GPa to improve electrode structural factor and ion conductivity.
By reducing the porosity of the solid electrolyte material in the electrode and increasing the torsion, the effective ion conductivity of the electrode is significantly improved, the resistance of the battery is reduced, and the high lithium ion conductivity is maintained in a temperature-changing environment.
Smart Images

Figure CN118974843A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a solid electrolyte material and a battery using the same. Background Art
[0002] Patent Document 1 discloses a solid electrolyte material containing Li, M, O, and X. M is at least one element selected from Nb and Ta, and X is at least one element selected from Cl, Br, and I.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: International Publication No. 2020 / 137153 Summary of the invention
[0006] Problems to be solved by the invention
[0007] An object of the present disclosure is to provide a solid electrolyte material which, when forming an electrode, can efficiently exert the ion conductivity of the material itself as the ion conductivity of the electrode.
[0008] Means for solving problems
[0009] The present disclosure relates to a solid electrolyte material, which is a solid electrolyte material comprising Li, M, A and X, wherein:
[0010] M is at least one selected from Nb, Ta and Zr,
[0011] A is at least one selected from O and S,
[0012] X is at least one selected from F, Cl, Br and I,
[0013] The solid electrolyte material has a Young's modulus below 23 GPa.
[0014] Effects of the Invention
[0015] The present disclosure provides a solid electrolyte material which can efficiently exert the ion conductivity of the material itself as the ion conductivity of the electrode when forming an electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 A cross-sectional view showing a battery 1000 according to a second embodiment.
[0017] Figure 2 A cross-sectional view showing an electrode material 1100 according to the second embodiment.
[0018] Figure 3A schematic diagram showing a press mold 300 for evaluating the ion conductivity of a solid electrolyte material. DETAILED DESCRIPTION
[0019] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings.
[0020] (First embodiment)
[0021] The solid electrolyte material of the first embodiment includes Li, M, A and X. M is at least one selected from Nb, Ta and Zr. A is at least one selected from O and S. X is at least one selected from F, Cl, Br and I. The solid electrolyte material of the first embodiment has a Young's modulus lower than 23 GPa.
[0022] When the solid electrolyte material of the first embodiment is formed into an electrode, the ion conductivity of the material itself can be efficiently exerted as the ion conductivity of the electrode. In other words, the solid electrolyte material of the first embodiment can improve the electrode structure factor.
[0023] Here, the electrode structure factor is explained. In order to reduce the resistance of the battery, it is necessary to increase the ionic conductivity (i.e., effective ionic conductivity) of the positive electrode or the negative electrode. The effective ionic conductivity depends not only on the ionic conductivity of the solid electrolyte material used in the electrode, but also, for example, on (1) the tortuosity of the solid electrolyte material in the electrode, the porosity of the solid electrolyte material in the electrode (i.e., the density of the solid electrolyte material), and the grain boundaries of the solid electrolyte material in the electrode. In addition, the tortuosity is the ratio of the length of the ionic conduction path of the solid electrolyte material in the electrode to the thickness of the electrode. The above-mentioned factors related to the structure of the solid electrolyte material in the electrode are the electrode structure factors. In other words, in addition to depending on the ionic conductivity of the solid electrolyte material used, the effective ionic conductivity also depends on the electrode structure factor. The electrode structure factor can be evaluated by the ratio of the effective ionic conductivity of the solid electrolyte material to the ionic conductivity. In other words, the larger the electrode structure factor, the higher the effective ionic conductivity.
[0024] The solid electrolyte material of the first embodiment has a low Young's modulus of less than 23 GPa. Therefore, the solid electrolyte material of the first embodiment increases the tortuosity while reducing the porosity of the solid electrolyte material in the electrode. As a result, the electrode structure factor of the battery using the solid electrolyte material of the first embodiment becomes larger, and the effective ion conductivity is improved. Therefore, the battery using the solid electrolyte material of the first embodiment has a low battery resistance.
[0025] The Young's modulus of the solid electrolyte material of the first embodiment can be measured, for example, by nanoindentation. Specifically, a nanoindentation device is used to arbitrarily select three particles from the particulate solid electrolyte material to measure the Young's modulus. The particle size of the selected particles is, for example, specified in the range of 1 μm to 100 μm. The Young's modulus is obtained by calculating the average value of the obtained measured values. In addition, when it is difficult to measure the Young's modulus of the solid electrolyte material by nanoindentation (for example, particles with a particle size suitable for measurement cannot be selected), as an alternative method, for example, the solid electrolyte material can be formed into a pellet shape, and the pellet is used as a measurement sample to measure the Young's modulus.
[0026] The solid electrolyte material of the first embodiment can maintain high lithium ion conductivity within the assumed battery operating temperature range (e.g., within the range of -30°C to 80°C). Therefore, the battery using the solid electrolyte material of the first embodiment can operate stably even in an environment with temperature changes. The so-called high lithium ion conductivity within the assumed battery operating temperature range is, for example, 1 mS / cm or more.
[0027] In order to improve the ion conductivity of the solid electrolyte material, the solid electrolyte material of the first embodiment may be substantially composed of Li, M, A and X. Here, "the solid electrolyte material of the first embodiment is substantially composed of Li, M, A and X" means that the molar ratio of the total amount of Li, M, A and X constituting the solid electrolyte material of the first embodiment to the total amount of all elements is 90% or more. As an example, the molar ratio may be 95% or more.
[0028] The solid electrolyte material of the first embodiment may be composed of Li, M, A, and X only in order to improve the ion conductivity of the solid electrolyte material.
[0029] In order to improve the electrode structure factor, the solid electrolyte material of the first embodiment may have a Young's modulus of 20 GPa or less. In order to further improve the electrode structure factor, the solid electrolyte material of the first embodiment may have a Young's modulus of 19.6 GPa or less.
[0030] The lower limit value of the Young's modulus of the solid electrolyte material of the first embodiment is not particularly limited, and the Young's modulus of the solid electrolyte material of the first embodiment may be, for example, 5 GPa or more.
[0031] In order to improve the electrode structure factor, the solid electrolyte material of the first embodiment may have a Young's modulus of 10.8 GPa or more and 19.6 GPa or less.
[0032] In order to improve the ion conductivity of the solid electrolyte material, in the solid electrolyte material of the first embodiment, X may contain Cl. X may be Cl.
[0033] In order to improve the ion conductivity of the solid electrolyte material, in the solid electrolyte material of the first embodiment, A may contain O. A may also be O.
[0034] In order to further improve the ion conductivity of the solid electrolyte material, in the solid electrolyte material of the first embodiment, A may contain both O and S. That is, A may be O and S.
[0035] In order to improve the ion conductivity of the solid electrolyte material, the molar ratio of Li to M may be 0.60 to 3.0, or 0.90 to 2.0.
[0036] In order to improve the ion conductivity of the solid electrolyte material, the molar ratio of O to X may be 0.05 or more and 0.35 or less.
[0037] In order to improve the ion conductivity of the solid electrolyte material, A may contain S, and the molar ratio of S to M may be 0.1 to 0.7.
[0038] The shape of the solid electrolyte material of the first embodiment is not limited. Examples of the shape are needle-shaped, spherical, and ellipsoidal. The solid electrolyte material of the first embodiment may also be particles. The solid electrolyte material of the first embodiment may also be formed in a pellet or plate shape.
[0039] When the shape of the solid electrolyte material of the first embodiment is a particle (e.g., spherical), the solid electrolyte material may also have a median particle size of 0.1 μm or more and 100 μm or less, or a median particle size of 0.5 μm or more and 10 μm or less. Thus, the solid electrolyte material of the first embodiment and other materials can be well dispersed. The median particle size of the particle refers to the particle size (d50) when the cumulative volume in the volume-based particle size distribution is equivalent to 50%. The volume-based particle size distribution can be measured by a laser diffraction measurement device or an image analysis device.
[0040] When the solid electrolyte material of the first embodiment is in the form of particles (eg, spheres), the solid electrolyte material may have a smaller median diameter than the active material. Thus, the solid electrolyte material of the first embodiment and the active material can be in a well-dispersed state.
[0041] <Method for producing solid electrolyte material>
[0042] The solid electrolyte material of the first embodiment can be produced by the following method.
[0043] The raw material powder is prepared so as to have a target composition. Examples of the raw material powder are oxides, hydroxides, halides or acid halides.
[0044] As an example, in a solid electrolyte material composed of Li, M, A and X, M is Ta, A is O, and X is Cl. When the molar ratio Li / M and the molar ratio A / X when the raw materials are mixed are 1.0 and 0.2, respectively, LiOH and TaCl5 are mixed at a molar ratio of LiOH: TaCl5 = 1: 1. M and X are determined by selecting the raw material powder. By appropriately selecting the mixing ratio of the raw material powder, the molar ratios of Li / M and A / X can be adjusted.
[0045] The mixture of raw material powders is reacted with each other in a mechanochemical manner (ie, by a mechanochemical grinding method) in a mixing device such as a planetary ball mill to obtain a reactant.
[0046] By reducing the energy applied to the raw material powder in mechanochemical grinding, the Young's modulus of the solid electrolyte material to be obtained can be reduced. That is, by adjusting the energy applied to the raw material powder during synthesis, the Young's modulus of the solid electrolyte material to be obtained can be controlled within a desired range. The amount of energy applied to the raw material powder can be adjusted by the rotation speed during the grinding process, or the material or size of the pulverizing medium used.
[0047] The composition of the solid electrolyte material can be determined by, for example, ICP emission spectrometry, ion chromatography, inert gas fusion-infrared absorption, or EPMA (Electron Probe Micro Analyzer) method.
[0048] (Second embodiment)
[0049] Hereinafter, the second embodiment will be described, and matters described in the first embodiment will be appropriately omitted.
[0050] The battery of the second embodiment includes a positive electrode, an electrolyte layer, and a negative electrode. The electrolyte layer is disposed between the positive electrode and the negative electrode. At least one selected from the positive electrode, the electrolyte layer, and the negative electrode contains the solid electrolyte material of the first embodiment.
[0051] The battery of the second embodiment has excellent charge and discharge characteristics.
[0052] Figure 1 A cross-sectional view showing a battery 1000 according to a second embodiment.
[0053] The battery 1000 includes a positive electrode 201 , an electrolyte layer 202 , and a negative electrode 203 . The electrolyte layer 202 is disposed between the positive electrode 201 and the negative electrode 203 .
[0054] The positive electrode 201 includes positive electrode active material particles 204 and solid electrolyte particles 100 .
[0055] The electrolyte layer 202 contains an electrolyte material. The electrolyte material is, for example, a solid electrolyte material.
[0056] The negative electrode 203 includes negative electrode active material particles 205 and solid electrolyte particles 100 .
[0057] The solid electrolyte particle 100 is a particle containing the solid electrolyte material of the first embodiment. The solid electrolyte particle 100 may also be a particle containing the solid electrolyte material of the first embodiment as a main component. The so-called particle containing the solid electrolyte material of the first embodiment as a main component refers to a particle containing the solid electrolyte material of the first embodiment as the largest component in terms of molar ratio. The solid electrolyte particle 100 may also be a particle composed of the solid electrolyte material of the first embodiment.
[0058] The positive electrode 201 contains a material that can absorb and release metal ions such as lithium ions. The positive electrode 201 contains, for example, a positive electrode active material (for example, positive electrode active material particles 204).
[0059] Examples of positive electrode active materials are lithium-containing transition metal oxides, transition metal fluorides, polyanionic materials, fluorinated polyanionic materials, transition metal sulfides, transition metal oxysulfides or transition metal oxynitrides. Examples of lithium-containing transition metal oxides are Li(Ni, Co, Al)O2, LiCoO2 or Li(Ni, Co, Mn)O2.
[0060] In the present disclosure, "(A, B, C)" means "at least one selected from A, B, and C." However, A, B, and C all represent elements.
[0061] From the perspective of battery cost and safety, lithium phosphate may be used as the positive electrode active material.
[0062] The positive electrode 201 contains the solid electrolyte material of the first embodiment, and when X contains I (i.e., iodine), lithium iron phosphate can also be used as the positive electrode active material. The solid electrolyte material of the first embodiment containing I is easily oxidized. If lithium iron phosphate is used as the positive electrode active material, the oxidation reaction of the solid electrolyte can be suppressed. In other words, the formation of an oxide layer with low lithium ion conductivity can be suppressed. As a result, the battery has a high charge and discharge efficiency.
[0063] The positive electrode 201 contains not only the solid electrolyte material of the first embodiment, but also a transition metal fluoride oxide as a positive electrode active material. Even if the solid electrolyte material of the first embodiment is fluorinated by a transition metal fluoride, it is difficult to form a resistance layer. As a result, the battery has a high charge and discharge efficiency.
[0064] Transition metal fluoride oxide contains oxygen and fluorine. As an example, the transition metal fluoride oxide can also be a composition formula Li p Me q O m F n wherein Me is at least one element selected from the group consisting of Mn, Co, Ni, Fe, Al, Cu, V, Nb, Mo, Ti, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, Ag, Ru, W, B, Si and P, and satisfies the following mathematical formula: 0.5≤p≤1.5, 0.5≤q≤1.0, 1≤m<2 and 0<n≤1. Examples of such transition metal fluoride oxides are Li 1.05 (Ni 0.35 Co 0.35 Mn 0.3 ) 0.95 O 1.9 F 0.1 .
[0065] The positive electrode active material particles 204 may also have a median particle size of 0.1 μm or more and 100 μm or less. When the positive electrode active material particles 204 have a median particle size of 0.1 μm or more, in the positive electrode 201, the positive electrode active material particles 204 and the solid electrolyte particles 100 can form a good dispersion state. As a result, the charge and discharge characteristics of the battery are improved. When the positive electrode active material particles 204 have a median particle size of 100 μm or less, the lithium diffusion rate in the positive electrode active material particles 204 is increased. As a result, the battery can operate at a high output power.
[0066] The positive electrode active material particles 204 may have a larger median diameter than the solid electrolyte particles 100. This allows the positive electrode active material particles 204 and the solid electrolyte particles 100 to be in a well-dispersed state.
[0067] To improve the energy density and output of the battery, in the positive electrode 201 , the ratio of the volume of the positive electrode active material particles 204 to the total volume of the positive electrode active material particles 204 and the volume of the solid electrolyte particles 100 may be 0.30 or more and 0.95 or less.
[0068] Figure 2A cross-sectional view of an electrode material 1100 according to a second embodiment is shown. The electrode material 1100 is contained in, for example, a positive electrode 201. In order to prevent the electrode active material particles 206 from reacting with the solid electrolyte particles 100, a coating layer 216 may be formed on the surface of the electrode active material particles 206. This can suppress the increase in the reaction overvoltage of the battery. Examples of the coating material contained in the coating layer 216 are sulfide solid electrolytes, oxide solid electrolytes, or halide solid electrolytes.
[0069] When the solid electrolyte particle 100 is a sulfide solid electrolyte, the coating material is the solid electrolyte material of the first embodiment, and X may be at least one element selected from Cl and Br. Such a solid electrolyte material of the first embodiment is less susceptible to oxidation than a sulfide solid electrolyte. As a result, the increase in the reaction overvoltage of the battery can be suppressed.
[0070] When the solid electrolyte particle 100 is the solid electrolyte material of the first embodiment and X contains I, the coating material may also be the solid electrolyte material of the first embodiment, and X may also be at least one element selected from Cl and Br. The solid electrolyte material of the first embodiment not containing I is less likely to be oxidized than the solid electrolyte material of the first embodiment containing I. As a result, the battery has high charge and discharge efficiency.
[0071] When the solid electrolyte particle 100 is the solid electrolyte material of the first embodiment and X includes I, the coating material may also contain an oxide solid electrolyte. The oxide solid electrolyte may also be lithium niobate which has excellent stability even at high potentials. Thus, the battery has high charge and discharge efficiency.
[0072] The positive electrode 201 may also be composed of a first positive electrode layer containing a first positive electrode active material and a second positive electrode layer containing a second positive electrode active material. Among them, the second positive electrode layer is arranged between the first positive electrode layer and the electrolyte layer 202, and the first positive electrode layer and the second positive electrode layer contain the solid electrolyte material of the first embodiment containing I, and a coating layer 216 is formed on the surface of the second positive electrode active material. According to the above structure, the solid electrolyte material of the first embodiment contained in the electrolyte layer 202 can be suppressed from being oxidized by the second positive electrode active material. As a result, the battery has a high charging capacity. Examples of the coating material contained in the coating layer 206 are sulfide solid electrolytes, oxide solid electrolytes, polymer solid electrolytes, or halide solid electrolytes. However, when the coating material is a halide solid electrolyte, I is not contained as a halogen element. The first positive electrode active material may also be the same material as the second positive electrode active material, or may be a material different from the second positive electrode active material.
[0073] In order to increase the energy density and output of the battery, the positive electrode 201 may have a thickness of 10 μm or more and 500 μm or less.
[0074] The electrolyte layer 202 contains an electrolyte material. The electrolyte material is, for example, a solid electrolyte material. The electrolyte layer 202 may also be a solid electrolyte layer. The solid electrolyte material contained in the electrolyte layer 202 may also contain the solid electrolyte material of the first embodiment. The solid electrolyte material contained in the electrolyte layer 202 may also be composed only of the solid electrolyte material of the first embodiment.
[0075] The solid electrolyte material contained in the electrolyte layer 202 may also be composed of only a solid electrolyte material different from the solid electrolyte material of the first embodiment. Examples of solid electrolyte materials different from the solid electrolyte material of the first embodiment are Li2MgX'4, Li2FeX'4, Li(Al, Ga, In)X'4, Li3(Al, Ga, In)X'6 or LiI. Here, X' is at least one element selected from F, Cl, Br and I.
[0076] Hereinafter, the solid electrolyte material of the first embodiment is referred to as a first solid electrolyte material. A solid electrolyte material different from the solid electrolyte material of the first embodiment is referred to as a second solid electrolyte material.
[0077] The electrolyte layer 202 may contain not only the first solid electrolyte material but also the second solid electrolyte material. The first solid electrolyte material and the second solid electrolyte material may be uniformly dispersed.
[0078] The electrolyte layer 202 may have a thickness of 1 μm or more and 100 μm or less. When the electrolyte layer 202 has a thickness of 1 μm or more, the positive electrode 201 and the negative electrode 203 are less likely to short-circuit. When the electrolyte layer 202 has a thickness of 100 μm or less, the battery can operate at a high output power.
[0079] Another electrolyte layer may be further provided between the electrolyte layer 202 and the negative electrode 203. For example, when the electrolyte layer 202 contains a first solid electrolyte material, in order to more stably maintain the high ion conductivity of the solid electrolyte material, an electrolyte layer composed of another solid electrolyte material that is electrochemically more stable than the solid electrolyte material may be further provided.
[0080] The negative electrode 203 contains a material that can insert and remove metal ions (eg, lithium ions). The negative electrode 203 contains, for example, a negative electrode active material (eg, negative electrode active material particles 205).
[0081] Examples of negative electrode active materials are metal materials, carbon materials, oxides, nitrides, tin compounds or silicon compounds. The metal material may be a simple metal or an alloy. Examples of metal materials are lithium metal or lithium alloys. Examples of carbon materials are natural graphite, coke, graphitizable carbon, carbon fiber, spherical carbon, artificial graphite or amorphous carbon. From the viewpoint of capacity density, suitable examples of negative electrode active materials are silicon (i.e. Si), tin (i.e. Sn), silicon compounds or tin compounds.
[0082] The negative electrode active material can also be selected based on the reduction resistance of the solid electrolyte material contained in the negative electrode 203. When the negative electrode 203 contains the first solid electrolyte, a material that can embed and deintercalate lithium ions at more than 0.27V relative to lithium can also be used as the negative electrode active material. As long as the negative electrode active material is such a material, it is possible to suppress the first solid electrolyte contained in the negative electrode 203 from being reduced. As a result, the battery has a high charge and discharge efficiency. Examples of the material are titanium oxide, indium metal or lithium alloy. An example of titanium oxide is Li4Ti5O 12 , LiTi2O4 or TiO2.
[0083] The negative electrode active material particles 205 may also have a median particle size of 0.1 μm or more and 100 μm or less. When the negative electrode active material particles 205 have a median particle size of 0.1 μm or more, the negative electrode active material particles 205 and the solid electrolyte particles 100 can form a good dispersion state in the negative electrode 203. As a result, the charge and discharge characteristics of the battery are improved. When the negative electrode active material particles 205 have a median particle size of 100 μm or less, the lithium diffusion rate in the negative electrode active material particles 205 is increased. As a result, the battery can operate at a high output power.
[0084] The negative electrode active material particles 205 may have a larger median diameter than the solid electrolyte particles 100. This allows the negative electrode active material particles 205 and the solid electrolyte particles 100 to be in a well-dispersed state.
[0085] To improve the energy density and output of the battery, in the negative electrode 203 , the ratio of the volume of the negative electrode active material particles 205 to the total volume of the negative electrode active material particles 205 and the volume of the solid electrolyte particles 100 may be 0.30 or more and 0.95 or less.
[0086] Figure 2The electrode material 1100 shown may also be contained in the negative electrode 203. In order to prevent the solid electrolyte particles 100 from reacting with the negative electrode active material (i.e., the electrode active material particles 206), a coating layer 216 may also be formed on the surface of the electrode active material particles 206. As a result, the battery has a high charge and discharge efficiency. Examples of the coating material contained in the coating layer 216 are sulfide solid electrolytes, oxide solid electrolytes, polymer solid electrolytes, or halide solid electrolytes.
[0087] When the solid electrolyte particle 100 is the first solid electrolyte material, the coating material may also be a sulfide solid electrolyte, an oxide solid electrolyte, or a polymer solid electrolyte. An example of a sulfide solid electrolyte is Li2S-P2S5. An example of an oxide solid electrolyte is trilithium phosphate. An example of a polymer solid electrolyte is a composite compound of polyethylene oxide and a lithium salt. An example of such a polymer solid electrolyte is lithium bis(trifluoromethanesulfonyl)imide.
[0088] In order to increase the energy density and output of the battery, the negative electrode 203 may have a thickness of 10 μm or more and 500 μm or less.
[0089] At least one selected from the positive electrode 201, the electrolyte layer 202, and the negative electrode 203 may contain a second solid electrolyte material for the purpose of improving ion conductivity. Examples of the second solid electrolyte material are sulfide solid electrolytes, oxide solid electrolytes, halide solid electrolytes, or organic polymer solid electrolytes.
[0090] In the present disclosure, the so-called "sulfide solid electrolyte" refers to a solid electrolyte containing sulfur. The so-called "oxide solid electrolyte" refers to a solid electrolyte containing oxygen. The oxide solid electrolyte may also contain anions other than oxygen (but excluding sulfur anions and halogen anions). The so-called "halide solid electrolyte" refers to a solid electrolyte containing halogen elements and no sulfur. The halide solid electrolyte contains not only halogen elements but also oxygen.
[0091] Examples of sulfide solid electrolytes are Li2S-P2S5, Li2S-SiS2, Li2S-B2S3, Li2S-GeS2, Li 3.25 Ge 0.25 P 0.75 S4 or Li 10 GeP2S 12 .
[0092] Examples of oxide solid electrolytes are:
[0093] (i) NASICON type solid electrolytes such as LiTi2(PO4)3 or its element substitution products,
[0094] (ii) Perovskite-type solid electrolytes such as (LaLi)TiO3,
[0095] (iii)Li 14 ZnGe4O 16 , LISICON type solid electrolytes such as Li4SiO4, LiGeO4 or their element substitution products,
[0096] (iv)Li7La3Zr2O 12 Or a garnet-type solid electrolyte such as an element-substituted body thereof, or (v) Li3PO4 or its N-substituted body.
[0097] An example of a halide solid electrolyte is Li a Me' b Y c A compound represented by Z6. Wherein, the mathematical formulas are satisfied: a+mb+3c=6 and c>0. Me' is at least one selected from metal elements and semi-metal elements other than Li and Y. Z is at least one selected from F, Cl, Br and I. The value of m represents the valence of Me'.
[0098] The so-called "semi-metallic elements" are B, Si, Ge, As, Sb and Te. The so-called "metallic elements" are all elements contained in Groups 1 to 12 of the periodic table (but excluding hydrogen) and all elements contained in Groups 13 to 16 of the periodic table (but excluding B, Si, Ge, As, Sb, Te, C, N, P, O, S and Se). Me' may also be at least one element selected from Mg, Ca, Sr, Ba, Zn, Sc, Al, Ga, Bi, Zr, Hf, Ti, Sn, Ta and Nb.
[0099] Examples of halide solid electrolytes are Li3YCl6 or Li3YBr6.
[0100] When the electrolyte layer 202 contains the first solid electrolyte material, the negative electrode 203 may also contain a sulfide solid electrolyte. Thus, the sulfide solid electrolyte, which is electrochemically stable with respect to the negative electrode active material, can suppress the first solid electrolyte material and the negative electrode active material from contacting each other. As a result, the battery has a low internal resistance.
[0101] An example of an organic polymer solid electrolyte is a compound of a polymer compound and a lithium salt. The polymer compound may also have an ethylene oxide structure. A polymer compound having an ethylene oxide structure can contain a large amount of lithium salt and thus has a higher ion conductivity.
[0102] Examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9) or LiC(SO2CF3)3. One lithium salt selected from these may be used alone. Alternatively, a mixture of two or more lithium salts selected from these may be used.
[0103] At least one selected from the positive electrode 201 , the electrolyte layer 202 , and the negative electrode 203 may contain a non-aqueous electrolyte solution, a gel electrolyte, or an ionic liquid for the purpose of facilitating the transfer of lithium ions and improving the output characteristics of the battery.
[0104] The non-aqueous electrolyte contains a non-aqueous solvent and a lithium salt dissolved in the non-aqueous solvent. Examples of non-aqueous solvents are cyclic carbonate solvents, chain carbonate solvents, cyclic ether solvents, chain ether solvents, cyclic ester solvents, chain ester solvents or fluorine solvents. Examples of cyclic carbonate solvents are ethylene carbonate, propylene carbonate or butylene carbonate. Examples of chain carbonate solvents are dimethyl carbonate, ethyl methyl carbonate or diethyl carbonate. Examples of cyclic ether solvents are tetrahydrofuran, 1,4-dioxane or 1,3-dioxolane. Examples of chain ether solvents are 1,2-dimethoxyethane or 1,2-diethoxyethane. Examples of cyclic ester solvents are γ-butyrolactone. Examples of chain ester solvents are methyl acetate. Examples of fluorine solvents are fluoroethylene carbonate, methyl fluoropropionate, fluorobenzene, ethyl fluoromethyl carbonate or dimethylene fluorocarbonate. One non-aqueous solvent selected from them can be used alone. Alternatively, a mixture of two or more nonaqueous solvents selected from these may be used.
[0105] Examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9) or LiC(SO2CF3)3. One lithium salt selected from these may be used alone. Alternatively, a mixture of two or more lithium salts selected from these may be used. The concentration of the lithium salt is, for example, in the range of 0.5 mol / liter or more and 2 mol / liter or less.
[0106] As the gel electrolyte, a polymer material impregnated with a non-aqueous electrolyte can be used. Examples of the polymer material are polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polymethyl methacrylate, or a polymer having an ethylene oxide bond.
[0107] Examples of cations contained in ionic liquids are:
[0108] (i) aliphatic chain quaternary salts such as tetraalkylammonium or tetraalkylphosphonium,
[0109] (ii) an aliphatic cyclic ammonium such as pyrrolidinium, morpholinium, imidazolinium, tetrahydropyrimidinium, piperazinium or piperidinium, or
[0110] (iii) Nitrogen-containing heterocyclic aromatic cations such as pyridinium and imidazolium cations.
[0111] An example of an anion contained in an ionic liquid is PF6 - 、BF4 - 、SbF6 - 、AsF6 - 、SO3CF3 - 、N(SO2CF3)2 - 、N(SO2C2F5)2 - 、N(SO2CF3)(SO2C4F9) - or C(SO2CF3)3 - .
[0112] The ionic liquid may also contain a lithium salt.
[0113] At least one selected from the positive electrode 201 , the electrolyte layer 202 , and the negative electrode 203 may contain a binder for the purpose of improving the adhesion between particles.
[0114] The example of binding agent is polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polypropylene, aramid resin, polyamide, polyimide, polyamide-imide, polyacrylonitrile, polyacrylic acid, polymethyl acrylate, polyethyl acrylate, polyhexyl acrylate, polymethacrylic acid, polymethyl methacrylate, polyethyl methacrylate, polyhexyl methacrylate, polyvinyl acetate, polyvinyl pyrrolidone, polyether, polyether sulfone, polyhexafluoropropylene, styrene-butadiene rubber or carboxymethyl cellulose. As binding agent, copolymer can also be used. The example of this binding agent is a copolymer of two or more materials selected from tetrafluoroethylene, hexafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, vinylidene fluoride, chlorotrifluoroethylene, ethylene, propylene, pentafluoropropylene, fluoromethyl vinyl ether, acrylic acid and hexadiene. A mixture of two or more selected from the above-mentioned materials can also be used.
[0115] At least one selected from the positive electrode 201 and the negative electrode 203 may contain a conductive auxiliary agent in order to improve electron conductivity.
[0116] Examples of conductive additives are:
[0117] (i) Graphites such as natural graphite or artificial graphite,
[0118] (ii) Carbon blacks such as acetylene black or Ketjen black,
[0119] (iii) Conductive fibers such as carbon fibers or metal fibers,
[0120] (iv) fluorinated carbon,
[0121] (v) Metal powders such as aluminum,
[0122] (vi) Conductive whiskers such as zinc oxide or potassium titanate,
[0123] (vii) conductive metal oxides such as titanium oxide, or
[0124] (viii) Conductive polymer compounds such as polyaniline, polypyrrole or polythiophene For cost reduction, the conductive auxiliary agent described in (i) or (ii) above may be used.
[0125] Examples of the shape of the battery of the second embodiment include a coin shape, a cylindrical shape, a square shape, a sheet shape, a button shape, a flat shape, or a laminated shape.
[0126] Example
[0127] Hereinafter, the present disclosure will be described in more detail with reference to examples.
[0128] (Example 1)
[0129] [Production of solid electrolyte materials]
[0130] In a dry atmosphere with a dew point below -30°C (hereinafter referred to as "dry atmosphere"), LiOH, LiCl and TaCl5 are prepared as raw material powders in a molar ratio of LiOH:LiCl:TaCl5=0.8:0.1:1.0. These raw material powders are crushed and mixed in a mortar to obtain a mixed powder. Then, a planetary ball mill is used to grind the obtained mixed powder for 24 hours at 500 rpm. In this way, the solid electrolyte material of Example 1 is obtained. The molar ratio Li / M is 0.9, and O / X is 0.19. In addition, with respect to the molar ratios Li / M and O / X, Li and M were determined by ICP emission spectrometry, X was determined by ion chromatography, and O was determined by inert gas fusion-infrared absorption. The devices used in the composition measurement are ICP emission spectrometry, ion chromatography and oxygen analysis.
[0131] [Evaluation of ion conductivity]
[0132] Figure 3 A schematic diagram showing a press mold 300 for evaluating the ion conductivity of a solid electrolyte material.
[0133] The press forming die 300 includes a punch upper portion 301, a frame die 302, and a punch lower portion 303. The frame die 302 is formed of insulating polycarbonate. The punch upper portion 301 and the punch lower portion 303 are both formed of electronically conductive stainless steel.
[0134] use Figure 3 The press molding die 300 shown was used to measure the ion conductivity of the solid electrolyte material of Example 1 by the following method.
[0135] In a dry atmosphere, the powder of the solid electrolyte material of Example 1 (i.e. Figure 3 The solid electrolyte material powder 101 is filled in the press mold 300. In the press mold 300, a pressure of 300 MPa is applied to the solid electrolyte material of Example 1 using the punch upper portion 301.
[0136] Keeping the state of the applied pressure unchanged, the punch upper part 301 and the punch lower part 303 are connected to a potentiostat (Versa STAT4 manufactured by Princeton Applied Research) equipped with a frequency response analyzer. The punch upper part 301 is connected to the working electrode and the potential measurement terminal. The punch lower part 303 is connected to the counter electrode and the reference electrode. At room temperature, the ionic conductivity of the solid electrolyte material of Example 1 was measured by electrochemical impedance spectroscopy. As a result, the ionic conductivity measured at 22°C was 5.6mS / cm.
[0137] [Evaluation of effective ion conductivity]
[0138] In an argon atmosphere having a dew point of -60°C or less, the solid electrolyte material of Example 1 and LiCoO2, which is a positive electrode active material, were prepared at a volume ratio of 75:25. These materials were mixed in a mortar to obtain a mixture.
[0139] In an insulating cylinder having an inner diameter of 9.5 mm, the sulfide solid electrolyte of Li2S-P2S5, the above-mentioned mixture, and the sulfide solid electrolyte of Li2S-P2S5 were stacked in sequence. Then, a pressure of 360 MPa was applied to the stack. In this way, an electrode containing the solid electrolyte material of Example 1 sandwiched by the sulfide solid electrolyte layer was produced.
[0140] Next, Li metal foils were stacked on the upper and lower sides of the electrode, and a pressure of 80 MPa was applied to the stacked body to form a cell for measuring effective ion conductivity.
[0141] A voltage was applied to the battery, and the resistance value of the battery was calculated from the detected current. Then, the conductivity was calculated from the reciprocal of the resistance value. By subtracting the conductivity of the sulfide solid electrolyte of Li2S-P2S5 from the obtained conductivity, the effective ion conductivity of the electrode containing the solid electrolyte material of Example 1 was determined. As a result, the effective ion conductivity measured at 22°C was 0.52mS / cm. The ratio of the effective ion conductivity to the ion conductivity, i.e., the electrode structure factor, was 0.09.
[0142] [Evaluation of Young's modulus]
[0143] The Young's modulus of the solid electrolyte material is calculated from a load-displacement curve measured using a nano indenter (TI980 manufactured by Bruker).
[0144] As a result, the Young's modulus of the solid electrolyte material of Example 1 was 10.8 GPa.
[0145] (Examples 2 to 3 and Comparative Examples 1 to 2)
[0146] [Production of solid electrolyte materials]
[0147] In Example 2, Li2O, LiOH, ZrCl4 and Li2S were prepared as raw material powders in a molar ratio of Li2O: LiOH: ZrCl4: Li2S = 0.7: 0.2: 1.0: 0.2. The composition of the obtained solid electrolyte material was analyzed in the same manner as in Example 1, and the molar ratios Li / M, O / X and S / M were determined from the analyzed composition. The molar ratios Li / M were 2.0, O / X were 0.20, and S / M were 0.2.
[0148] In Example 3, LiOH and TaCl5 were prepared as raw material powders in a molar ratio of LiOH:TaCl5=0.9:1.0. The composition of the obtained solid electrolyte material was analyzed in the same manner as in Example 1, and the molar ratios Li / M and O / X were determined from the analyzed composition. The molar ratios Li / M and O / X were 0.9 and 0.23, respectively.
[0149] Solid electrolyte materials of Examples 2 and 3 were obtained in the same manner as in Example 1 except for the above matters.
[0150] In Comparative Example 1, LiOH and TaCl5 are prepared as raw material powders in a molar ratio of LiOH:TaCl5=0.9:1.0. These raw material powders are crushed and mixed in a mortar to obtain a mixed powder. The obtained mixed powder is calcined at 230°C for 3 hours. The obtained calcined product is crushed in an agate mortar. In this way, the solid electrolyte material of Comparative Example 1 is obtained. The composition of the obtained solid electrolyte material is analyzed in the same manner as in Example 1, and the molar ratios Li / M and O / X are determined from the analyzed composition. The molar ratio Li / M is 0.9, and O / X is 0.22.
[0151] In Comparative Example 2, LiOH and TaCl5 are prepared as raw material powders in a molar ratio of LiOH:TaCl5=0.9:1.0. These raw material powders are crushed and mixed in a mortar to obtain a mixed powder. The obtained mixed powder is ground using a planetary ball mill at 600 rpm for 24 hours. In this way, the solid electrolyte material of Comparative Example 2 is obtained. The composition of the obtained solid electrolyte material is analyzed in the same manner as in Example 1, and the molar ratios Li / M and O / X are determined from the analyzed composition. The molar ratio Li / M is 0.9, and O / X is 0.25.
[0152] [Evaluation of ion conductivity]
[0153] The ion conductivity of the solid electrolyte materials of Examples 2 to 3 and Comparative Examples 1 to 2 was measured in the same manner as in Example 1. Table 1 shows the measurement results.
[0154] [Evaluation of effective ion conductivity]
[0155] The effective ion conductivity of the solid electrolyte materials of Examples 2 to 3 and Comparative Examples 1 to 2 was calculated in the same manner as in Example 1. Table 1 shows the measurement results.
[0156] Table 1 also shows the ratio of the effective ion conductivity to the ion conductivity, that is, the electrode structure factor.
[0157] [Evaluation of Young's modulus]
[0158] The Young's modulus of the solid electrolyte materials of Examples 2 to 3 and Comparative Examples 1 to 2 was measured in the same manner as in Example 1. Table 1 shows the measurement results.
[0159] Table 1
[0160]
[0161] (Inspection)
[0162] Table 1 shows that in the solid electrolyte materials of Examples 1 to 3, the ratio of the effective ion conductivity to the ion conductivity, that is, the electrode structure factor, is large.
[0163] Comparison between Examples 1 to 3 and Comparative Examples 1 to 2 shows that if the Young's modulus is large, the electrode structure factor is reduced.
[0164] The inventors have found that the Young's modulus of the solid electrolyte material can be controlled by changing the production conditions of the solid electrolyte material. As in Comparative Example 1, the solid electrolyte material produced by heat treatment after treatment with a planetary ball mill has a high Young's modulus. In addition, as in Comparative Example 2, the solid electrolyte material produced by increasing the input energy of the planetary ball mill also has a high Young's modulus.
[0165] As described above, the solid electrolyte material of the present disclosure is suitable for providing a battery having excellent charge and discharge characteristics because it can achieve a large electrode form factor.
[0166] Industrial Applicability
[0167] The battery disclosed herein can be used, for example, as an all-solid lithium ion secondary battery.
[0168] Explanation of symbols:
[0169] 100 solid electrolyte particles
[0170] 101 Solid Electrolyte Material Powder
[0171] 201 positive electrode
[0172] 202 electrolyte layer
[0173] 203 negative electrode
[0174] 204 Positive electrode active material particles
[0175] 205 Negative electrode active material particles
[0176] 206 Electrode active material particles
[0177] 216 coating layer
[0178] 300 Pressurized Forming Die
[0179] 301 punch upper part
[0180] 302 frame mold
[0181] 303 punch lower part
[0182] 1000 battery
[0183] 1100 Electrode Materials
Claims
1. A solid electrolyte material comprising Li, M, A and X, in, M is at least one selected from Nb, Ta and Zr, A is at least one selected from O and S, X is at least one selected from F, Cl, Br and I, The solid electrolyte material has a Young's modulus below 23 GPa.
2. The solid electrolyte material according to claim 1, wherein X contains Cl.
3. The solid electrolyte material according to claim 1 or 2, wherein A contains O.
4. The solid electrolyte material according to claim 3, wherein A is O and S.
5. The solid electrolyte material according to any one of claims 1 to 4, wherein It has a Young's modulus of 20 GPa or less.
6. The solid electrolyte material according to claim 5, wherein It has a Young's modulus of 10.8 GPa or more and 19.6 GPa or less.
7. The solid electrolyte material according to any one of claims 1 to 6, wherein The molar ratio of Li to M is 0.60 or more and 3.0 or less.
8. The solid electrolyte material according to claim 7, wherein The molar ratio of Li to M is 0.90 or more and 2.0 or less.
9. The solid electrolyte material according to claim 3, wherein The molar ratio of O to X is 0.05 or more and 0.35 or less.
10. The solid electrolyte material according to any one of claims 1 to 9, wherein A contains S, and The molar ratio of S to M is 0.1 or more and 0.7 or less.
11. A battery comprising: positive electrode, Negative electrode, and an electrolyte layer provided between the positive electrode and the negative electrode, in, At least one selected from the positive electrode, the negative electrode, and the electrolyte layer contains the solid electrolyte material according to any one of claims 1 to 10.