Solid state battery with aluminum-based anode
Through the combination of aluminum-based anode material and solid electrolyte, the safety hazards and insufficient energy density of existing lithium-ion batteries in the manufacturing process are solved, higher energy density and safety are achieved, and carbon footprint and wet processing are reduced. Use of
Patent Information
- Application Number
- CN202380032255.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-08
- Filing Date
- 2023-04-07
- Publication Date
- 2024-11-15
AI Technical Summary
The existing lithium-ion batteries use liquid electrolytes and wet processing during the manufacturing process, which has safety hazards and environmental impacts, and the energy density of the anode material is insufficient.
The aluminum-based anode material is used to combine with the solid electrolyte, and the anode and inorganic solid electrolyte are alloyed by aluminum-based alkali metal, reducing or eliminating liquid treatment, improving the specific capacity and safety of the anode.
Higher energy density and safety are achieved, wet processing is avoided, carbon footprint is reduced, and the manufacturability of the battery system is improved.
Smart Images

Figure CN118974971A_ABST
Abstract
Description
[0001] Citation of Related Applications
[0002] This application claims the benefit of and priority to U.S. Provisional Patent Application No. 63 / 362,722, filed on April 8, 2022, and entitled “SOLID-STATE BATTERIES WITH ALUMINUM-BASED ANODES,” the contents of which are hereby incorporated by reference in their entirety. Technical Field
[0003] The present disclosure relates generally to metallurgy, and more particularly to solid-state batteries containing aluminum-based anode active materials. Background Art
[0004] Conventional lithium-ion batteries typically include a cathode, an anode, and a separator therebetween that is impregnated with an electrolyte. Current collectors on the cathode and anode sides are used to conduct current between the cathode and anode, while the electrolyte allows lithium ions to be transported between the cathode and anode. Due to the potentials involved, copper is typically used as the anode current collector, and aluminum is typically used as the cathode current collector. Lithium metal oxides, such as lithium cobalt oxide, are typically used as lithium-ion battery cathodes, while graphite is typically used as lithium-ion battery anodes. Summary of the invention
[0005] The term embodiment and similar terms are intended to refer broadly to the subject matter of the present disclosure and the entirety of the following claims. Statements containing these terms should not be understood to limit the subject matter described herein, or to limit the meaning or scope of the following claims. The embodiments of the present disclosure covered herein are defined by the following claims rather than by this disclosure. This disclosure is a high-level overview of various aspects of the present disclosure and introduces some of the concepts further described in the following detailed description section. This disclosure is neither intended to identify the key or essential features of the claimed subject matter nor to be used independently to determine the scope of the claimed subject matter. The subject matter should be understood by reference to appropriate portions of the entire specification of the present disclosure, any or all drawings, and each claim.
[0006] In various aspects, solid-state batteries or electrochemical cells are described herein. The solid-state batteries described herein include aluminum-based anode materials, which can be used as alkali metal alloying anodes and are different from the anodes used in conventional lithium-ion batteries and solid-state batteries. Aluminum-based alkali metal alloying anodes can exhibit significantly higher lithium capacity than conventional anode materials (such as graphite). For example, aluminum-based alkali metal alloying anodes can incorporate lithium atoms into the crystalline matrix of aluminum, which means that more lithium can be incorporated per unit volume compared to an equal volume of graphite, where the lithium atoms are inserted and accommodated between graphite layers. In this way, the size and / or mass of the anode can be reduced compared to conventional graphite anodes while maintaining or even increasing the total capacity. In some examples, the solid-state batteries described herein may include an anode exhibiting a specific capacity of 300mAh / g to 1000mAh / g, such as 300mAh / g to 350mAh / g, 350mAh / g to 400mAh / g, 400mAh / g to 450mAh / g, 450mAh / g to 500mAh / g, 500mAh / g to 550mAh / g, 550mAh / g to 600mAh / g, 600mAh / g to 650mAh / g, 650mAh / g to 700mAh / g, 700mAh / g to 750mAh / g, 750mAh / g to 800mAh / g, 800mAh / g to 850mAh / g, 850mAh / g to 900mAh / g, 900mAh / g to 950mAh / g, or 950mAh / g to 1000mAh / g.
[0007] In addition, the solid-state batteries described herein include a solid electrolyte, which is different from conventional liquid electrolytes and provides many advantages over conventional liquid electrolytes. The combination of an aluminum-based anode and a solid electrolyte can also be advantageous by reducing or eliminating solution or liquid handling during various manufacturing steps, because both the solid electrolyte and the aluminum-based anode can be assembled as solid materials with a prepared cathode material to produce a solid-state battery.
[0008] In some examples, a solid-state battery may include an anode (such as an anode including aluminum as an anode active material), a cathode, and a solid electrolyte between the anode and the cathode. For example, the anode may include an aluminum-based alkali metal alloyed anode, such as where the alkali metal is lithium. Optionally, the anode includes an aluminum alloy or a recycled content aluminum alloy. For example, the use of recycled content aluminum alloys can be used to increase the sustainability of solid-state batteries or reduce the overall carbon footprint associated with solid-state batteries.
[0009] In an example, the anode may include or be in the form of a foil, such as an aluminum-based multi-component foil. In some examples, the thickness of the anode is 5 μm to 60 μm, such as 5 μm to 10 μm, 10 μm to 15 μm, 15 μm to 20 μm, 20 μm to 25 μm, 25 μm to 30 μm, 30 μm to 35 μm, 35 μm to 40 μm, 40 μm to 45 μm, 45 μm to 50 μm, 50 μm to 55 μm, or 55 μm to 60 μm.
[0010] Optionally, the aluminum-based multi-component foil may include aluminum or an aluminum alloy and one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc, or silver. It should be understood that the aluminum-based anode may undergo volume changes during the absorption and release of lithium; these non-aluminum elements can enhance the ability of the aluminum to be used as an alloying anode, such as by providing structural integrity and / or a conductive matrix for the alloying anode. In some examples, the anode comprises a foil comprising 40% to 99% by weight of aluminum or an aluminum alloy and 30% to 60% by weight of one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc, or silver. For example, the anode may include aluminum or an aluminum alloy in an amount of 40 wt % to 45 wt %, 45 wt % to 50 wt %, 50 wt % to 55 wt %, 55 wt % to 60 wt %, 60 wt % to 65 wt %, 65 wt % to 70 wt %, 70 wt % to 75 wt %, 75 wt % to 80 wt %, 80 wt % to 85 wt %, 85 wt % to 90 wt %, 90 wt % to 95 wt %, or 95 wt % to 99 wt %. Optionally, the anode may include one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc, or silver in an amount of 30 wt % to 35 wt %, 35 wt % to 40 wt %, 40 wt % to 45 wt %, 45 wt % to 50 wt %, 50 wt % to 55 wt %, or 55 wt % to 60 wt %. In some examples, the aluminum alloy may be a brazing alloy,
[0011] In some examples, the anode comprises a composite foil, such as including a first plurality of aluminum or aluminum alloy particles and a second plurality of particles selected from at least one of metal particles or non-metal particles. Useful metal or non-metal particles may include elements other than aluminum, such as one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc, or silver.
[0012] Any suitable solid electrolyte can be used for the solid-state battery described herein. For example, the solid electrolyte can be an inorganic solid electrolyte or include an inorganic solid electrolyte, but other solid electrolytes such as polymer solid electrolytes or gel polymer electrolytes can also be used. Optionally, the solid electrolyte includes lithium argyrodite material, Li6PS5Cl, lithium superion conductor (LISICON), doped garnet material, Li7La3Zr2O 12 (LLZO), Li 10 GeP2S 12 , Li 10 SnP2S 12 , lithium phosphorus sulfide (Li3PS4) or lithium phosphorus oxynitride (LIPON). The solid electrolyte may have any suitable thickness. In an example, the thickness of the solid electrolyte may be about 10 μm to about 300 μm, such as 10 μm to 20 μm, 20 μm to 30 μm, 30 μm to 40 μm, 40 μm to 50 μm, 50 μm to 75 μm, 75 μm to 100 μm, 100 μm to 125 μm, 125 μm to 150 μm, 150 μm to 175 μm, 175 μm to 200 μm, 200 μm to 225 μm, 225 μm to 250 μm, 250 μm to 275 μm, or 275 μm to 300 μm.
[0013] Any suitable cathode can be used in the solid-state battery described herein. For example, the cathode can include an alkali ion host material or an alkali metal-transition metal oxide cathode active material. Optionally, the cathode can include lithium nickel manganese cobalt oxide, lithium nickel cobalt aluminum oxide, lithium manganese oxide, lithium iron phosphate, lithium cobalt oxide, conversion cathode, FeS2, FeF3, sulfur-based cathode or sulfur.
[0014] Other suitable components may optionally be included in the solid-state battery described herein. For example, the solid-state battery may further include one or more of the following: a cathode current collector in contact with the cathode; or an anode current collector in contact with the anode. Optionally, the anode current collector and / or the cathode current collector comprises a protected aluminum alloy foil. Optionally, the anode current collector comprises a copper foil.
[0015] In some examples, the anode, the solid electrolyte, and the cathode are stacked, and a pressure is applied between them. For example, the stacking pressure applied between the anode and the cathode may be about 0.1 MPa to about 30 MPa, such as 0.1 MPa to 0.5 MPa, 0.5 MPa to 1 MPa, 1 MPa to 2 MPa, 2 MPa to 3 MPa, 3 MPa to 4 MPa, 4 MPa to 5 MPa, 5 MPa to 7.5 MPa, 7.5 MPa to 10 MPa, 10 MPa to 12.5 MPa, 12.5 MPa to 15 MPa, 15 MPa to 17.5 MPa, 17.5 MPa to 20, 20 MPa to 22.5 MPa, 22.5 MPa to 25 MPa, 25 MPa to 27.5 MPa, 27.5 MPa to 30 MPa.
[0016] In another example, another component that can be optionally included is an interface material. For example, the solid-state battery can also include an interface material between the anode and the solid electrolyte. Optionally, the interface material includes a solid electrolyte interphase, an artificial solid electrolyte interphase, a polymer coating, a carbon coating, or an inorganic coating.
[0017] In another aspect, a method of making a solid-state battery or electrochemical cell is described herein. An example method of this aspect includes: providing an anode, such as an anode comprising aluminum as an anode active material; providing a cathode; and positioning a solid-state electrolyte between the anode and the cathode. The method of this aspect may include or further include one or more of the following: contacting the anode with an anode current collector or contacting the cathode with a cathode current collector.
[0018] Optionally, providing the anode comprises preparing an aluminum-based multi-component foil, such as an aluminum-based multi-component foil comprising aluminum or an aluminum anode and one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc, or silver.
[0019] Various methods may be used to prepare the aluminum-based multi-component foil. In some examples, preparing the aluminum-based multi-component foil includes: casting an aluminum-based multi-component product comprising aluminum and one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc, or silver to produce an aluminum-based multi-component product; and rolling the aluminum-based multi-component product into a foil. In some examples, preparing the aluminum-based multi-component foil includes: obtaining a powder mixture of aluminum and one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc, or silver; and performing a laser powder bed fusion process on the powder mixture to produce the aluminum-based multi-component product. In some examples, preparing the aluminum-based multi-component foil includes cumulative roll bonding of aluminum or an aluminum alloy and a certain amount of one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc, or silver to produce the aluminum-based multi-component product. In some examples, preparing the aluminum-based multi-component foil includes using powder metallurgy, additive manufacturing, metal foam, forming perforations by laser or deep etching, dealloying (e.g., chemical dealloying) or other methods to form a microporous or nanoporous aluminum-based multi-component product. Optionally, preparing the aluminum-based multi-component foil includes or also includes rolling the aluminum-based multi-component product into a foil.
[0020] Other objects and advantages will become apparent from the following detailed description given by way of non-limiting example. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The description makes reference to the following drawings, in which the use of like reference numerals in different drawings is intended to describe like or similar components.
[0022] Figure 1 A schematic diagram of an example method of manufacturing a rolled aluminum alloy product is provided.
[0023] Figure 2 A schematic diagram of an example solid-state electrochemical cell is provided that includes an anode comprising aluminum as the anode active material.
[0024] Figure 3 Schematic diagrams of example solid-state electrochemical cells are provided that include an anode comprising aluminum as the anode active material and a protected aluminum anode current collector.
[0025] Figure 4 Data showing example cell cycling data for a first example solid state electrochemical cell is provided.
[0026] Figure 5 Data showing cycling capacity data for a first example solid state electrochemical cell is provided.
[0027] Figure 6 Data showing Coulombic efficiency data for a first example solid-state electrochemical cell is provided.
[0028] Figure 7Data showing example cell cycling data for a second example solid state electrochemical cell is provided.
[0029] Figure 8 Data showing cycling capacity data for a second example solid state electrochemical cell is provided.
[0030] Fig. 9 Data showing Coulombic efficiency data for a second example solid-state electrochemical cell is provided.
[0031] Fig.10 Data showing example cell cycling data for an example reference half-cell employing a liquid electrolyte is provided.
[0032] Fig.11 Data showing cycling capacity data for example reference half-cells employing liquid electrolytes is provided.
[0033] Fig.12 Data showing coulombic efficiency data for example reference half-cells employing liquid electrolytes is provided. DETAILED DESCRIPTION
[0034] Solid-state electrochemical cells doped with solid electrolytes and aluminum materials as anode active materials are described herein. The use of aluminum as an anode active material can drive increases in energy density and specific energy compared to cells using conventional anode materials (e.g., graphite), improve secondary cell safety compared to cells using lithium metal anodes or compared to cells using liquid electrolytes, and avoid wet processing, the use of liquid solvents during manufacturing, and the use of liquid electrolytes, at least for the anode side.
[0035] The aluminum anode active material may include an alkali metal alloyed anode. For example, lithium may form an alloy with aluminum at a low potential, wherein lithium ions may be reduced and incorporated into the aluminum material body in the form of an alloy. The aluminum used for the anode active material may be a foil (e.g., a composite foil or an alloy foil), such as a foil comprising aluminum or an aluminum alloy and optionally including one or more other elements (in an amount of 0.5 mol % to 50 mol %), such as silicon, tin, indium, gallium, antimony, lead, nickel, copper, zinc, carbon, germanium, silver, etc. The foil may be or include a eutectic alloy, a solid solution alloy, a mixed metal system, or a composite particle system. As described herein, the foil may be processed using metal casting and rolling processes, but other techniques may also be used to prepare the foil, including powder-based sintering or laser melting processes, such as laser powder bed fusion techniques. In addition, the foil may be prepared to have an engineered structure, such as by using powder metallurgy techniques, forming a microporous or nanoporous structure by additive manufacturing, using metal foam, forming perforations by laser or deep etching, dealloying (e.g., chemical dealloying) or other methods. In some examples, a metal product produced by a powder-based or engineered process may be subjected to rolling to at least partially consolidate and / or produce a foil from the metal product.
[0036] Definition and Description:
[0037] As used herein, the terms "invention," "the invention," "this invention," and "present invention" are intended to broadly refer to all subject matter of this patent application and the appended claims. Statements containing these terms should not be construed as limiting the subject matter described herein, or limiting the meaning or scope of the appended patent claims.
[0038] In this specification, reference is made to aluminum alloys identified by AA numbers and other related designations such as "Series" or "7xxx". To understand the most commonly used numerical designation system for naming and identifying aluminum and its alloys, see "International Alloy Designations and Chemical Composition Limits for Wrought Aluminum and Wrought Aluminum Alloys" or "Registration Record of Aluminum Association Alloy Designations and Chemical Compositions Limits for Aluminum Alloys in the Form of Castings and Ingot", both published by The Aluminum Association.
[0039] As used herein, the thickness of a plate is generally greater than about 15 mm. For example, a plate may refer to an aluminum product having a thickness greater than about 15 mm, greater than about 20 mm, greater than about 25 mm, greater than about 30 mm, greater than about 35 mm, greater than about 40 mm, greater than about 45 mm, greater than about 50 mm, or greater than about 100 mm.
[0040] As used herein, the thickness of the Saudi board (also referred to as a thin plate type board) is generally about 4 mm to about 15 mm. For example, the thickness of the Saudi board can be about 4 mm, about 5 mm, about 6 mm, about 7 mm, about 8 mm, about 9 mm, about 10 mm, about 11 mm, about 12 mm, about 13 mm, about 14 mm or about 15 mm.
[0041] As used herein, a thin plate generally refers to an aluminum product having a thickness of less than about 4 mm. For example, the thickness of a thin plate may be less than about 4 mm, less than about 3 mm, less than about 2 mm, less than about 1 mm, less than about 0.5 mm, or less than about 0.3 mm (e.g., about 0.2 mm). As used herein, a foil comprises a subset of thin plates and is generally less than about 200 μm in thickness. In some examples, the thickness of the foil may be about 10 μm to about 200 μm, such as about 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, or 200 μm.
[0042] Reference may be made to alloy states or conditions in this application. To understand the most commonly used alloy state descriptions, please refer to "American National Standards (ANSI) H35 on Alloy and Temper Designation Systems". F condition or state refers to a manufactured aluminum alloy. O condition or state refers to an aluminum alloy after annealing. Hxx condition or state (also referred to herein as H state) refers to a non-heat-treatable aluminum alloy that has been subjected to or not subjected to heat treatment (e.g., annealing) after cold rolling. Suitable H states include HX1, HX2, HX3, HX4, HX5, HX6, HX7, HX8 or HX9 states. T1 condition or state refers to an aluminum alloy that has been cooled from hot working and subjected to natural aging treatment (e.g., at room temperature). T2 condition or state refers to an aluminum alloy that has been cooled from hot working, cold worked and subjected to natural aging treatment. T3 condition or state refers to an aluminum alloy that has been subjected to solution heat treatment, cold working and natural aging treatment. T4 condition or state refers to an aluminum alloy that has been subjected to solution heat treatment and natural aging treatment. The T5 condition or state refers to aluminum alloys that have been cooled from hot working and artificially aged (at elevated temperatures). The T6 condition or state refers to aluminum alloys that have been solution heat treated and artificially aged. The T7 condition or state refers to aluminum alloys that have been solution heat treated and artificially aged. The T8x condition or state refers to aluminum alloys that have been solution heat treated, cold worked, and artificially aged. The T9 condition or state refers to aluminum alloys that have been solution heat treated, artificially aged, and cold worked. The W condition or state refers to aluminum alloys that have been solution heat treated.
[0043] As used herein, terms such as "cast metal product", "cast product", "cast aluminum alloy product" and the like are interchangeable and refer to products produced by direct chill casting (including direct chill co-casting) or semi-continuous casting, continuous casting (including, for example, by using a twin-belt caster, a twin-roll caster, a block caster or any other continuous casting machine), electromagnetic casting, hot top casting or any other casting method.
[0044] As used herein, "room temperature" may include a temperature from about 15° C. to about 30° C., such as about 15° C., about 16° C., about 17° C., about 18° C., about 19° C., about 20° C., about 21° C., about 22° C., about 23° C., about 24° C., about 25° C., about 26° C., about 27° C., about 28° C., about 29° C., or about 30° C. As used herein, "ambient conditions" may include a temperature of approximately room temperature, a relative humidity of about 20% to about 100%, and an atmospheric pressure of about 975 millibars (mbar) to about 1050 mbar. For example, the relative humidity can be about 20%, about 21%, about 22%, about 23%, about 24%, about 25%, about 26%, about 27%, about 28%, about 29%, about 30%, about 31%, about 32%, about 33%, about 34%, about 35%, about 36%, about 37%, about 38%, about 39%, about 40%, about 41%, about 42%, about 43%, about 44%, about 45%, about 46%, about 47%, about 48%, about 49%, about 50%, about 51%, about 52%, about 53%, about 54%, about 55%, about 56%, about 57%, about 58%, about 59%, about 60%, about 61%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 73%, about 74%, about 75%, about 76%, about 77%, about 78%, about 79%, about 80%, about 81%, about 82%, about 83%, about 84%, about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92%, about 93%, about 94%, about 95%, about 96%, about 97%, about 98%, about 99%, about 100%, about 101%, about 102%, about 103%, about 104%, about 105%, about 106%, about 107%, about 108%, about 109%, about 110%, about 111%, about 112%, about 113%, about 114%, about 115%, about 116%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92%, about 93%, about 94%, about 95%, about 96%, about 97%, about 98%, about 99%, about 100%, about 100%, about 101%, about 102%, about 103%, about 104%, about 105%, about 106%, about 107%, about 108%, about 109%, about 110%, about 111%, about 112%, about 113%, about 114%, about 115%, about 116%, about 117%, about 118%, about 119%, about 120%, about 121%, about 122%, about 123%, about 124%, about 125%, about 126%, about 127%, about 128%, about 129%, about 130%, about 131%, about 132%, about 133%, about 134%, about 135%, about 136%, about 137%, about 138%, about 139%, about 140%, about 141%, about 142%, about 143%, about 144%, about 145%, about 146%, about 147%, about 148%, about 149%, about 150%, about For example, the atmospheric pressure may be about 975 mbar, about 980 mbar, about 985 mbar, about 990 mbar, about 995 mbar, about 1000 mbar, about 1005 mbar, about 1010 mbar, about 1015 mbar, about 1020 mbar, about 1025 mbar, about 1030 mbar, about 1035 mbar, about 1040 mbar, about 1045 mbar, about 1050 mbar, or any value therebetween.
[0045] All ranges disclosed herein should be understood to encompass any and all subranges included therein. For example, a specified range of "1 to 10" should be considered to include any and all subranges between a minimum of 1 and a maximum of 10 (and including 1 and 10); that is, all subranges start with a minimum of 1 or greater (e.g., 1 to 6.1) and end with a maximum of 10 or less (e.g., 5.5 to 10). Unless otherwise stated, when referring to the composition amount of an element, the expression "up to" means that the element is optional and includes zero percent composition of the particular element. Unless otherwise stated, all composition percentages are weight percent (wt%).
[0046] As used herein, "a," "an," and "the" include both singular and plural references unless the context clearly indicates otherwise.
[0047] In the following examples, aluminum alloy products and their components may be described according to their elemental composition expressed as weight percent (wt%) or atomic percent (atom %) or molar percent (mol %). In each alloy, the remainder is aluminum, wherein the maximum weight % of the sum of all impurities is 1% (e.g., less than or about 0.15%, 0.25%, 0.5%, 0.75%, or 1%). In some examples, impurities refer to unspecified elemental components other than those specifically indicated in a particular alloy or composition. In some examples, an aluminum alloy or composite material is described herein that includes aluminum and one or more other components, wherein the other components may be present in an amount up to 30 mol %, 40 mol %, or 50 mol %.
[0048] Incidental elements, such as grain refiners and deoxidizers, or other additives may be present in the present invention and may themselves add other properties without departing from or significantly changing the alloys described herein or the properties of the alloys described herein.
[0049] Small amounts of unavoidable impurities, including materials or elements, may be present in the alloy due to the inherent properties of aluminum or leaching when in contact with processing equipment. As described, some alloys may contain no more than about 0.25% by weight of any element other than alloying or constituent elements, incidental elements, and unavoidable impurities.
[0050] Method for producing aluminum alloy products
[0051] The aluminum alloy products described herein (such as aluminum alloy foil or aluminum-based foil) can be prepared using a suitable method. For example, the aluminum alloy can be cast, homogenized, hot rolled, cold rolled, heat treated, formed or similarly processed to produce an aluminum alloy product.
[0052] Figure 1An overview of an example method of making an aluminum alloy product is provided. Figure 1 The method begins at 105, where an aluminum alloy 106 is cast to form a cast aluminum alloy product 107, such as an ingot or other cast product. At 110, the cast aluminum alloy product 107 is homogenized to form a homogenized aluminum alloy product 111. At 115, the homogenized aluminum alloy product 111 is subjected to one or more hot rolling passes and / or one or more cold rolling passes to form a rolled aluminum alloy product 112, which may correspond to an aluminum alloy article, such as an aluminum alloy plate, an aluminum alloy slat, or an aluminum alloy sheet. Optionally, the rolled aluminum alloy product 112 is subjected to additional processing steps as described below to form an aluminum alloy article.
[0053] Non-limiting examples of casting processes include direct chill (DC) casting processes or continuous casting (CC) processes. For example, Figure 1 A schematic diagram of a DC casting process is depicted at 105, but other casting processes may be used. A continuous casting system may include a pair of moving opposing casting surfaces (e.g., moving opposing belts, rollers, or blocks), a casting cavity between the pair of moving opposing casting surfaces, and a molten metal injector. The molten metal injector may have an end opening from which the molten metal may exit the molten metal injector and be injected into the casting cavity.
[0054] Cast aluminum alloy products such as ingots, billets or other cast products can be processed by any desired technique. Optionally, the processing steps can be used to produce rolled aluminum alloy products, such as aluminum alloy sheets. Example optional processing steps include, but are not limited to, homogenization, hot rolling, cold rolling, annealing, solution heat treatment, and pre-aging.
[0055] In the homogenization step, the cast product may be heated to a temperature in the range of about 400°C to about 600°C. For example, the cast product may be heated to a temperature of about 400°C, about 410°C, about 420°C, about 430°C, about 440°C, about 450°C, about 460°C, about 470°C, about 480°C, about 490°C, about 500°C, about 510°C, about 520°C, about 530°C, about 540°C, about 550°C, about 560°C, about 570°C, about 580°C, about 590°C, or about 600°C. The product may then be allowed to soak (i.e., remain at a specified temperature) for a period of time to form a homogenized product. In some examples, the total time of the homogenization step (including the heating and soaking stages) may be up to 24 hours. For example, in a homogenization step with a total time of up to 18 hours, the product may be heated to up to 500°C to 600°C and soaked. Optionally, in a homogenization step with a total time of more than 18 hours, the product may be heated to less than 490°C and homogenized. In some cases, the homogenization step includes multiple processes. In some non-limiting examples, the homogenization step includes heating the cast product to a first temperature for a first period of time, and then heating to a second temperature for a second period of time. For example, the cast product may be heated to about 465°C for about 3.5 hours, and then heated to about 480°C for about 6 hours.
[0056] After the homogenization step, a hot rolling step may optionally be performed. Before starting hot rolling, the homogenized product may be allowed to cool to a temperature between 300° C. and 450° C. For example, the homogenized product may be allowed to cool to a temperature between 325° C. and 425° C. or from 350° C. to 400° C. The homogenized product may then be hot rolled at a temperature between 300°C and 450°C to form a hot rolled plate, hot rolled satur plate or hot rolled sheet having a specification between 3 mm and 200 mm (e.g., 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, 15 mm, 20 mm, 25 mm, 30 mm, 35 mm, 40 mm, 45 mm, 50 mm, 55 mm, 60 mm, 65 mm, 70 mm, 75 mm, 80 mm, 85 mm, 90 mm, 95 mm, 100 mm, 110 mm, 120 mm, 130 mm, 140 mm, 150 mm, 160 mm, 170 mm, 180 mm, 190 mm, 200 mm or any value therebetween).
[0057] Optionally, the cast product may be a continuously cast product which may be allowed to cool to a temperature between 300° C. and 450° C. For example, the continuously cast product may be allowed to cool to a temperature between 325° C. and 425° C. or from 350° C. to 400° C. The continuously cast product may then be hot rolled at a temperature between 300° C. and 450° C. to form a hot rolled plate, hot rolled satur plate or hot rolled sheet having a specification between 3 mm and 200 mm (e.g., 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, 15 mm, 20 mm, 25 mm, 30 mm, 35 mm, 40 mm, 45 mm, 50 mm, 55 mm, 60 mm, 65 mm, 70 mm, 75 mm, 80 mm, 85 mm, 90 mm, 95 mm, 100 mm, 110 mm, 120 mm, 130 mm, 140 mm, 150 mm, 160 mm, 170 mm, 180 mm, 190 mm, 200 mm or any value therebetween). During hot rolling, temperature and other operating parameters may be controlled so that the temperature of the hot rolled intermediate product does not exceed 470°C, 450°C, 440°C or 430°C when leaving the hot rolling mill.
[0058] The product through casting, homogenization or hot rolling can be optionally cold-rolled into thinner products, such as cold-rolled thin plates or foils using a cold rolling mill. The specification of the cold-rolled product can be optionally between about 0.5 and 10 mm, for example between about 0.7 and 6.5 mm. Optionally, the cold-rolled product can have the following specifications: 0.5 mm, 1.0 mm, 1.5 mm, 2.0 mm, 2.5 mm, 3.0 mm, 3.5 mm, 4.0 mm, 4.5 mm, 5.0 mm, 5.5 mm, 6.0 mm, 6.5 mm, 7.0 mm, 7.5 mm, 8.0 mm, 8.5 mm, 9.0 mm, 9.5 mm or 10.0 mm. Cold rolling may be performed to obtain a final gauge thickness representing a gauge reduction of up to 85% (e.g., a reduction of up to 10%, up to 20%, up to 30%, up to 40%, up to 50%, up to 60%, up to 70%, up to 80%, or up to 85%) compared to the gauge before cold rolling began. In the case of foil, cold rolling may be performed to achieve a final thickness of the foil, such as less than 0.2 mm. Optionally, an intermediate annealing step may be performed during the cold rolling step, such as where a first cold rolling process is applied, followed by an annealing process (intermediate annealing), followed by a second cold rolling process. The intermediate annealing step may be performed at a temperature of about 300°C to about 450°C (e.g., about 310°C, about 320°C, about 330°C, about 340°C, about 350°C, about 360°C, about 370°C, about 380°C, about 390°C, about 400°C, about 410°C, about 420°C, about 430°C, about 440°C, or about 450°C). In some cases, the intermediate annealing step includes a plurality of processes. In some non-limiting examples, the intermediate annealing step includes heating the partially cold-rolled product to a first temperature for a first time period, and then heating to a second temperature for a second time period. For example, the partially cold-rolled product may be heated to about 410°C for about 1 hour, and then heated to about 330°C for about 2 hours.
[0059] Subsequently, the cast, homogenized or rolled product may optionally be subjected to a solution heat treatment step. The solution heat treatment step may be any suitable treatment of the product that results in the solubilization of soluble particles. The cast, homogenized or rolled product may be heated to a peak metal temperature (PMT) of up to 590°C (e.g., 400°C to 590°C) and soaked for a period of time at the PMT to form a hot product. For example, the cast, homogenized or rolled product may be soaked at 480°C for up to 30 minutes (e.g., 0 seconds, 60 seconds, 75 seconds, 90 seconds, 5 minutes, 10 minutes, 20 minutes, 25 minutes or 30 minutes) of soaking time. After heating and soaking, the hot product is rapidly cooled to a temperature between 500°C and 200°C at a rate greater than 200°C / second to form a heat-treated product. In one example, the hot product is cooled to a temperature between 450°C and 200°C at a quenching rate greater than 200°C / second. Optionally, in other cases, the cooling rate may be faster. Optionally, in other cases, the temperature may be lower. In one example, the hot product is cooled to a temperature between 450°C and 200°C at a quenching rate greater than 200°C / second.
[0060] After quenching, the heat treated product may optionally be subjected to a pre-aging treatment by reheating before coiling. The pre-aging treatment may be performed at a temperature of about 70°C to about 125°C for a period of up to 6 hours. For example, the pre-aging treatment may be performed at a temperature of about 70°C, about 75°C, about 80°C, about 85°C, about 90°C, about 95°C, about 100°C, about 105°C, about 110°C, about 115°C, about 120°C, or about 125°C. Optionally, the pre-aging treatment may be performed for about 30 minutes, about 1 hour, about 2 hours, about 3 hours, about 4 hours, about 5 hours, or about 6 hours. The pre-aging treatment may be performed by passing the heat treated product through a heating device, such as a device that emits radiant heat, convection heat, induction heat, infrared heat, or the like.
[0061] Cast products as described herein can be used to manufacture products in the form of thin plates (including foils), plates or other suitable products. For example, plates including products as described herein can be prepared in the following manner: in a homogenization step, ingots are processed, or products are cast in a continuous casting machine, followed by a hot rolling step. In the hot rolling step, cast products can be hot rolled to a specification of 200 mm thick or less (for example, about 10 mm to about 200 mm). For example, cast products can be hot rolled into plates with the following final specification thickness: about 10 mm to about 175 mm, about 15 mm to about 150 mm, about 20 mm to about 125 mm, about 25 mm to about 100 mm, about 30 mm to about 75 mm, or about 35 mm to about 50 mm. In some cases, plates can be rolled into thinner metal products, such as thin plates or foils.
[0062] In addition to casting and rolling, other techniques may be used to produce aluminum alloys or other metal products, such as foils. In some examples, a powder-based sintering or melting process may be used, optionally in conjunction with rolling or other processing techniques. In some examples, the metal product may be produced using selective laser melting, direct metal laser sintering, laser powder bed fusion, or other additive manufacturing techniques. In some examples, the metal product produced by a powder-based, additive manufacturing, or composite engineering process may be rolled to at least partially consolidate and / or produce a foil from the metal product.
[0063] Example Metals and Metal Alloys
[0064] Methods for preparing and using metals and metal alloys (including aluminum, aluminum alloys, etc.), the resulting metals and metal alloys, and devices incorporating the metals and metal alloys are described herein. In some examples, the metals used in the methods and devices described herein include aluminum alloys, such as 1xxx series aluminum alloys, 2xxx series aluminum alloys, 3xxx series aluminum alloys, 4xxx series aluminum alloys, 5xxx series aluminum alloys, 6xxx series aluminum alloys, 7xxx series aluminum alloys, or 8xxx series aluminum alloys. In some examples, the materials used in the methods described herein include non-ferrous materials, including aluminum, aluminum alloys, and aluminum-based composite materials, such as including aluminum and non-aluminum components, such as silicon, tin, indium, gallium, antimony, lead, nickel, copper, zinc, carbon, germanium, silver, etc. In some examples, iron-containing aluminum alloys can be used in the methods and devices described herein.
[0065] As non-limiting examples, exemplary 1xxx series aluminum alloys for use in the methods and apparatus described herein may include AA1100, AA1100A, AA1200, AA1200A, AA1300, AA1110, AA1120, AA1230, AA1230A, AA1235, AA1435, AA1145, AA1345, AA1445, AA1150, AA1350, AA1350A, AA1450, AA1370, AA1275, AA1185, AA1285, AA1385, AA1188, AA1190, AA1290, AA1193, AA1198, or AA1199.
[0066] Non-limiting exemplary 2xxx series aluminum alloys for use in the methods and apparatuses described herein may include AA2001, AA2002, AA2004, AA2005, AA2006, AA2007, AA2007A, AA2007B, AA2008, AA2009, AA2010, AA2011, AA2011A, AA2111, AA2111A, AA2111B, AA2012, AA2013, AA2014, AA2015, AA2016, AA2017, AA2018, AA2019, AA2020, AA2021 AA2014A, AA2214, AA2015, AA2016, AA2017, AA2017A, AA2117, AA2018, AA2218, AA2618, AA2618A, AA2219 ,AA2319,AA2419,AA2519,AA2021,AA2022,AA2023,AA2024,AA2024A,AA2124,AA2224,AA2224A,AA2324, AA2424, AA2524, AA2624, AA2724, AA2824, AA2025, AA2026, AA2027, AA2028, AA2028A, AA2028B, AA2028C ,AA2029,AA2030,AA2031,AA2032,AA2034,AA2036,AA2037,AA2038,AA2039,AA2139,AA2040,AA2041,AA 2044, AA2045, AA2050, AA2055, AA2056, AA2060, AA2065, AA2070, AA2076, AA2090, AA2091, AA2094, AA20 95, AA2195, AA2295, AA2196, AA2296, AA2097, AA2197, AA2297, AA2397, AA2098, AA2198, AA2099 or AA2199.
[0067] Non-limiting exemplary 3xxx series aluminum alloys for use in the methods and apparatus described herein may include AA3002, AA3102, AA3003, AA3103, AA3103A, AA3103B, AA3203, AA3403, AA3004, AA3004A, AA3104, AA3204, AA3304, AA3005, AA3005A, AA3105, AA3105A, AA3105B, AA3203, AA3403, AA3004, AA3004A, AA3104, AA3204, AA3304, AA3005 AA3007, AA3107, AA3207, AA3207A, AA3307, AA3009, AA3010, AA3110, AA3011, AA3012, AA3012A, AA3013, AA3014, AA3015, AA3016, AA3017, AA3019, AA3020, AA3021, AA3025, AA3026, AA3030, AA3130, or AA3065.
[0068] Non-limiting exemplary 4xxx series aluminum alloys for use in the methods and apparatuses described herein may include AA4045, AA4004, AA4104, AA4006, AA4007, AA4008, AA4009, AA4010, AA4013, AA4014, AA4015, AA4015A, AA4115, AA4016, AA4017, AA4018, AA4019, AA4020, AA4021, AA4026, AA4032, AA4043, AA4043A, AA4143, AA4343, AA4643, AA4943, AA4044, AA4145, AA4145A, AA4046, AA4047, AA4047A, or AA4147.
[0069] Non-limiting exemplary 5xxx series aluminum alloys for use in the methods, products and apparatus described herein may include AA5182, AA5183, AA5005, AA5005A, AA5205, AA5305, AA5505, AA5605, AA5006, AA5106, AA5010, AA5110, AA5110A, AA5210, AA5310, AA5016, AA5017, AA5018, AA5018A, AA5019, AA5019A, AA5110, AA5111A, AA5210, AA5310, AA5016, AA5017, AA5018, AA5018A, AA5019, AA5019A, AA5110 9. AA5119A, AA5021, AA5022, AA5023, AA5024, AA5026, AA5027, AA5028, AA5040, AA5140, AA5041, AA5042, AA5043, AA5 049, AA5149, AA5249, AA5349, AA5449, AA5449A, AA5050, AA5050A, AA5050C, AA5150, AA5051, AA5051A, AA5151, AA525 1. AA5251A, AA5351, AA5451, AA5052, AA5252, AA5352, AA5154, AA5154A, AA5154B, AA5154C, AA5254, AA5354, AA5454, AA5554, AA5654, AA5654A, AA5754, AA5854, AA5954, AA5056, AA5356, AA5356A, AA5456, AA5456A, AA5456B, AA5556, AA 5556A, AA5556B, AA5556C, AA5257, AA5457, AA5557, AA5657, AA5058, AA5059, AA5070, AA5180, AA5180A, AA5082, AA51 82. AA5083, AA5183, AA5183A, AA5283, AA5283A, AA5283B, AA5383, AA5483, AA5086, AA5186, AA5087, AA5187 or AA5088.
[0070] Non-limiting exemplary 6xxx series aluminum alloys for use in the methods and apparatuses described herein may include AA6101, AA6101A, AA6101B, AA6201, AA6201A, AA6401, AA6501, AA6002, AA6003, AA6103, AA6005, AA6005A, AA6005B, AA6005C, AA6105, AA6205, AA6305, AA6006, AA6106, AA6206, AA6306, AA6008, AA6009, AA6010, AA6110, AA6110A, AA6011, AA6111, AA6012, AA6012A, AA6013, AA6113, AA6014, AA6015, A A6016, AA6016A, AA6116, AA6018, AA6019, AA6020, AA6021, AA6022, AA6023, AA6024, AA6025, AA6026, AA6027, AA6 028, AA6031, AA6032, AA6033, AA6040, AA6041, AA6042, AA6043, AA6151, AA6351, AA6351A, AA6451, AA6951, AA605 3. AA6055, AA6056, AA6156, AA6060, AA6160, AA6260, AA6360, AA6460, AA6460B, AA6560, AA6660, AA6061, AA6061A , AA6261, AA6361, AA6162, AA6262, AA6262A, AA6063, AA6063A, AA6463, AA6463A, AA6763, A6963, AA6064, AA6064A, AA6065, AA6066, AA6068, AA6069, AA6070, AA6081, AA6181, AA6181A, AA6082, AA6082A, AA6182, AA6091, or AA6092.
[0071] Non-limiting exemplary 7xxx series aluminum alloys for use in the methods and apparatus described herein may include AA7011, AA7019, AA7020, AA7021, AA7039, AA7072, AA7075, AA7085, AA7108, AA7108A, AA7015, AA7017, AA7018, AA7019A, AA7024, AA7025 ... 8. AA7030, AA7031, AA7033, AA7035, AA7035A, AA7046, AA7046A, AA7003, AA7004, AA7005, AA7 009, AA7010, AA7011, AA7012, AA7014, AA7016, AA7116, AA7122, AA7023, AA7026, AA7029, AA7 129, AA7229, AA7032, AA7033, AA7034, AA7036, AA7136, AA7037, AA7040, AA7140, AA7041, AA7 049, AA7049A, AA7149, AA7204, AA7249, AA7349, AA7449, AA7050, AA7050A, AA7150, AA7250, A AA7055, AA7155, AA7255, AA7056, AA7060, AA7064, AA7065, AA7068, AA7168, AA7175, AA7475, AA7076, AA7178, AA7278, AA7278A, AA7081, AA7181, AA7185, AA7090, AA7093, AA7095, or AA7099.
[0072] Non-limiting exemplary 8xxx series aluminum alloys for use in the methods and apparatus described herein may include AA8005, AA8006, AA8007, AA8008, AA8010, AA8011, AA8011A, AA8111, AA8211, AA8112, AA8014, AA8015, AA8016, AA8017, AA8018, AA8019, AA8020, AA8021, AA8022, AA8023, AA8024, AA8025, AA8026, AA8027, AA8028, AA8029, AA8030, AA8031, AA8032, AA8033, AA8034, AA8035, AA8036, AA8037, AA8038, AA8039, AA8040, AA8041, AA8042, AA8043, AA8044, AA8045, AA8046, AA8047, AA8048, AA8049, AA8050, AA8051 21. AA8021A, AA8021B, AA8022, AA8023, AA8024, AA8025, AA8026, AA8030, AA8130, AA8040, AA8050, AA8150, AA8076, AA8076A, AA8176, AA8077, AA8177, AA8079, AA8090, AA8091, or AA8093.
[0073] Methods of using the disclosed aluminum alloy products
[0074] The aluminum alloy products described herein can be used in battery applications. For example, the disclosed aluminum alloy products can be used as current collectors and / or electrode materials for batteries or electrochemical cells.
[0075] The aluminum alloy products and methods described herein can also be used in electronic applications. For example, the aluminum alloy products and methods described herein can be used to prepare housings for electronic devices including batteries. In some examples, the aluminum alloy products can be used to prepare housings for mobile phones (e.g., smart phones), tablet chassis, single-cell and multi-cell batteries, and other portable electronic devices.
[0076] As described above, solid-state electrochemical cells doped with solid electrolytes can advantageously be doped with aluminum materials as anode active materials. As alloyed electrodes, aluminum can exhibit higher energy storage density than commonly used anode materials (such as graphite) for lithium-ion batteries because aluminum has a higher storage potential for lithium than graphite. Although the storage capacity of aluminum may not be as high as that of metallic lithium, aluminum alloyed anodes are not affected by dendrite formation, thus providing safer operation of rechargeable batteries or secondary batteries compared to lithium metal batteries.
[0077] In addition, avoiding the use of graphite as an anode material can not only increase the anode storage capacity, but also limit the use of wet processing, because the aluminum-based alloyed anode can be incorporated as a material film or foil, rather than a slurry deposited on the collector. In some cases, the aluminum-based alloyed anode can allow for use as an anode material without a collector, but a conventional anode collector, such as copper foil, can also be used. In some cases, the collector may include aluminum foil, such as an aluminum foil that is different from the active material of the anode. In some examples, a protected aluminum foil can be used as an anode collector, such as described in International Application Publication No. WO 2021 / 184035, which is hereby incorporated by reference.
[0078] Incorporating aluminum-based materials as active materials into solid-state electrochemical cells can also allow recycled content materials to be directly incorporated into the electrodes of the electrochemical cells. For example, the anode active material of the solid-state electrochemical cells described herein can include aluminum alloys doped with a large amount of recycled content, such as up to 10%, up to 20%, up to 30%, up to 40%, or more.
[0079] The use of solid electrolyte components can also enhance the safety, manufacturability and other characteristics of the battery system. Lithium-ion batteries generally incorporate liquid organic solvents, such as carbonate solvents, in the electrolyte. Such solvents are generally flammable and produce undesirable side reactions at the surface of the anode active material at the potentials involved. These side reactions can form a solid electrolyte interphase (SEI) layer, which degrades performance and reduces capacity.
[0080] The use of liquid electrolytes with aluminum-based active materials can exacerbate the formation of the SEI layer because the aluminum-based active materials undergo volume changes when absorbing or releasing lithium ions. As the active material absorbs lithium, the active material expands, thereby disrupting any SEI material on the surface of the active material and exposing fresh active material to the liquid electrolyte, which can further react at the exposed active material and form additional SEI material. In this way, liquid electrolytes used with aluminum-based active materials can allow SEI materials to accumulate above the active material.
[0081] However, when a solid electrolyte is used, such accumulation of SEI materials may not occur. For example, a solid electrolyte may include solid materials, such as ceramic sulfate materials, such as lithium argyrodite materials (e.g., Li6PS5Cl), which do not flow like liquid electrolytes. When such a solid electrolyte encounters volume expansion of the anode active material due to absorption of lithium, the solid electrolyte cannot flow into the cracks and interfaces of the exposed fresh active material, thereby limiting the formation of SEI materials.
[0082] Pressure may be applied between the solid electrolyte and the aluminum-based active anode material to ensure good electrical and ionic communication during charge or discharge and to account for volume contraction or expansion due to release or absorption of lithium atoms or ions. Such pressure may be applied as stacking pressure between the anode and cathode with the solid electrolyte located between them. Stacking pressure may be applied by a sleeve or other component. Example stacking pressures may be in the range of 0.1 MPa to 30 MPa.
[0083] Figure 2 A schematic diagram of an example solid-state electrochemical cell 200 is provided, the solid-state electrochemical cell comprising an anode active material 205, a cathode active material 210, a solid electrolyte 215, an anode current collector 220, and a cathode current collector 225. In a conventional lithium-ion battery system, the cathode current collector comprises a high-purity aluminum foil, the cathode active material comprises a lithium metal oxide, a porous non-conductive material impregnated with a liquid electrolyte comprising an organic solvent and a lithium salt is located between the anode active material and the cathode active material, the anode active material comprises graphite, and the anode current collector comprises copper foil. Some of these materials may be used in solid-state electrochemical cells, but other materials, such as liquid electrolytes, may not be used.
[0084] For example, cathode active material 210 and cathode current collector 225 can be doped with materials used in conventional battery systems. Optionally, cathode current collector 225 can include aluminum, such as in the form of aluminum alloy foil. In some cases, cathode current collector 225 can include a high purity aluminum alloy, such as 99.00 wt% Al or more. The use of a high purity aluminum alloy can be used to maintain the conductivity of cathode current collector 225 at a level as high as possible. Cathode active material 210 can include any suitable cathode active material, including but not limited to an alkali metal host material or an alkali metal-transition metal oxide cathode active material, such as lithium nickel manganese cobalt oxide, lithium nickel cobalt aluminum oxide, lithium manganese oxide, lithium iron phosphate or lithium metal cobalt oxide.
[0085] The anode active material 205 may include, for example, an alkali metal alloying anode. Lithium may form an alloy with aluminum at the potential encountered at the anode, wherein during charging, lithium ions may be reduced and incorporated into the bulk of the aluminum material in the form of an alloy. During discharge, lithium may be oxidized and released from the alkali metal alloying anode in the form of lithium ions. The aluminum used for the anode active material 205 may be a foil, such as a foil comprising aluminum or an aluminum alloy, optionally a composite or mixed metal foil, such as one or more other metals or semiconductors, such as silicon, tin, indium, gallium, antimony, lead, nickel, copper, zinc, carbon, germanium, silver or the like, optionally in an amount up to 50 mol%. As described herein, the foil may be processed using metal casting and rolling processes, but other techniques may also be used to prepare the foil, including powder-based sintering or laser melting processes, such as laser powder bed fusion techniques. The anode active material can exhibit a specific capacity of about 300 mAh / g to about 1000 mAh / g or more, such as 300 mAh / g to 350 mAh / g, 400 mAh / g to 450 mAh / g, 450 mAh / g to 500 mAh / g, 500 mAh / g to 550 mAh / g, 550 mAh / g to 600 mAh / g, 600 mAh / g to 650 mAh / g, 650 mAh / g to 700 mAh / g, 700 mAh / g to 750 mAh / g, 750 mAh / g to 800 mAh / g, 800 mAh / g to 850 mAh / g, 850 mAh / g to 900 mAh / g, 900 mAh / g to 950 mAh / g, or 950 mAh / g to 1000 mAh / g. In some examples, the specific capacity may be higher, such as if other components with higher specific capacity are included in the anode active material, such as silicon.
[0086] The anode active material 205 may include an aluminum alloy or a multi-component system, such as a eutectic alloy, a solid solution alloy, a mixed metal system, or a composite particle system. In some examples, the anode active material 205 may include a multi-component foil including aluminum and one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc, or silver. In some examples, the amount of aluminum in the anode active material 205 may be from about 40 wt % to about 100 wt % aluminum, such as 40 wt % to 45 wt %, 45 wt % to 50 wt %, 50 wt % to 55 wt %, 55 wt % to 60 wt %, 60 wt % to 65 wt %, 65 wt % to 70 wt %, 70 wt % to 75 wt %, 75 wt % to 80 wt %, 80 wt % to 85 wt %, 85 wt % to 90 wt %, 90 wt % to 95 wt %, 95 wt % to 99 wt %, 99 wt % to 99.9 wt %, or 99.9 wt % to 99.99 wt %. In some examples, the amount of non-aluminum elements (such as one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc, or silver) can be about 0.1 wt % to about 60 wt %, or less than or about 1 wt %, such as 0.1 wt % to 0.5 wt %, 0.5 wt % to 1 wt % to 2 wt %, 2 wt % to 5 wt %, 5 wt % to 10 wt %, 10 wt % to 15 wt %, 15 wt % to 20 wt %, 20 wt % to 25 wt %, 25 wt % to 30 wt %, 30 wt % to 35 wt %, 35 wt % to 40 wt %, 40 wt % to 45 wt %, 45 wt % to 50 wt %, 50 wt % to 55 wt %, or 55 wt % to 60 wt %. In some examples, the anode active material 205 can include a composite material including a first plurality of aluminum or aluminum alloy particles and a second plurality of particles selected from at least one of metal particles or non-metal particles. Additional details regarding composite anodes can be found in U.S. Provisional Application No. 63 / 261,216, which is hereby incorporated by reference.
[0087] Anode current collector 220 may include any suitable material, such as copper or other conductive materials, such as aluminum. Copper may be suitable for use as anode current collector 220 because copper does not react at the potential involved in the lithium battery system and exhibits high conductivity. Aluminum can form an alloy with lithium at the potential involved, making it usable as an anode active material 205, but such properties may not be desirable for using aluminum as an anode current collector 220. However, in some examples, aluminum may be used as an anode current collector 220 because aluminum is also a highly conductive material and can be configured as a foil. Optionally, when the anode active material 205 includes a metal foil, the anode current collector 220 may not be used because an electrical connection may be established directly with the anode active material 205 to provide electronic conduction to / from an external circuit (e.g., a load or power supply). In some cases, aluminum may be used as an anode current collector 220 in the form of a protected aluminum foil.
[0088] Anode current collector 220 can also be made with engineered structure.By engineering the structure, the structure can include extra space and microporosity.Not bound by theory, such extra space and / or microporosity can compensate for the volume change in anode current collector 220.This engineered structure can be formed using various methods, including powder metallurgy, micropore or nanopore structure formed by additive manufacturing, using metal foam, perforation formed by laser or deep etching, dealloying (e.g., chemical dealloying) or other methods.In some examples, the engineered structure can be processed by rolling to at least partially consolidate or otherwise manufacture foil by the engineered structure.In some examples, the engineered structure can include or couple, engage or be bonded to solid aluminum-based or aluminum alloy-based structure (e.g., foil) as a solid substrate layer.In some examples, the engineered structure can be coupled, engaged or bonded to a collector, such as a collector based on foil, such as a copper collector or a protected or coated aluminum or aluminum alloy collector (e.g., aluminum or aluminum foil coated with Fe, TiN, Ni or the like). Examples of aluminum-based current collectors, including protected or coated aluminum current collectors, are described in PCT International Application No. PCT / US2021 / 070250, which is hereby incorporated by reference.
[0089] Any suitable solid electrolyte 215 can be used in the solid electrochemical cell 200. For example, the solid electrolyte 215 can include ion-conducting and electrically insulating materials, such as inorganic solid electrolytes. In some cases, the solid electrolyte 215 can include a solid polymer electrolyte, a composite polymer electrolyte, a polymer gel electrolyte, or a gel electrolyte, but in some examples, the solid electrolyte 215 explicitly includes an inorganic solid electrolyte rather than a solid polymer electrolyte, a composite polymer electrolyte, or a gel electrolyte. Inorganic solid electrolytes include, but are not limited to, crystalline, glassy, or ceramic ion-conducting materials (e.g., alkali metal ion-conducting materials). Example solid electrolytes include, but are not limited to, solid electrolytes comprising one or more of the following: lithium superion conductors (LISICON), silver germanium sulfide materials (e.g., Li6PS5Cl), doped garnet materials (e.g., Li7La3Zr2O 12 ,LLZO),Li 10 GeP2S 12 and related materials, such as Li 10 SnP2S 12 , lithium phosphorus sulfide (e.g., Li3PS4) or lithium phosphorus oxynitride (LIPON). Suitable materials for solid electrolyte 215 may exhibit a carbonylation rate of greater than or about 10 -4 S / cm (e.g., 10 -4 S / cm to 0.01 S / cm).
[0090] Figure 3 A schematic diagram of another solid-state electrochemical cell 300 is provided. The solid-state electrochemical cell 300 may include components similar to or the same as the solid-state electrochemical cell 300. For example, the solid-state electrochemical cell 300 may include an anode active material 305, a cathode active material 310, a solid-state electrolyte 315, an anode current collector 320, and a cathode current collector 325. Such components may include the same materials as described above.
[0091] The solid-state electrochemical cell 300 also includes a protective coating 335 surrounding the anode current collector 320. The use of the protective coating 335 can allow the anode current collector 320 to include a material (such as aluminum) that forms an alloy with an alkali metal as a current collector without subjecting the anode current collector 320 to harmful effects that may occur during alloying. For example, the protective coating 335 may include a conductive material that blocks the transmission of lithium atoms, thereby allowing electrons to be conducted to the anode current collector 320 while preventing lithium atoms from reaching the anode current collector 320 and forming an alloy therewith. Example materials and configurations of the protective coating 335 are described in International Application Publication No. WO 2021 / 184035. In a non-limiting example, the protective coating 335 includes an iron coating.
[0092] The solid-state electrochemical cell 300 also includes an interface material 340 between the anode active material 305 and the solid electrolyte 315. In some examples, the interface material 340 corresponds to a SEI layer, which can be formed during the cycle of the solid-state electrochemical cell 300, or is an artificial SEI. In other examples, the interface material 340 is another material located between the anode active material 305 and the solid electrolyte 315, such as a polymer coating, a carbon coating, or an inorganic coating. In some examples, the interface material 340 can improve the contact between the anode active material 305 and the solid electrolyte 315 or improve the ionic conductivity between the anode active material 305 and the solid electrolyte 315, and / or provide, for example, a buffer for absorbing and / or releasing lithium ions. In some cases, the interface material 340 can prevent the formation of dendrites when the anode active material 305 is driven to absorb lithium exceeding its alloying capacity.
[0093] Without limitation, any suitable size of anode active material, anode current collector, cathode active material, cathode current collector, solid electrolyte, interface material or protective coating may be used. In some examples, the thickness of the solid electrolyte may be about 10 μm to about 300 μm, such as 10 μm to 20 μm, 20 μm to 30 μm, 30 μm to 40 μm, 40 μm to 50 μm, 50 μm to 75 μm, 75 μm to 100 μm, 100 μm to 125 μm, 125 μm to 150 μm, 150 μm to 175 μm, 175 μm to 200 μm, 200 μm to 250 μm, or 250 μm to 300 μm. In some examples, the thickness of the anode or anode active material may be about 5 μm to about 60 μm, such as 5 μm to 10 μm, 10 μm to 15 μm, 15 μm to 20 μm, 20 μm to 25 μm, 25 μm to 30 μm, 30 μm to 35 μm, 35 μm to 40 μm, 40 μm to 45 μm, 45 μm to 50 μm, 50 μm to 55 μm, or 55 μm to 60 μm.
[0094] The examples disclosed herein will be used to further illustrate aspects of the present invention, but will not constitute any limitation of the present invention at the same time. On the contrary, it is clearly understood that it may be necessary to resort to various embodiments, modifications and equivalents thereof that can be thought of by those skilled in the art after reading the description herein without departing from the spirit of the present invention. Unless otherwise specified, the examples and embodiments described herein may also utilize conventional procedures. Some programs are described herein for illustrative purposes.
[0095] Example 1
[0096] This example describes details of comparative testing of electrochemical cells including a solid electrochemical cell doped with an aluminum active anode material and a solid electrolyte and a comparative cell doped with an aluminum active anode material and a liquid electrolyte.
[0097] The chemical formula is LiNi 0.6 Mn 0.2 Co 0.2 Solid-state electrochemical cells were prepared using a lithium nickel manganese cobalt oxide cathode of O2 (NMC-622) and an aluminum alloy-based anode. The Li6PS5Cl solid electrolyte is located between the cathode and the anode. As a reference cell, the same aluminum alloy-based anode was assembled into a half-cell battery with a liquid electrolyte, using a lithium metal counter electrode, wherein a porous spacer was provided between the aluminum alloy-based anode and the lithium metal counter electrode, and the porous spacer was impregnated with an electrolyte containing 1.0 M lithium bis(fluorosulfonyl)imide (LiFSI) and 1.0 M lithium difluorooxalate borate (LiDFOB) in a 3:7 mixture by volume of fluoroethylene carbonate: diethyl carbonate (FEC: DEC). The aluminum alloy-based anode had a thickness of approximately 30 μm and a diameter of 1 cm, and was either high-purity aluminum or an aluminum alloy with 6 atomic % indium. The solid-state cell was first cycled at C / 40 in two cycles, then at C / 20 in three cycles, and then at C / 10 in the remaining cycles. A stacking pressure of approximately 24 MPa is applied to the solid-state battery cell.
[0098] The solid-state cells were cycled between 2.2 V and 4.0 V, and the areal capacity (mAh cm) was monitored based on the number of cycles. -2 ). Figure 4 The anode to cathode capacity ratio (N:P) of the solid-state battery is 1.44, and Figure 7 The anode to cathode capacity ratio (N:P) of the solid-state cell in the embodiment is 1.60. The reference half-cell was cycled and controlled to have 3.0 mAh cm during each step of lithiation of the aluminum alloy-based anode. -2 area capacity until the reference cell fails.
[0099] exist Figure 4 and Figure 7 The voltage versus capacity curves of the first, second, and tenth cycles of two example solid-state electrochemical cells are shown in FIG. Fig.10 The voltage-to-capacity curves for the first, second, and tenth cycles of the reference half-cell are shown in FIG. Figure 5 and Figure 8 The capacity versus cycle number of two example solid-state electrochemical cells is shown in FIG. Fig.11 A graph of the capacity of a reference half-cell versus the number of cycles is shown in FIG. Figure 6 and Fig. 9The coulombic efficiency versus cycle number of two example solid-state electrochemical cells is shown in Fig.12 A graph of the coulombic efficiency versus cycle number for a reference half-cell is shown in FIG. Figure 6 and Fig. 9 As shown, the example solid-state electrochemical cells exhibited an initial coulombic efficiency (ICE) of 58% and 86% for the first cycle. The reference half-cell exhibited an initial coulombic efficiency (ICE) of about 91% for the first cycle.
[0100] The example solid-state electrochemical cells exhibit very high coulombic efficiencies compared to the reference half-cells, wherein the coulombic efficiencies of the solid-state electrochemical cells are generally above 97% (and for one of the solid-state cells, above 99% after 10 cycles), while the reference half-cell peaks at approximately 8 or 10 cycles and then steadily decreases until a sharp drop is observed at approximately 45 cycles.
[0101] Illustrative aspects
[0102] As used below, any reference to a series of aspects (e.g., “Aspects 1 to 4”) or an unlisted group of aspects (e.g., “any previous or subsequent aspect”) should be understood as a separate reference to each of those aspects (e.g., “Aspects 1 to 4” should be understood as “Aspect 1, Aspect 2, Aspect 3, or Aspect 4”).
[0103] Aspect 1 is a solid-state battery comprising: an anode comprising aluminum as an anode active material; a cathode; and a solid-state electrolyte between the anode and the cathode.
[0104] Aspect 2 is the solid-state battery of any preceding or subsequent aspect, wherein the anode comprises an aluminum-based alkali metal alloyed anode.
[0105] Aspect 3 is the solid-state battery of any preceding or subsequent aspect, wherein the alkali metal is lithium.
[0106] Aspect 4 is the solid-state battery of any preceding or subsequent aspect, wherein the anode comprises an aluminum alloy or a recycled content aluminum alloy.
[0107] Aspect 5 is the solid-state battery of any preceding or subsequent aspect, wherein the anode comprises an aluminum-based multi-component foil comprising aluminum and one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc, or silver.
[0108] Aspect 6 is the solid-state battery of any previous or subsequent aspect, wherein the anode comprises a foil comprising 40 wt % to 99 wt % aluminum and 30 wt % to 60 wt % of one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc, or silver.
[0109] Aspect 7 is the solid-state battery of any preceding or subsequent aspect, wherein the anode has a thickness of 5 μm to 60 μm.
[0110] Aspect 8 is the solid-state battery of any preceding or subsequent aspect, wherein the anode exhibits a specific capacity of 300 mAh / g to 1000 mAh / g.
[0111] Aspect 9 is the solid-state battery of any preceding or subsequent aspect, wherein the anode comprises a composite foil including a first plurality of aluminum and aluminum alloy particles and a second plurality of particles selected from at least one of metallic particles or non-metallic particles.
[0112] Aspect 10 is the solid-state battery of any preceding or subsequent aspect, wherein the solid-state electrolyte is an inorganic solid electrolyte.
[0113] Aspect 11 is a solid-state battery of any previous or subsequent aspect, wherein the solid-state electrolyte comprises lithium argyrodite material, Li6PS5Cl, lithium superion conductor (LISICON), doped garnet material, Li7La3Zr2O 12 (LLZO), Li 10 GeP2S 12 , Li 10 SnP2S 12 , lithium phosphorus sulfide (Li3PS4), lithium phosphorus oxynitride (LIPON), polymer solid electrolyte or gel polymer electrolyte.
[0114] Aspect 12 is the solid-state battery of any preceding or subsequent aspect, wherein the solid-state electrolyte has a thickness of 10 μm to 300 μm.
[0115] Aspect 13 is the solid-state battery of any preceding or subsequent aspect, wherein the cathode comprises an alkali metal host material or an alkali metal-transition metal oxide cathode active material.
[0116] Aspect 14 is the solid-state battery of any preceding or subsequent aspect, wherein the cathode comprises lithium nickel manganese cobalt oxide, lithium nickel cobalt aluminum oxide, lithium manganese oxide, lithium iron phosphate, lithium cobalt oxide, a conversion cathode, FeS2, FeF3, a sulfur-based cathode, or sulfur.
[0117] Aspect 15 is the solid-state battery of any preceding or subsequent aspect, further comprising one or more of: a cathode current collector in contact with the cathode; or an anode current collector in contact with the anode.
[0118] Aspect 16 is the solid-state battery of any preceding or subsequent aspect, wherein the anode current collector comprises a protected aluminum alloy foil.
[0119] Aspect 17 is the solid-state battery of any preceding or subsequent aspect, wherein a stacking pressure is applied between the anode and the cathode, wherein the stacking pressure is 0.1 MPa to 30 MPa.
[0120] Aspect 18 is the solid-state battery of any preceding or subsequent aspect, further comprising an interface material between the anode and the solid-state electrolyte.
[0121] Aspect 19 is the solid-state battery of any preceding or subsequent aspect, wherein the interface material comprises a solid electrolyte interphase, an artificial solid electrolyte interphase, a polymer coating, a carbon coating, or an inorganic coating.
[0122] Aspect 20 is a method of manufacturing a solid-state battery, the method comprising: providing an anode, the anode comprising aluminum as an anode active material; providing a cathode; and positioning a solid-state electrolyte between the anode and the cathode.
[0123] Aspect 21 is the method of any preceding or subsequent aspect, wherein providing the anode comprises preparing an aluminum-based multi-component foil comprising aluminum and one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc, or silver.
[0124] Aspect 22 is a method of any previous or subsequent aspect, wherein preparing the aluminum-based multi-component foil comprises: casting an aluminum-based multi-component product, the aluminum-based multi-component product comprising aluminum and one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc or silver to produce an aluminum-based multi-component product; and rolling the aluminum-based multi-component product into a foil.
[0125] Aspect 23 is a method of any previous or subsequent aspect, wherein preparing the aluminum-based multi-component foil comprises: obtaining a powder mixture of aluminum and one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc or silver; and subjecting the powder mixture to a laser powder bed fusion process to produce an aluminum-based multi-component product.
[0126] Aspect 24 is a method of any previous or subsequent aspect, wherein preparing the aluminum-based multi-component foil comprises: cumulatively rolling and bonding aluminum or an aluminum alloy and a certain amount of one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc or silver to produce an aluminum-based multi-component product.
[0127] Aspect 25 is the method of any preceding or subsequent aspect, wherein preparing the aluminum-based multi-component foil comprises: forming a microporous or nanoporous aluminum-based multi-component product using powder metallurgy, additive manufacturing, metal foam, perforation by laser or deep etching, or dealloying.
[0128] Aspect 26 is the method of any previous aspect, wherein preparing the aluminum-based multi-component foil further comprises: rolling the aluminum-based multi-component product into a foil.
[0129] Aspect 27 is the method of any preceding or subsequent aspect, further comprising one or more of: contacting the anode with an anode current collector; or contacting the cathode with a cathode current collector.
[0130] Aspect 28 is the method of any previous aspect, wherein the solid-state battery comprises the solid-state battery of any previous aspect.
[0131] All patents and disclosures cited herein are incorporated by reference in their entirety. The foregoing description of the embodiments, including the illustrated embodiments, is presented for the purpose of illustration and description only and is not intended to be exhaustive or limited to the precise form disclosed. For those skilled in the art, numerous modifications, variations and uses of the present invention will be apparent.
Claims
1. A solid-state battery comprising: an anode comprising aluminum as an anode active material; a cathode; and A solid electrolyte is provided between the anode and the cathode.
2. The solid-state battery of claim 1, wherein the anode comprises an aluminum-based alkali metal alloyed anode.
3. The solid-state battery of claim 2, wherein the alkali metal is lithium.
4. The solid-state battery of claim 1, wherein the anode comprises an aluminum alloy, a recycled content aluminum alloy, or an aluminum brazing alloy.
5. The solid-state battery of claim 1, wherein the anode comprises an aluminum-based multi-component foil comprising aluminum and one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc, or silver.
6. The solid-state battery of claim 1, wherein the anode comprises a foil comprising 40 to 99 weight percent aluminum and 30 to 60 weight percent of one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc, or silver. 7 . The solid-state battery according to claim 1 , wherein the thickness of the anode is 5 μm to 60 μm.
8. The solid-state battery of claim 1, wherein the anode exhibits a specific capacity of 300 mAh / g to 1000 mAh / g.
9. The solid-state battery of claim 1, wherein the anode comprises a composite foil including a first plurality of aluminum and aluminum alloy particles and a second plurality of particles selected from at least one of metallic particles or non-metallic particles.
10. The solid-state battery according to claim 1, wherein the solid-state electrolyte is an inorganic solid electrolyte.
11. The solid-state battery according to claim 1, wherein the solid-state electrolyte comprises lithium argyrodite material, Li6PS5Cl, lithium superion conductor (LISICON), doped garnet material, Li7La3Zr2O 12 (LLZO), Li 10 GeP2S 12 , Li 10 SnP2S 12 , lithium phosphorus sulfide (Li3PS4), lithium phosphorus oxynitride (LIPON), polymer solid electrolyte or gel polymer electrolyte. 12 . The solid-state battery according to claim 1 , wherein the solid-state electrolyte has a thickness of 10 μm to 300 μm.
13. The solid-state battery of claim 1, wherein the cathode comprises an alkali metal host material or an alkali metal-transition metal oxide cathode active material.
14. A solid-state battery as described in claim 1, wherein the cathode comprises lithium nickel manganese cobalt oxide, lithium nickel cobalt aluminum oxide, lithium manganese oxide, lithium iron phosphate, lithium cobalt oxide, a conversion cathode, FeS2, FeF3, a sulfur-based cathode or sulfur.
15. The solid-state battery of claim 1, further comprising one or more of the following: a cathode current collector in contact with the cathode; or An anode current collector is in contact with the anode.
16. The solid-state battery of claim 15, wherein the anode current collector comprises a protected aluminum alloy foil. 17 . The solid-state battery of claim 1 , wherein a stacking pressure is applied between the anode and the cathode, wherein the stacking pressure is 0.1 MPa to 30 MPa.
18. The solid-state battery of claim 1, further comprising an interface material between the anode and the solid-state electrolyte.
19. The solid-state battery of claim 1, wherein the interface material comprises a solid electrolyte interphase, an artificial solid electrolyte interphase, a polymer coating, a carbon coating, or an inorganic coating.
20. A method for manufacturing a solid-state battery, the method comprising: providing an anode comprising aluminum as an anode active material; providing a cathode; as well as A solid state electrolyte is positioned between the anode and the cathode.
21. The method of claim 20, wherein providing the anode comprises: An aluminum-based multi-component foil is prepared, the aluminum-based multi-component foil comprising aluminum and one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc or silver.
22. The method of claim 21, wherein preparing the aluminum-based multi-component foil comprises: casting an aluminum-based multi-component product comprising aluminum and one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc, or silver to produce an aluminum-based multi-component product; and The aluminum-based multi-component product is rolled into a foil.
23. The method of claim 21, wherein preparing the aluminum-based multi-component foil comprises: obtaining a powder mixture of aluminum and one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc or silver; and The powder mixture is subjected to a laser powder bed fusion process to produce an aluminum-based multi-component product.
24. The method of claim 21, wherein preparing the aluminum-based multi-component foil comprises: Aluminum or an aluminum alloy and a certain amount of one or more of silicon, tin, indium, gallium, antimony, lead, nickel, copper, carbon, germanium, zinc or silver are cumulatively rolled to produce an aluminum-based multi-component product.
25. The method of claim 21, wherein preparing the aluminum-based multi-component foil comprises: Microporous or nanoporous aluminum-based multi-component products are formed using powder metallurgy, additive manufacturing, metal foams, perforation by laser or deep etching, or dealloying.
26. The method of any one of claims 23 to 25, wherein preparing the aluminum-based multi-component foil further comprises: The aluminum-based multi-component product is rolled into a foil.
27. The method of claim 20, further comprising one or more of the following: contacting the anode with an anode current collector; or The cathode is in contact with a cathode current collector.
28. The method of any one of claims 20 to 27, wherein the solid-state battery comprises the solid-state battery of any one of claims 1 to 19.
Citation Information
Patent Citations
Distribution device, key information sharing system, method of controlling distribution device, and recording medium
US20210070250A1
Aluminum anode current collectors for lithium ion batteries
WO2021184035A1