Method for stabilizing calcium-arsenic slag by using copper tailings
By using the coordinated treatment of copper tailslag and flotation copper tailslag, and through acid solution stirring and evaporation crystallization technology, the problems of long stabilization treatment cycle and high energy consumption in the existing technology are solved, and calcium and arsenic slag are realized The rapid stabilization and low-cost treatment avoid secondary environmental pollution.
Patent Information
- Application Number
- CN202411278373.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-12
AI Technical Summary
The existing arsenic-containing waste slag stabilization technology has the problems of long treatment cycles, large capacity increase ratios, high energy consumption and easy to cause secondary pollution to the environment.
Copper tailings are used as a multifunctional stabilizer, and then mixed with flotation copper tailings is carried out by lime precipitation method, and acid solution is added for stirring and evaporation and crystallization, so as to re-establish the mineral phase in the calcium and arsenic slag to reduce the stability of arsenic.
It has achieved rapid stabilization of calcium and arsenic slag, reduced the leaching toxicity of arsenic, comply with the requirements of the "Hazardous Waste Landfill Pollution Control Standards", and has a simple process, low cost, and does not cause secondary pollution to the environment.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of stabilization of arsenic-containing waste slag, and in particular relates to a method for stabilizing calcium-arsenic slag by utilizing copper tailings. Background Art
[0002] Arsenic is a ubiquitous toxic nonmetal that is widely associated with nonferrous metal ores (such as copper, lead, zinc, antimony, and gold). It is estimated that my country's nonferrous metal industry discharges tens of thousands of tons of arsenic every year. Due to the high toxicity of arsenic and the limited market, most of the arsenic must be removed from arsenic-containing wastewater in the form of solid precipitation. The most common precipitation methods include lime neutralization, iron-arsenic co-precipitation, sulfide precipitation, and scorodite precipitation. Due to its relatively low cost and simple operation, lime neutralization is widely used for arsenic-containing wastewater treatment in most metal metallurgical industries around the world. However, the process inevitably produces a large amount of arsenic calcium slag, which is a hazardous solid waste with high arsenic content and poor stability. Calcium arsenite or calcium arsenate is unstable in the environment and usually shows high arsenic leaching concentrations, which may cause serious arsenic contamination in storage areas. Therefore, they must be handled safely and effectively. Today, stabilization technology has been widely used as a pre-landfill waste treatment strategy to reduce the environmental risks of arsenic-containing solid wastes. To date, a large number of studies have focused on the solidification of arsenic-containing solid wastes using cheap cementitious materials such as cement, fly ash, and geopolymers. However, these methods generally have disadvantages such as high volume expansion rate and poor long-term stability. Since calcium-containing agents and iron-containing agents are widely used in the stabilization of arsenic-contaminated soil and low-arsenic tailings, researchers have applied them to the stabilization of hazardous solid wastes, especially solid wastes with high arsenic content, in recent years. Among them, lime, calcium hydroxide and ferrous sulfate have become the most commonly used stabilizers due to their low cost.
[0003] Patent CN113443843B discloses a method for preparing a composite gelling agent for detoxification of arsenic-containing waste residues, wherein industrial waste residues, diatomaceous earth, and sodium hydroxide are prepared into a mixed solution, subjected to hydrothermal reaction, solid-liquid separation, roasted, ball-milled, and sieved to obtain a composite gelling agent, which can produce efficient and specific binding with free arsenic in arsenic-containing waste residues, produce strong physical and coordination adsorption, and form a dense coating structure in a short time to reduce the mobility of arsenic, thereby achieving the purpose of detoxification of arsenic-containing waste residues. However, this method has too many control conditions, and the activity of the composite gelling agent is easily inhibited.
[0004] Patent CN110606512B discloses a method for stabilizing arsenic calcium slag, which mixes arsenic calcium slag, water-soluble iron salt and water, and adjusts the pH to make the mixture undergo a chemical reaction to generate calcium iron arsenate, thereby achieving stabilization of the arsenic calcium slag. However, the chemical reaction time required for this method is too long, and the As concentration in the slurry after treatment does not reach the national standard limit for discharge, so a deep treatment process needs to be added.
[0005] Patent CN103028587A discloses a method for solidification treatment of arsenic calcium slag or arsenic iron slag, which dries the arsenic-containing waste slag and then oxidizes and roasts it at 600-1000°C for 1-3 hours. The As concentration in the leaching solution of the arsenic-containing waste slag treated by the invention method is far lower than the national limit (5 mg / L). However, the temperature for oxidation-reduction of this technology is too high, and the energy consumption is huge, which is not conducive to the realization of the "dual carbon" goal.
[0006] Patent CN106362347A discloses a method for treating high-concentration arsenic slag. The method uses magnesium-based stabilizers, iron-based stabilizers and silica powder as stabilizers, lime to adjust the pH, and cement as a curing agent. After treatment, the arsenic leaching toxicity is less than 2.5 mg / L. However, the method requires a pH of not less than 13, and is prone to secondary pollution under strong alkaline conditions. It cannot be safely landfilled, and the treatment cycle is relatively long.
[0007] Patent CN110746168A discloses a method for solidifying arsenic-containing sludge with steel slag and silica fume cementitious materials, which comprises mixing arsenic-containing sludge, steel slag and silica fume, using sodium silicate and sodium hydroxide as alkali activators, pressing and molding, and curing the solidified blocks for more than 28 days. The method has simple process operation and low production cost, but the material parameters are too large and the curing time is too long. Summary of the invention
[0008] The existing arsenic-containing waste slag stabilization treatment technology has problems such as long treatment cycle, large volume expansion ratio, high energy consumption and easy secondary pollution to the environment. The present invention provides a method for stabilizing calcium arsenic slag using copper tailings as a multifunctional stabilizer. The iron and silicate in the copper tailings are conducive to the stabilization of arsenic in the calcium arsenic slag, and the mineral phase of arsenic in the calcium arsenic slag is re-established through evaporation and crystallization. Compared with the traditional process, the method of the present invention has cheap and easy-to-obtain raw materials, simple operation, short treatment cycle, low energy consumption and no secondary pollution to the environment. After the calcium arsenic slag is stabilized, various indicators can meet the limit requirements specified in the "Hazardous Waste Landfill Pollution Control Standard" (GB18598-2019), and can be safely landfilled.
[0009] In order to achieve the above object, the present invention provides the following technical solutions:
[0010] A method for stabilizing calcium arsenic slag by using copper tailings comprises the following steps:
[0011] (1) treating arsenic-containing waste liquid by lime precipitation to obtain calcium arsenic slag, and drying the obtained calcium arsenic slag to constant weight;
[0012] (2) taking out the calcium arsenic slag after drying in step (1) and ball milling it;
[0013] (3) mixing the powder obtained in step (2) and the flotation copper tailings uniformly, and then adding an acid solution for mixing and stirring, wherein the liquid-to-solid ratio of the acid solution to the calcium arsenic slag in step (1) is 1-5 mL:1 g, and the iron-arsenic molar ratio of the mixture obtained by uniformly mixing the powder and the flotation copper tailings is 2-4:1;
[0014] (4) Evaporating the mixture obtained in step (3) until the acid solution is evaporated to dryness, thereby achieving stabilization treatment of the calcium arsenic slag.
[0015] Furthermore, in step (1), the specific process of treating the arsenic-containing waste liquid by the lime precipitation method is as follows: adding calcium carbonate to the arsenic-containing waste liquid for reaction, adjusting the pH, reacting for a period of time, filtering, and collecting solid calcium sulfate; adding calcium hydroxide to the filtrate for reaction, adjusting the pH, reacting for a period of time, filtering, and collecting calcium arsenic slag; the calcium carbonate is used to adjust the pH of the arsenic-containing waste liquid to 2-3, preferably 2-2.5, and the reaction time is 0.1-24h, preferably 1-10h; the calcium hydroxide is used to adjust the pH of the filtrate to 11-13, preferably 12-13, and the reaction time is 1-15h, preferably 1-8h; the arsenic-containing waste liquid is arsenic-containing waste liquid generated in the process of non-ferrous metal smelting; the drying treatment conditions are: the oven temperature is 60-120°C, and the heating time is 4-8h; preferably, the heating temperature is 60-80°C, and the heating time is 6-8h.
[0016] Furthermore, the ball milling conditions in step (2) are: ball milling speed of 150-250 rpm, ball milling time of 2-4 h, and ball to material ratio of 1-3:1; preferably, the ball milling speed is 200-250 rpm, the ball milling time is 2-3 h, and the ball to material ratio is 1-2:1; in the calcium arsenic slag obtained by ball milling, the particle size D90≤0.165 mm, the particle size D80≤0.165 mm, and the particle size D10<0.074 mm.
[0017] Furthermore, in step (3), the acid solution is sulfuric acid, and the concentration of the acid solution is 0.5-3.5 mol / L; preferably, the concentration of the acid solution is 0.5-2 mol / L; the liquid-solid ratio of the acid solution to the calcium arsenic slag is 2-4 mL:1 g; preferably, the molar ratio of iron to arsenic is 2-3.5:1.
[0018] Furthermore, in step (4), the evaporation temperature is 60-100° C.; preferably, the evaporation temperature is 90-100° C.; the evaporation time is 0.5 h to 2.5 h; preferably, the evaporation time is 1 h to 1.5 h.
[0019] The principle of stabilizing arsenic in calcium arsenic slag of the present invention is:
[0020] The invention utilizes sulfuric acid to dissolve and release iron and silicon in the flotation tailings of a copper smelter. During the mixing, stirring and heating process, As(III) in the calcium arsenic slag and ferrous ions released by dissolving the flotation copper tailings of the copper smelter are oxidized into As(V) and Fe(III) by oxygen in the air, and iron-arsenic-containing minerals are further generated to stabilize arsenic. Finally, a mixture including CaSO4·2H2O, Fe(H2AsO4)3 and Ca2SiO4 is obtained, and its stability is enhanced, and the leaching toxicity of arsenic is further reduced.
[0021] Compared with the prior art, the present invention has the advantages of:
[0022] (1) The present invention uses the tailings after flotation of a copper smelter as raw material to treat hazardous solid waste. No auxiliary materials need to be added, and the synergistic treatment of copper tailings and calcium arsenic slag is achieved. Compared with other solidification technologies, the present method has a small volume increase ratio, reduces the accumulation of solid waste, and achieves the purpose of protecting the environment.
[0023] (2) The process flow of the present invention is simple and low-cost. It adopts a low-temperature heating method to effectively reduce energy consumption. The treatment cycle is short, and the arsenic pollution leakage problem caused by the accumulation of calcium arsenic slag can be effectively solved.
[0024] (3) The method adopted by the present invention is to reconstruct the arsenate substances in the calcium arsenic slag and the flotation copper tailings in the low-temperature mineral phase in an acidic environment to form iron-arsenic mineral crystal nuclei. At the same time, silicates, as associated minerals, are combined with the newly generated iron-arsenic minerals, thereby enhancing their stability and limiting their diffusion. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The basic flow chart of the calcium arsenic slag stabilization method of the present invention;
[0026] Figure 2 This is the XRD spectrum of the raw material calcium arsenic slag of Example 1 of the present invention;
[0027] Figure 3 This is the XRD spectrum of the calcium arsenic slag after treatment in Example 1 of the present invention;
[0028] Figure 4 This is the infrared spectrum of the raw material calcium arsenic slag of Example 1 of the present invention;
[0029] Figure 5 This is the infrared spectrum of the calcium arsenic slag after treatment in Example 1 of the present invention. DETAILED DESCRIPTION
[0030] The applicant will now further describe the present invention in detail with reference to the accompanying drawings and specific embodiments. The embodiments are only used to help understand the present invention, but the protection scope requested by the claims of the present invention is not limited thereto.
[0031] The flotation copper tailings used in Examples 1-3 were provided by Hubei Zhonghua Dajiang Environmental Protection Technology Co., Ltd. The total iron in the flotation copper tailings was 327.21 g / kg, and the main chemical components and contents were shown in Table 1; the calcium arsenic slag was obtained by treating arsenic-containing waste liquid with a lime precipitation method, and the main chemical components and contents were shown in Table 2; the specific process of treating arsenic-containing waste liquid with the lime precipitation method was as follows: adding calcium carbonate to the arsenic-containing waste liquid for reaction, adjusting the pH to 2, and filtering after reacting for 6 hours to collect solid calcium sulfate; adding calcium hydroxide to the filtrate for reaction, adjusting the pH to 12, and filtering after reacting for 5 hours to collect the calcium arsenic slag; the arsenic-containing waste liquid was arsenic-containing waste liquid generated in the non-ferrous metal smelting process.
[0032] Table 1 Main components and contents of flotation copper tailings (wt%)
[0033]
[0034] Table 2 Main components and contents of calcium arsenic slag (wt%)
[0035]
[0036] Example 1
[0037] A method for stabilizing calcium arsenic slag using copper tailings, the specific steps are as follows:
[0038] (1) Place 5 g of calcium arsenic slag in an electric heated air drying oven and dry at 80°C for 6 h until constant weight is reached;
[0039] (2) The calcium arsenic slag after drying in step (1) is taken out and ball milled at a ball milling speed of 200 rpm, a ball milling time of 3 h, and a ball-to-material ratio of 2:1.
[0040] (3) mixing the calcium arsenic slag powder obtained in step (2) and the flotation copper tailings in a total iron-arsenic molar ratio of 2.5:1, adding 15 mL of a 1.5 mol / L sulfuric acid solution, and stirring to obtain a mixture;
[0041] (4) The mixture obtained in step (3) was placed in a constant temperature heated magnetic stirrer, heated and stirred at 100° C. for 1 h, the solution was evaporated to dryness, and the leaching toxicity test and BCR continuous extraction method were performed to analyze the heavy metal form. The test results are shown in Tables 3 and 4.
[0042] Example 2
[0043] A method for stabilizing calcium arsenic slag using copper tailings, the specific steps are as follows:
[0044] (1) Place 5 g of calcium arsenic slag in an electric heated air drying oven and dry at 60°C for 8 h until constant weight is reached;
[0045] (2) The calcium arsenic slag after drying in step (1) is taken out and ball milled at a ball milling speed of 250 rpm, a ball milling time of 2 h, and a ball-to-material ratio of 2:1.
[0046] (3) mixing the calcium arsenic slag powder obtained in step (2) and the flotation copper tailings in a total iron-arsenic molar ratio of 2:1, adding 15 mL of a 1.5 mol / L sulfuric acid solution, and stirring to obtain a mixture;
[0047] (4) The mixture obtained in step (3) was placed in a constant temperature heated magnetic stirrer, heated and stirred at 100° C. for 1 h, the solution was evaporated to dryness, and the leaching toxicity test and BCR continuous extraction method were performed to analyze the heavy metal forms. The test results are shown in Tables 3 and 4.
[0048] Example 3
[0049] A method for stabilizing calcium arsenic slag using copper tailings, the specific steps are as follows:
[0050] (1) Place 5 g of calcium arsenic slag in an electric heated air drying oven and dry at 70°C for 7 h until constant weight is reached;
[0051] (2) The calcium arsenic slag after drying in step (1) is taken out and ball milled at a ball milling speed of 250 rpm, a ball milling time of 2 h, and a ball-to-material ratio of 2:1.
[0052] (3) mixing the calcium arsenic slag powder obtained in step (2) and the flotation copper tailings in a total iron-arsenic molar ratio of 2:1, adding 20 mL of 1.5 mol / L sulfuric acid solution, and stirring to obtain a mixture;
[0053] (4) The mixture obtained in step (3) was placed in a constant temperature heated magnetic stirrer, heated and stirred at 100° C. for 1 h, the solution was evaporated to dryness, and the leaching toxicity test and BCR continuous extraction method were performed to analyze the heavy metal forms. The test results are shown in Tables 3 and 4.
[0054] Table 3 Leaching toxicity test of Examples 1 to 3
[0055]
[0056] The obtained iron-arsenic mineral was subjected to leaching toxicity evaluation (HJ / T 299-2007). The arsenic leaching concentration was far less than the 5 mg / L limit specified in the leaching toxicity evaluation. The generated iron-arsenic mineral had good phase stability and could meet the control limit for landfill allowed by the "Hazardous Waste Landfill Pollution Control Standard" (GB 18598-2019).
[0057] Table 4 Analysis of heavy metal forms by BCR continuous extraction method
[0058]
[0059] The BCR continuous extraction method was used to analyze the arsenic occurrence forms in the calcium arsenic slag, and the mobility of arsenic in the calcium arsenic slag before and after treatment and the potential risks to the environment were evaluated. The occurrence forms of heavy metal arsenic are divided into acid soluble state, reducible state, oxidizable state, and residual state. The weak acid extraction state can be directly dissolved in an acidic / neutral water environment and is the most harmful; the reducible state corresponds to the form of arsenic and metal oxides, and the oxidizable state refers to the form of organic arsenic. The reducible and oxidizable states will also dissolve in appropriate pH and redox environments; the residual state is arsenic in a stable mineral form, which is the most stable and not easy to dissolve.
[0060] The results show that the low-temperature mineral phase reconstruction method adopted in the present invention converts the unstable arsenic forms (including acid-soluble, reducible, and oxidizable states) in the original calcium arsenic slag into a stable residual form, thereby achieving the stabilization of the calcium arsenic slag.
Claims
1. A method for stabilizing calcium arsenic slag using copper tailings, comprising the following steps: (1) treating arsenic-containing waste liquid by lime precipitation to obtain calcium arsenic slag, and drying the obtained calcium arsenic slag to constant weight; (2) taking out the calcium arsenic slag after drying in step (1) and ball milling it; (3) The powder obtained in step (2) is mixed evenly with the flotation copper tailings, and then an acid solution is added and mixed and stirred, wherein: The liquid-to-solid ratio of the acid solution to the calcium arsenic slag of step (1) is 1-5 mL: 1 g, and the iron-arsenic molar ratio of the obtained mixture obtained by uniformly mixing the powder with the copper tailings after flotation is 2-4:1; (4) Evaporating the mixture obtained in step (3) until the acid solution is evaporated to dryness, thereby achieving the stabilization treatment of the calcium arsenic slag.
2. The method according to claim 1, characterized in that In step (1), the specific process of treating arsenic-containing waste liquid by lime precipitation method is as follows: adding calcium carbonate to the arsenic-containing waste liquid for reaction, adjusting the pH, reacting for a period of time, filtering, and collecting solid calcium sulfate; adding calcium hydroxide to the filtrate for reaction, adjusting the pH, reacting for a period of time, filtering, and collecting calcium arsenic slag; the calcium carbonate is used to adjust the pH value of the arsenic-containing waste liquid to 2-3, preferably 2-2.5, and the reaction time is 0.1-24 h, preferably 1-10 h; the calcium hydroxide is used to adjust the pH value of the filtrate to 11-13, preferably 12-13, and the reaction time is 1-15 h, preferably 1-8 h; the arsenic-containing waste liquid is arsenic-containing waste liquid generated in the process of non-ferrous metal smelting; the drying treatment conditions are: the oven temperature is 60-120 ° C, and the heating time is 4-8 h; preferably, the heating temperature is 60-80 ° C, and the heating time is 6-8 h.
3. The method according to claim 1, characterized in that The ball milling conditions in step (2) are: ball milling speed of 150-250 rpm, ball milling time of 2-4 h, and ball to material ratio of 1-3:1; preferably, the ball milling speed is 200-250 rpm, the ball milling time is 2-3 h, and the ball to material ratio is 1-2:1; in the calcium arsenic slag obtained by ball milling, the particle size D90 is ≤0.165 mm, the particle size D80 is 0.074 mm ≤0.165 mm, and the particle size D10 is <0.074 mm.
4. The method according to claim 1, characterized in that: In step (3), the acid solution is sulfuric acid, and the concentration of the acid solution is 0.5-3.5 mol / L; preferably, the concentration of the acid solution is 0.5-2 mol / L; the liquid-solid ratio of the acid solution to the calcium arsenic slag is 2-4 mL:1 g; preferably, the molar ratio of iron to arsenic is 2-3.5:
1.
5. The method according to claim 1, characterized in that In step (4), the evaporation temperature is 60-100°C; preferably, the evaporation temperature is 90-100°C; the evaporation time is 0.5 h-2.5 h; preferably, the evaporation time is 1 h-1.5 h.
Citation Information
Patent Citations
Method for treating arsenic-containing wastewater with high acidity from zinc smelting
CN102730880A
Stabilizing treatment method for sulfide arsenic-removed dregs
CN105499250A
Method for curing arsenic-containing waste residues through industrial waste residues
CN105537247A
Method of sulfur removal and arsenic and mercury removal with copper smeltery tailing slurry
CN106731629A
Method for preparing high-stability solid arsenic minerals by hydrothermal process
CN106823234A