Heat-assisted chemical bath rotary film forming equipment and preparation method of perovskite thin film
Through the use of thermally assisted chemical bath rotary film forming equipment, the problems of low material utilization and poor film formation quality in perovskite film preparation are solved, efficient large-area preparation and photoelectric conversion efficiency are improved, and pertitanium is promoted Industrialization of mine solar cells.
Patent Information
- Application Number
- CN202411044963.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
The existing perovskite film preparation methods have problems such as low material utilization, poor film formation quality, high equipment requirements and low battery efficiency, making it difficult to achieve efficient large-area preparation.
Thermal assisted chemical bath rotary film formation equipment is adopted, including heating devices, rotatable top surfaces and liquid supply systems, to promote film nucleation and growth through rotation and heating, improve material utilization and film formation quality, and reduce grain boundaries.
It has achieved efficient preparation of large-area and high-quality perovskite films, improved the photoelectric conversion efficiency, and promoted the industrial production of perovskite solar cells.
Smart Images

Figure BDA0004974664730000081 
Figure BDA0004974664730000091 
Figure HDA0004974664860000011
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar cells, and in particular to a device for heat-assisted chemical bath rotational film formation and a method for preparing a perovskite film. Background Art
[0002] In recent years, perovskite photovoltaic cells have developed rapidly and have received extensive attention from scientific research and industry. Their photoelectric conversion efficiency has been rapidly improved. The current single-junction cell efficiency is 26.1%, and the perovskite / crystalline silicon stacked cell efficiency is 34.6%. In addition, the preparation steps of perovskite cells are few and the process is easy to achieve large-scale production. At the same time, perovskite solar cells have a wide range of application scenarios, including: centralized power stations, distributed power stations, photovoltaic building integration (BIPV), flexible photovoltaics, wearable electronic devices, Internet of Things devices (IoT), etc.
[0003] At present, perovskite photovoltaic technology is at a critical moment of industrialization, and the premise of industrialization is the development of large-scale preparation technology of perovskite thin films. The key to preparing large-area perovskite cells lies in the preparation of high-quality perovskite films.
[0004] At present, the methods used to prepare perovskite films mainly include spin coating, vapor-assisted deposition, spray pyrolysis, blade coating, slot extrusion coating, inkjet printing, roller printing, soft cover deposition and vacuum flash solution treatment. Among them, the preparation methods of spin coating and vacuum flash evaporation result in low material utilization, blade coating results in average film quality of perovskite films, slot extrusion coating has relatively high requirements for equipment, and inkjet printing has low battery efficiency.
[0005] Therefore, it is of great significance to study and develop a new device for preparing perovskite films to solve the practical difficulties of the above-mentioned methods for preparing perovskite films. Summary of the invention
[0006] In view of this, the technical problem to be solved by the present invention is to provide a device for heat-assisted chemical bath rotary film forming and a method for preparing a perovskite film. The device for heat-assisted chemical bath rotary film forming can realize large-area preparation of a perovskite film, and the prepared perovskite film has a high photoelectric conversion efficiency.
[0007] In order to achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0008] The present invention provides a thermally assisted chemical bath rotary film forming device, comprising a film forming system and a liquid supply system;
[0009] The film forming system includes a heating device;
[0010] A rotatable top surface is arranged above the heating device, the rotatable top surface is used to place the substrate and can rotate in a vertical direction;
[0011] The rotatable top surface is provided with a groove for reflux of unreacted raw material liquid;
[0012] A device connected to the rotatable top surface device for providing vacuum adsorption to fix the substrate;
[0013] The liquid outlet of the liquid supply system is arranged above the rotatable top surface.
[0014] The liquid outlet of the liquid supply system includes but is not limited to a liquid adding arm and the like.
[0015] The present invention controls the film preparation process by adjusting the temperature of the heating device, and the optimized temperature regulation helps to accelerate the nucleation and growth of crystals in the film, thereby obtaining a high-quality film.
[0016] The heating device includes but is not limited to a heating wire, an infrared lamp, a laser, a semiconductor heater, a silicone heating plate, etc. In some specific embodiments of the present invention, a heating wire is preferred.
[0017] The temperature of the heating wire is preferably between room temperature and 150°C;
[0018] The room temperature is preferably 10°C to 30°C.
[0019] The device for providing vacuum adsorption to fix the substrate comprises a vacuum adsorption component and an air supply component.
[0020] The main function of the vacuum adsorption component is to fix the substrate to prevent it from moving during the film preparation process, thereby affecting the film quality.
[0021] The main function of the gas supply component is to quickly ventilate and release the vacuum adsorption state of the substrate after the film preparation is completed, so as to facilitate the robot to quickly remove the substrate and proceed to the next step.
[0022] The vacuum adsorption component includes but is not limited to a vacuum pump, and the air supply component includes but is not limited to a COA compressed air device.
[0023] Preferably, the liquid supply system of the present invention further comprises a raw material mixing device;
[0024] Preferably, the inlet of the raw material mixing device is connected to the inlet tube of the film precursor source, and the outlet is connected to the liquid outlet of the liquid supply system.
[0025] The raw material mixing device mixes various reaction raw material liquids of the film precursor to obtain a uniform and stable film precursor solution (also called mixed reaction raw material liquid).
[0026] In some specific embodiments of the present invention, the raw material mixing device includes but is not limited to a mixed liquid chamber.
[0027] Preferably, the rotation of the rotatable top surface is 10° to 90° clockwise and counterclockwise respectively, and the rotation angle is the same; more preferably 30° to 60°. In some specific embodiments of the present invention, the rotation is specifically 30° clockwise and counterclockwise respectively, or 45° clockwise and counterclockwise respectively, or 60° clockwise and counterclockwise respectively.
[0028] When rotating, the left and right rotation angles are kept consistent to ensure the uniformity of the film.
[0029] Preferably, in the present invention, the film forming system further comprises a shaking device connected to the heating device.
[0030] The functions of the shaking device include: 1) obtaining a large-area thin film layer with uniform thickness through rotation and shaking; 2) spinning out the excess thin film precursor solution (also known as mixed reaction raw material solution) and returning it to the recovery device through the grooves around the substrate table to avoid contamination of the film and further improve the utilization rate of the raw materials.
[0031] The shaking device includes but is not limited to a rocker arm, a turntable, etc.
[0032] Preferably, the groove is connected to a pipeline device;
[0033] Preferably, the pipeline device is connected to a recovery device for recovering unreacted raw material liquid. The above device can quickly place or remove the substrate by a manipulator, thereby improving the efficiency of film preparation.
[0034] The thermally assisted chemical bath rotary film forming device of the present invention is helpful to efficiently prepare large-area, high-quality films.
[0035] The present invention also provides a method for preparing a perovskite film, which uses the above-mentioned thermally assisted chemical bath rotary film forming device to prepare the perovskite film;
[0036] The preparation method is specifically:
[0037] The perovskite film substrate is rotated and heated in a solution of a perovskite film precursor source, and then annealed to obtain a perovskite film.
[0038] The device and preparation method of the present invention can realize the preparation of large-area perovskite thin films, thereby promoting the large-scale production of perovskite solar cells.
[0039] Preferably, the composition of the perovskite film is ABX 3, wherein A is selected from one or more of Cs, Rb, MA, FA, and PEA, B is selected from Pb or Sn, and X is selected from one or more of Cl, Br, and I.
[0040] The heating device under the rotatable plane device in the film forming system of the above-mentioned heat-assisted chemical bath rotary film forming equipment is beneficial to the nucleation and growth of perovskite film crystals, can reduce grain boundaries, and improve the photoelectric conversion efficiency of the perovskite film.
[0041] More preferably, the composition of the perovskite film is MA x FA 1-x PbI x Cl 3-x (0<x≤1). In some specific embodiments of the present invention, the composition of the perovskite film is preferably MA 0.1 FA 0.9 PbI 2.95 Cl 0.05 .
[0042] Preferably, the rotation is 10° to 90° clockwise and counterclockwise respectively, and the rotation angles are the same; more preferably, the rotation is 30° to 60° clockwise and counterclockwise respectively, and the rotation angles are the same. More preferably, the rotation is 30° clockwise and counterclockwise respectively, or 45° clockwise and counterclockwise respectively, or 60° clockwise and counterclockwise respectively.
[0043] When the rotation angle is 30°, 45° or 60°, it is beneficial for the excess precursor solution to flow back, thereby improving the utilization rate of the material.
[0044] The heating device in the described setup promotes high-quality film formation of perovskite thin films.
[0045] In the present invention, the heating temperature is preferably 40°C to 90°C; more preferably 60°C to 90°C; further preferably 70°C or 80°C.
[0046] Preferably, the annealing temperature is 40°C to 90°C; more preferably 70°C to 90°C.
[0047] Preferably, the annealing time is 10 to 30 minutes, more preferably 15 to 25 minutes, and further preferably 20 minutes.
[0048] Preferably, the perovskite thin film substrate is selected from glass whose surface is covered with an ITO or FTO conductive layer.
[0049] The present invention also provides a perovskite film, which is prepared by the above-mentioned preparation method;
[0050] The perovskite film is prepared by the equipment and preparation method of the present invention.
[0051] Preferably, the effective area of the perovskite film is not less than 30*30cm 2 Preferably, the thickness of the perovskite film is 300-600 nm.
[0052] The present invention also provides a perovskite battery, comprising the above-mentioned perovskite film.
[0053] Preferably, the perovskite cell is composed of ITO / FTO conductive glass (1), a hole transport layer (2), a perovskite absorption layer (3), an electron transport layer (4) and an electrode layer (5), and the perovskite absorption layer is the above-mentioned perovskite film.
[0054] The preparation method of the perovskite battery comprises the following steps:
[0055] 1) A hole transport layer is prepared on the surface of ITO / FTO conductive glass by spray pyrolysis;
[0056] 2) preparing a perovskite film on the surface of the hole transport layer prepared above by using a heat-assisted chemical bath spin film forming method;
[0057] 3) Preparing an electron transport layer and a silver electrode layer on the surface of the perovskite film described in step 2) by vacuum evaporation to obtain a perovskite cell.
[0058] In some specific embodiments of the present invention, the area of the ITO or FTO conductive layer in step 1) is 65×50 cm 2 .
[0059] The hole transport layer in step 1) is selected from NiO hole transport layer.
[0060] The thickness of the NiO hole transport layer is preferably 15 to 30 nm.
[0061] The method of spray pyrolysis in step 1) is specifically as follows:
[0062] NiNO 3 The precursor solution is sprayed and sintered to obtain a NiO hole transport layer.
[0063] The NiNO 3 The concentration of the precursor solution is preferably 0.05 to 0.5 mol.L -1 , more preferably 0.08 to 0.2 mol.L -1 .
[0064] The number of the spraying cycles is 16 to 27 cycles.
[0065] The sintering temperature is preferably 350°C to 450°C.
[0066] The sintering time is preferably 10 to 90 minutes, more preferably 20 to 60 minutes.
[0067] The composition of the perovskite film in step 2) is ABX 3 , wherein A is selected from one or more of MA (methylamino), FA (formamidinium), PEA (phenylethylamino), B is selected from Pb or Sn, and X is selected from one or more of Cl, Br, and I.
[0068] Preferably, the composition of the perovskite film is MA x FA 1-x PbI x Cl 3-x (0<x≤1).
[0069] The thickness of the electron transport layer in step 3) is preferably 100 to 300 nm.
[0070] PC is preferred 71 BM material ([6,6]-phenyl C 71 Methyl butyrate).
[0071] The PC 71 The thickness of the BM material is preferably 150 nm.
[0072] The preparation of the electron transport layer is as follows: 71 The slurry of BM material is coated on the surface of the perovskite film.
[0073] The slurry is PC 71 The chloroform dispersion of BM material has a concentration of 15 g / L.
[0074] The coating method is preferably blade coating.
[0075] The speed of the scraping is preferably 10 to 20 mm / s, more preferably 15 mm / s.
[0076] The temperature of the scraping is room temperature, and the room temperature is preferably 10°C to 30°C.
[0077] The distance between the scraper used for scraping and the substrate (perovskite film) is 10 to 500 μm.
[0078] After the above-mentioned scraping is completed, it is naturally dried in an inert gas.
[0079] The inert gas includes, but is not limited to, nitrogen.
[0080] The natural drying time is preferably 5 to 40 minutes.
[0081] Then, a metal electrode layer is prepared on the surface of the electron transport layer.
[0082] In some specific embodiments of the present invention, the metal electrode layer is selected from Ag metal electrode layer.
[0083] The thickness of the Ag metal electrode layer is preferably 50 to 80 nm.
[0084] The preparation method is preferably evaporation.
[0085] Compared with the prior art, the device for heat-assisted chemical bath rotary film formation provided by the present invention includes a film forming system and a liquid supply system; the film forming system includes a heating device; a rotatable top surface arranged above the heating device, the rotatable top surface is used to place the substrate and can rotate in the vertical direction; the rotatable top surface is provided with a groove for reflux of unreacted raw material liquid; a device connected to the rotatable top surface device for providing vacuum adsorption to fix the substrate; the liquid outlet of the liquid supply system is arranged above the rotatable top surface. The use of the device can improve the nucleation and growth of perovskite thin film crystals, reduce grain boundaries, further improve the photoelectric conversion efficiency, and can realize large-area preparation of perovskite thin films. BRIEF DESCRIPTION OF THE DRAWINGS
[0086] Figure 1 This is a schematic diagram of the structure of a perovskite solar cell prepared in Example 1;
[0087] Figure 2 Schematic diagram of the preparation of perovskite film using the thermally assisted chemical bath spin film forming equipment in Example 1. DETAILED DESCRIPTION
[0088] In order to further illustrate the present invention, the thermally assisted chemical bath rotary film forming equipment and the preparation method of the perovskite film and perovskite battery provided by the present invention are described in detail in combination with the embodiments.
[0089] The following examples use the thermally assisted chemical bath rotary film forming equipment of the present invention to prepare perovskite thin films.
[0090] The thermally assisted chemical bath rotary film forming device of the present invention is as follows Figure 2 As shown, it includes a film forming system and a liquid supply system;
[0091] Wherein, the film forming system comprises a heating device. In some specific embodiments of the present invention, the heating device is preferably a heating wire.
[0092] The temperature of the heating wire is preferably 60°C to 90°C.
[0093] The film forming system further comprises a rotatable top surface arranged above the heating device, the rotatable top surface is used to place the substrate and can be rotated in a vertical direction. The rotation of the rotatable top surface is 10° to 90° clockwise and counterclockwise respectively, and the rotation angles are the same.
[0094] The film forming system also includes a groove arranged on the rotatable top surface for reflux of unreacted raw material liquid, thereby allowing the unreacted raw material liquid to be recycled.
[0095] The groove is connected to a pipeline device, and the pipeline device is connected to a recovery device for recovering unreacted raw material liquid.
[0096] The film forming system also includes a device connected to the rotatable top surface device for providing vacuum adsorption to fix the substrate;
[0097] The device for providing vacuum adsorption to fix the substrate comprises a vacuum adsorption component and an air supply component.
[0098] In some specific embodiments of the present invention, the vacuum adsorption component is preferably a vacuum pump (also called a mechanical pump), and the air supply component is preferably a COA compressed air device.
[0099] The liquid outlet of the liquid supply system is arranged above the rotatable top surface. Figure 2 As shown, the liquid outlet is preferably a liquid adding arm, which adds the thin film precursor solution (also called mixed reaction raw material liquid) in the liquid supply system to the rotatable top surface above the heating device in the film forming system, and then heats the rotatable top surface through the heating device to react and prepare the perovskite film.
[0100] The liquid supply system also includes a raw material mixing device;
[0101] The inlet of the raw material mixing device is connected to the sample inlet tube of the film precursor source, and the outlet is connected to the liquid outlet of the liquid supply system.
[0102] like Figure 2 As shown, in some specific embodiments of the present invention, the raw material mixing device is preferably a mixed liquid chamber, which mixes the reaction raw material liquids of the perovskite film to obtain a uniform and stable film precursor solution (also called mixed reaction raw material liquid).
[0103] In some specific embodiments of the present invention, the rotation is specifically 30° clockwise and 30° counterclockwise, or 45° clockwise and 45° counterclockwise, or 60° clockwise and 60° counterclockwise.
[0104] The film forming system also includes a shaking device connected to the heating device. Figure 2 As shown, in some specific embodiments of the present invention, the rocking device is preferably a rocker arm.
[0105] Examples 1 to 7
[0106] The ITO-coated transparent conductive glass was ultrasonically treated with deionized water, acetone, and isopropanol for 15 minutes, then cleaned with a UV cleaner for 10 minutes and dried with nitrogen gas. -1 NiNO 3 The precursor solution was sprayed 18 times and sintered at 375°C for 30 min to obtain a NiO hole transport layer with a thickness of 20 nm.
[0107] The substrate covered with the hole transport layer is transferred to the CBD chemical bath reaction chamber, and the temperature of the substrate is controlled at 60℃~90℃. The specific process is as follows: after the robot grabs the glass substrate, it is loaded into the machine and placed on the heating plate. The glass substrate is fixed by vacuum adsorption, and the chemical reaction raw materials - lead iodide, methylamine chloride, methylamine iodide, and formamidine iodide are added, and the mixed liquid cavity is stirred through the injection tube. After sufficient mixing, the gate valve is opened and 10~50mL of the stirred MA is added. 0.1 FA 0.9 PbI 2.95 Cl 0.05 The precursor solution flows into the chemical liquid adding arm, and then flows into the glass substrate of the reaction chamber. After standing for 1 to 3 minutes, the substrate is driven by the rocker arm to rotate 30°, 45° or 60° to the left (counterclockwise) or right (clockwise), and in one embodiment, the counterclockwise and clockwise rotation angles are the same. The excess precursor solution flows back to the waste liquid barrel through the groove, and is annealed at 70°C to 90°C for 10 minutes. The thickness of the obtained perovskite active layer (also called perovskite film) is about 300 to 600nm, and the effective area is 65×50cm 2 .
[0108] The schematic diagram of the thermally assisted chemical bath spin film forming device for preparing perovskite thin films is shown in FIG. Figure 2 shown.
[0109] Then, a 150 nm thick PC was prepared by scraping at a speed of 15 mm / s on the perovskite active layer. 71 BM electron transport layer.
[0110] Finally, a 60nm layer of Ag was evaporated on the electron transport layer to form a metal electrode layer, and 7 types of perovskite solar cells were obtained and the conversion efficiency was tested. The test method refers to the China Photovoltaic Industry Association group standard "Current-voltage (IV) Characteristics Measurement Method of Perovskite Solar Cells and Modules" (Standard No.: T / CPIA0032-2022).
[0111] The schematic diagram of the structure of the perovskite solar cell is as follows Figure 1 As shown, the perovskite solar cell comprises, from bottom to top, ITO / FTO conductive glass (1), hole transport layer (2), perovskite absorption layer (3), electron transport layer (4) and electrode layer (5). The perovskite absorption layer (3) is the perovskite film described in the present invention.
[0112] The test results of the conversion efficiency of the perovskite solar cell are shown in Table 1.
[0113] Table 1 Effect of process parameters of different perovskite absorber layers (thin films) on solar cell performance
[0114]
[0115]
[0116] In summary, the thermally assisted chemical bath rotary film forming device of the present invention can realize the preparation of large-area perovskite films, and improve the conversion efficiency of large-area perovskite films with a basic structure without a modified layer.
[0117] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A thermally assisted chemical bath rotary film forming device, characterized in that: Including film forming system and liquid supply system; The film forming system includes a heating device; A rotatable top surface is arranged above the heating device, the rotatable top surface is used to place the substrate and can rotate in a vertical direction; The rotatable top surface is provided with a groove for reflux of unreacted raw material liquid; A device connected to the rotatable top surface device for providing vacuum adsorption to fix the substrate; The liquid outlet of the liquid supply system is arranged above the rotatable top surface.
2. The thermally assisted chemical bath rotary film forming device according to claim 1, characterized in that: The liquid supply system also includes a raw material mixing device; The inlet of the raw material mixing device is connected to the sample inlet tube of the film precursor source, and the outlet is connected to the liquid outlet of the liquid supply system.
3. The thermally assisted chemical bath rotary film forming device according to claim 1, characterized in that: The rotation of the rotatable top surface is 10° to 90° clockwise and counterclockwise respectively, and the rotation angles are the same.
4. The thermally assisted chemical bath rotary film forming device according to claim 1, characterized in that: The film forming system also includes a shaking device connected to the heating device; The groove is connected to the pipeline device; The pipeline device is connected to a recovery device for recovering unreacted raw material liquid.
5. A method for preparing a perovskite film, characterized in that: The perovskite film is prepared by using the thermally assisted chemical bath rotary film forming device as described in any one of claims 1 to 4; The preparation method is specifically: The perovskite film substrate is rotated and heated in a solution of a perovskite film precursor source, and then annealed to obtain a perovskite film.
6. The preparation method according to claim 5, characterized in that: The composition of the perovskite film is ABX3, wherein A is selected from one or more of Cs, Rb, MA, FA, and PEA, B is selected from Pb or Sn, and X is selected from one or more of Cl, Br, and I.
7. The preparation method according to claim 6, characterized in that: The composition of the perovskite film is MA x FA 1- x PbI x Cl 3-x (0<x≤1).
8. The preparation method according to claim 5, characterized in that: The rotation is 10° to 90° clockwise and counterclockwise respectively, and the rotation angles are the same; The heating temperature is 40°C to 90°C; The annealing temperature is 40°C to 90°C; The annealing time is 10 to 30 minutes.
9. A perovskite film, characterized in that: Prepared by the preparation method according to any one of claims 5 to 8; The effective area of the perovskite film is not less than 30*30cm 2 ; The thickness of the perovskite film is 300-600nm.
10. A perovskite battery, characterized in that: Comprising the perovskite film as described in claim 9.