Multifunctional special-shaped composite chinlon 6 fully-drawn yarn fiber and preparation method thereof
By using the combination of alkali-soluble polyester masterbatch and nylon 6 slices in nylon 6 fibers, and using the "king-shaped" spinneret holes and drafting components, a multifunctional special-shaped composite nylon 6 fully drafted silk fiber is formed, solving the problem of The existing fiber performance is problematic, and efficient moisture-wicking, anti-UV and thermal conductivity are achieved, and are suitable for multifunctional composite textile and clothing.
Patent Information
- Application Number
- CN202411123652.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-15
AI Technical Summary
The existing nylon 6 fiber lacks multifunctional composite performance in outdoor clothing and casual clothing, and cannot achieve sun protection, coolness, and breathable and dry effects at the same time. It has a single performance and cannot meet the diverse needs of consumers.
Using a combination of alkali-soluble polyester masterbatch and nylon 6 slices, the design of the special spinning process includes melt extrusion under the spinning hole with the shape of the spinning hole "king-shaped" and in the pre-networker and The drawing assembly is stretched and high-temperature shaped to form a multi-functional special-shaped composite nylon 6 fully drafted wire fiber, which enhances the moisture absorption and sweating, anti-ultraviolet and thermal conductivity of the fiber.
It improves the moisture-wicking, UV resistance and thermal conductivity of the fiber, increases the surface area of the fiber, enhances breathability and coolness, reduces wear, and improves the overall performance of the fiber. It is suitable for multi-functional composite textile and clothing.
Smart Images

Figure CN118979310A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical fibers, and particularly relates to a multifunctional special-shaped composite nylon 6 fully drawn yarn fiber and a preparation method thereof. Background Art
[0002] With the rapid development of the textile industry and the increasing diversification of consumer demand, the requirements for the functionality and morphology of fiber materials are becoming higher and higher. Nylon fiber is a synthetic fiber, and its unique characteristics make it have a wide range of application prospects in outdoor clothing and casual clothing. Especially in outdoor sports activities, people need to protect their skin from sun damage while maintaining comfort, so the demand for multifunctional composite textile clothing products that combine sun protection, cool comfort, and breathability and dryness continues to grow. Therefore, the development of a multifunctional nylon 6 fiber has become a question for researchers in the industry.
[0003] The Chinese patent application number CN201510200793.6 discloses a method for producing nylon 6 shaped fibers, using nylon 6 slices as raw materials, and the production method comprises the following steps: (1) drying and screw extruding nylon 6 slices; (2) the melt enters the spinning assembly through a metering pump, is filtered through different coarse and fine filter sand ratios, and finally is extruded through the spinneret holes on the spinneret; wherein the spinneret hole cross-section is cross-shaped, and the length of the "vertical" in the cross-shaped cross is equal to half of the length of the "horizontal"; (3) the filaments extruded from the spinneret holes are bundled and oiled after cooling by annular air blowing; (4) the oiled filaments are shaped by hot rollers and wound into shape after a network nozzle. The nylon 6 shaped fibers produced by the method provided by the invention have a cross-shaped cross-section, and the outer contour of the fiber has four obvious grooves. The enhanced capillary effect enables the fiber to quickly absorb moisture and sweat from the skin surface, so it has a strong moisture conduction and sweat removal ability, but its performance is single, and other performances are not covered too much. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a multifunctional special-shaped composite nylon 6 fully drawn silk fiber and a preparation method thereof, which cleverly combines multiple functional components and special-shaped cross-section design, while retaining the original excellent properties of nylon 6 fiber, it also gives it the development and professional application of multiple composite functional properties, realizing the integration of multiple technologies. The high-performance fiber produced in this way has the characteristics of low cost and high added value, which can improve the market competitiveness of the product.
[0005] The technical solution of the present invention is as follows:
[0006] One of the purposes of the present invention is to provide a method for preparing a multifunctional special-shaped composite nylon 6 fully drawn filament fiber, comprising the following steps:
[0007] S1: Alkali-soluble polyester masterbatch and nylon 6 chips are mixed in a uniform proportion by a batching machine and fed into a screw extruder for melting, mixing, metering and extrusion of the melt under high temperature conditions;
[0008] S2: The extruded melt is sent to the melt metering pump through the bend of the spinning box to form a melt stream, and then ejected through the spinneret holes on the spinneret plate. During the process of ejecting the tow, the monomer suction device is used to suck the nylon 6 monomer, and the tow is cooled by the side blowing device and then oiled to obtain a primary tow; the shape of the spinneret hole is similar to a "W" shape, and both ends of the three vertical holes of the "W" shape spinneret hole are arc-shaped;
[0009] S3: The functional moisture-absorbing primary filament bundle enters the pre-network device and then enters the drawing component for stretching and high-temperature shaping, and then is rolled into a yarn roll by a winding device to obtain the multifunctional special-shaped composite nylon 6 fully drawn yarn fiber.
[0010] Furthermore, in step S1, the mass ratio of the alkali-soluble polyester masterbatch to the nylon 6 chips is (5-15): (85-95).
[0011] Furthermore, in step S1, the alkali-soluble polyester masterbatch has a relative viscosity of 1.0-1.5, a melting point of 230-240° C., and a water content of ≤500 ppm.
[0012] Furthermore, in step S1, the relative viscosity of the nylon 6 slice is 2.44-2.47, the melting point is 220-225° C., and the water content is ≤500 ppm.
[0013] Furthermore, in step S1, the processing temperature of the screw extruder is: the temperature of zone 1 is 245-252°C, the temperature of zone 2 is 251-256°C, the temperature of zone 3 is 255-261°C, the temperature of zone 4 is 261-266°C, and the temperature of zone 5 is 265-270°C. The screw extruder adopts biphenyl insulation, the temperature of the biphenyl insulation is 250-266°C, and the reduction ratio of the melt metering pump is 45-60.
[0014] Furthermore, in step S2, the side blowing temperature of the side blowing device is 17-24°C, the wind speed is 0.3-0.65m / s, and the relative humidity is 65-75%.
[0015] Furthermore, in step S2, the oiling agent model is 6352AY, the concentration is 8-12%, and the oiling amount of the tow is 1.2-1.6%.
[0016] Furthermore, in step S3, the pre-network air pressure of the pre-network device is 1.60-1.70 bar; the stretching ratio of the stretching process is 1.2-1.6; during the high-temperature shaping, the temperature of the hot roller is 160-170°C; the main network air pressure of the main network device is 2.60-2.65 bar; the winding speed of the winding device is 4100-4500 m / min
[0017] The second object of the present invention is to provide a multifunctional special-shaped composite nylon 6 fully drawn silk fiber, the cross-section of the multifunctional special-shaped composite nylon 6 fully drawn silk fiber is "W-shaped", and the middle part of the fiber is relatively wide and thick, showing an obvious expansion state.
[0018] Furthermore, the multifunctional special-shaped composite nylon 6 fully drawn yarn fiber is prepared by any of the above-mentioned preparation methods.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The present invention provides a method for preparing a multifunctional special-shaped composite nylon 6 fully drawn silk fiber, which uses alkali-soluble polyester masterbatch and nylon 6 chips as raw materials, and adopts an alkali reduction process to match them. The obtained yarn has gully pores, which can improve its moisture absorption and perspiration performance.
[0021] 2. The present invention provides a method for preparing a multifunctional special-shaped composite nylon 6 fully drawn silk fiber. During the spinning process, the spinneret hole of the special spinning assembly has a "W-shaped" special-shaped cross-section. At the moment when the melt is extruded through the "W-shaped" spinneret, due to the super-large force and the influence of thermal expansion and contraction, the radius of the middle vertical hole of the actual cross-section of the extruded fiber is larger than the radius of the vertical holes on both sides, and the protrusion of the middle position of the cross-section of the extruded fiber monofilament is larger than that on both sides, so that the special-shaped fiber monofilament has grooves of different heights on both sides, and then the special-shaped yarn spun by the fiber cannot fit together perfectly, and the grooves with arc-shaped structures themselves have deviations in the pore size of the yarn. If the same D number of fibers are produced, the yarn spun from the shaped composite fiber monofilament will be relatively thicker, and the number of pores will increase, resulting in better air permeability, so that the anti-ultraviolet performance of the yarn can be improved while its moisture absorption and quick-drying effect can be enhanced; at the same time, the structure of the fiber monofilament forms an arc-shaped groove structure, so that the entire shaped fiber monofilament is in an arc shape, and the light will be diffusely reflected on the surface of the fiber, and no bright spots will be generated. Since there are no sharp edges and corners, the wear of the components is less affected during the spinning or downstream weaving process; in addition, since the cross-section of the shaped fiber monofilament presents a multi-faceted arc shape, the surface area of the fiber is larger than that of ordinary circular, ordinary flat straight, cross or triangular shaped fibers. When the yarn spun from the shaped fiber is woven into a fabric that contacts human skin, the increase in contact area accelerates the thermal conductivity, thereby increasing the cool feeling at the moment of contact.
[0022] 3. The present invention provides a method for preparing a multifunctional special-shaped composite nylon 6 fully drawn silk fiber. Due to the difference in melting points between alkali-soluble polyester and nylon, in order to ensure normal spinning conditions and the spinnability of the fiber, the temperature is controlled in stages and regions during the blending process to reduce possible problems such as uneven yarns in the prepared fibers, which may affect the downstream weaving process.
[0023] 4. The present invention provides a method for preparing a multifunctional special-shaped composite nylon 6 fully drawn silk fiber, which adopts nylon 6 masterbatch and alkali-soluble polyester chips, and increases the "wicking" effect of the fiber by ensuring the special shape of the fiber. The prepared fiber has a groove phenomenon, and at the same time, the alkali reduction method is used in the subsequent dyeing and finishing process to control the alkali concentration at 5%-20%. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 A schematic diagram of the structure of a multifunctional special-shaped composite nylon 6 fully drawn yarn fiber provided by the present invention;
[0025] Figure 2 It is a schematic structural diagram of the "W-shaped" spinneret hole in the present invention. DETAILED DESCRIPTION
[0026] The following is in conjunction with the preferred embodiment and with reference to the attached Figure 1 , the present invention is further described. The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values; for numerical ranges, the endpoint values of each range, the endpoint values of each range and individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed herein; the materials, reagents, etc. used in the following examples, unless otherwise specified, can be obtained from commercial channels; the experimental methods in the following examples, unless otherwise specified, are all conventional methods.
[0027] Example 1
[0028] This embodiment provides a method for preparing a multifunctional special-shaped composite nylon 6 fully drawn filament fiber with a specification of 50D / 48F, comprising the following steps:
[0029] S1: Fully mix the alkali-soluble polyester masterbatch and nylon 6 chips in a mass ratio of 5:95 through a batching machine, and feed them into a screw extruder, and melt, mix, meter and extrude the melt under high temperature conditions; wherein the relative viscosity of the alkali-soluble polyester masterbatch is 1.25, the melting point is 235°C, and the water content is ≤500ppm; the relative viscosity of the nylon 6 chips is 2.45, the melting point is 222°C, and the water content is ≤500ppm;
[0030] In this embodiment, the five-zone temperatures of the screw extruder are 248°C, 252°C, 259°C, 262°C, and 266°C, respectively. The screw extruder adopts biphenyl insulation, the temperature of the biphenyl insulation is 260°C, and the speed reduction ratio of the melt metering pump is 45;
[0031] S2: The extruded melt is sent to the melt metering pump through the bend of the spinning box to form a melt stream, and then ejected through the spinneret holes on the spinneret. During the process of ejecting the tow, the monomer suction device is used to suck the nylon 6 monomer, and the tow is cooled by the side blowing device and then oiled to obtain a primary tow; the cross section of the spinneret holes on the spinneret is "W-shaped", and both ends of the three vertical holes of the "W-shaped" spinneret holes are arc-shaped, such as Figure 2 As shown, in this embodiment, the total length of the spinneret hole is 5.7 mm, the distance between the vertical holes is 2.4 mm, the length of the vertical hole is 2.1 mm, and the width of the transverse hole is 0.7 mm.
[0032] In this embodiment, the side blowing temperature of the side blowing device is 17°C, the wind speed is 0.3m / s, the relative humidity is 65%, the oiling agent model is 6352AY, the concentration is 8%, and the oiling amount of the tow is 1.2%;
[0033] S3: After the functional moisture-absorbing初生 silk bundle enters the pre-networker, it enters the drafting assembly for stretching and high-temperature setting, and then is wound into a silk roll by the winding device to obtain the multifunctional profiled composite polyamide 6 full-drawn yarn fiber. The schematic structural diagram is as Figure 1 shown. The cross-section of the multifunctional profiled composite polyamide 6 full-drawn yarn fiber is in the shape of a "king character", and the middle part of the fiber is relatively thick and wide, showing an obvious swelling shape.
[0034] In this embodiment, the pre-network air pressure of the pre-networker is 1.62 bar; the draw ratio in the stretching process is 1.2; in the high-temperature setting, the temperature of the hot roller is 162 °C; the main network air pressure of the main networker is 2.61 bar; the winding speed of the winding device is 4130 m / min.
[0035] Example 2
[0036] This embodiment provides a method for preparing a multifunctional profiled composite polyamide 6 full-drawn yarn fiber with a specification of 70D / 48F, including the following steps:
[0037] S1: The alkali-soluble polyester masterbatch and polyamide 6 chips with a mass ratio of 10:90 are mixed by a batching machine and put into a screw extruder. After melting, mixing, metering and extruding the melt under high-temperature conditions;
[0038] Among them, the relative viscosity of the alkali-soluble polyester masterbatch is 1.0, the melting point is 230 °C, and the water content ≤ 500 ppm; the relative viscosity of the polyamide 6 chips is 2.44, the melting point is 220 °C, and the water content ≤ 500 ppm;
[0039] In this embodiment, the five-zone temperatures of the screw extruder are 249 °C, 253 °C, 260 °C, 263 °C, and 266 °C respectively. The screw extruder uses diphenyl insulation, and the temperature of the diphenyl insulation is 245 °C. The reduction ratio of the melt metering pump is 50;
[0040] S2: The extruded melt is sent into the melt metering pump through the bend of the spinning box to form a melt stream, and then is ejected through the spinneret holes on the spinneret. During the process of spraying the silk bundle, the polyamide 6 monomer is sucked by the monomer suction device. After the silk bundle is cooled by the side blowing device, it is oiled to obtain the初生 silk bundle; the cross-section of the spinneret hole is in the shape of a "king character", and both ends of the three vertical holes of the "king character" spinneret hole are circular arcs;
[0041] In this embodiment, the side blowing temperature of the side blowing device is 20 °C, the wind speed is 0.5 m / s, the relative humidity is 70%, the oil agent model for oiling is 6352AY, the concentration is 10%, and the oil content on the silk bundle is 1.4%;
[0042] S3: The functional moisture-absorbing primary filament bundle enters the pre-network device and then enters the drawing component for stretching and high-temperature shaping, and then is rolled into a yarn roll by the winding device to obtain the multifunctional special-shaped composite nylon 6 fully drawn silk fiber. In this embodiment, the cross-section of the obtained multifunctional special-shaped composite nylon 6 fully drawn silk fiber is "W-shaped", and the middle part of the fiber is relatively wide and thick, showing an obvious expansion state.
[0043] In this embodiment, the pre-network air pressure of the pre-network device is 1.63 bar; the stretching ratio of the stretching process is 1.3; during the high-temperature setting, the temperature of the hot roller is 163°C; the main network air pressure of the main network device is 2.63 bar; and the winding speed of the winding device is 4200 m / min.
[0044] Example 3
[0045] This embodiment provides a method for preparing a multifunctional special-shaped composite nylon 6 fully drawn yarn fiber, the fully drawn yarn having a specification of 140D / 48F, comprising the following steps:
[0046] S1: Alkali-soluble polyester masterbatch and nylon 6 chips with a mass ratio of 15:85 are mixed by a batching machine and fed into a screw extruder, and the melt is melted, mixed, metered and extruded under high temperature conditions; wherein the relative viscosity of the alkali-soluble polyester masterbatch is 1.5, the melting point is 240°C, and the water content is ≤500ppm; the relative viscosity of the nylon 6 chips is 2.47, the melting point is 225°C, and the water content is ≤500ppm;
[0047] In this embodiment, the five-zone temperatures of the screw extruder are 250°C, 254°C, 260°C, 264°C, and 266°C, respectively. The screw extruder uses biphenyl insulation, the biphenyl insulation temperature is 250°C, and the melt metering pump reduction ratio is 60;
[0048] S2: The extruded melt is sent to the melt metering pump through the bend of the spinning box to form a melt stream, and then ejected through the spinneret holes on the spinneret plate. During the process of ejecting the tow, the monomer suction device is used to suck the nylon 6 monomer, and the tow is cooled by the side blowing device and then oiled to obtain a primary tow; the cross section of the spinneret hole is "W-shaped", and both ends of the three vertical holes of the "W-shaped" spinneret hole are arc-shaped;
[0049] In this embodiment, the side blowing temperature of the side blowing device is 24°C, the wind speed is 0.65m / s, the relative humidity is 75%, the oiling agent model is 6352AY, the concentration is 12%, and the oiling amount of the tow is 1.6%;
[0050] S3: The functional moisture-absorbing primary filament bundle enters the pre-network device and then enters the drawing component for stretching and high-temperature shaping, and then is rolled into a yarn roll by the winding device to obtain the multifunctional special-shaped composite nylon 6 fully drawn silk fiber. In this embodiment, the cross-section of the obtained multifunctional special-shaped composite nylon 6 fully drawn silk fiber is "W-shaped", and the middle part of the fiber is relatively wide and thick, showing an obvious expansion state.
[0051] In this embodiment, the pre-network air pressure of the pre-network device is 1.64 bar; the stretching ratio of the stretching process is 1.6; during the high-temperature setting, the temperature of the hot roller is 166°C; the main network air pressure of the main network device is 2.65 bar; and the winding speed of the winding device is 4430 m / min.
[0052] Comparative Example 1
[0053] The difference from Example 1 is that:
[0054] In step 1 of this comparative example, alkali-soluble polyester masterbatch and nylon 6 chips in a mass ratio of 0:100 are mixed by a batching machine and fed into a screw extruder.
[0055] Comparative Example 2
[0056] The difference from Example 1 is that:
[0057] In step S2 of this comparative example, the spinneret holes on the spinneret used are in a straight line shape.
[0058] Comparative Example 3
[0059] The difference from Example 1 is that:
[0060] In step S2 of this comparative example, the spinneret holes on the spinneret used are circular.
[0061] Implementation effect evaluation
[0062] The excellent effects achieved by the present invention are further illustrated by conducting specific tests on the nylon 6 fibers and woven fabrics obtained in Examples 1-3 and Comparative Examples 1-3, respectively:
[0063] The physical property test results are shown in the table below:
[0064] Table 1 Statistics of physical properties results
[0065]
[0066] Cooling performance test: According to the relevant standards of GB / T 35263-2017, a heat detection plate with a temperature higher than the specified temperature difference of the sample is brought into contact with the sample at a certain pressure. The maximum value of the heat flux density during the heat transfer process after the heat detection plate contacts the sample is used to calculate the contact cooling coefficient of the fabric;
[0067] Anti-ultraviolet performance test: According to the relevant standards of GB / T18830-2019, the ratio of the average effect of ultraviolet radiation calculated when the skin is unprotected to the average effect of ultraviolet radiation calculated when the skin is protected by fabric is UPF;
[0068] Moisture permeability (g / m 2 24h) test: moisture permeability test is carried out according to the relevant standards of GB / T12704.1-2009;
[0069] Evaporation rate test: According to the relevant standards of GB / T 21655.1-2008, a certain amount of water is dropped on the fabric, and then hung in the standard atmosphere to evaporate naturally. The evaporation mass per unit time in the linear interval of the time-evaporation curve is calculated;
[0070] Moisture absorption and quick-drying test: According to the relevant standards of GB / T 21655.2-2008, multiple fabric data are tested and calculated, such as wetting time and level, water absorption rate and level, maximum wetting radius of the penetration surface, etc., to judge whether the moisture absorption and quick-drying performance of the fabric meets the standards in multiple dimensions.
[0071] Table 2 Test results statistics
[0072]
[0073] As can be seen from the above table, in the cooling performance test results of the fabrics woven from nylon 6 fibers obtained in Examples 1-3, the contact cooling coefficient is 0.25-0.29, all greater than 0.15, indicating that the fabrics woven from the fibers of the present invention have instant air-drying performance upon contact; from the anti-ultraviolet performance test results, it can be seen that the anti-ultraviolet value UPF of the fabrics of Examples 1-3 is greater than 50, and it can be seen from the experimental data of Example 1 and Comparative Examples 1-3 that the fibers prepared by the present invention can greatly improve the anti-ultraviolet performance of the woven fabrics; from the data of Examples 1-3 and Comparative Examples 1-3, it can be seen that the perspective rates of Examples 1-3 are all greater than 10000, indicating that the fabrics woven from the fibers of the present invention have good perspective performance; from the evaporation rate test results of Examples 1-3, it can be seen that the test data are all greater than 0.18, indicating that the fabrics woven from the fibers of the present invention have good evaporation performance; from the moisture absorption and quick-drying and perspiration test data of Example 1 and Comparative Examples 1-3, it can be seen that the present invention can improve the moisture absorption and quick-drying and moisture absorption and perspiration properties of the fibers.
[0074] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several modifications and improvements without departing from the inventive concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for preparing a multifunctional special-shaped composite nylon 6 fully drawn yarn fiber, characterized in that: The following steps are involved: S1: Alkali-soluble polyester masterbatch and nylon 6 chips are mixed in a uniform proportion by a batching machine and fed into a screw extruder for melting, mixing, metering and extrusion of the melt under high temperature conditions; S2: The extruded melt is sent to the melt metering pump through the bend of the spinning box to form a melt stream, and then ejected through the spinneret holes on the spinneret plate. During the process of ejecting the tow, the monomer suction device is used to suck the nylon 6 monomer, and the tow is cooled by the side blowing device and then oiled to obtain a primary tow; the shape of the spinneret hole is similar to a "W" shape, and both ends of the three vertical holes of the "W" shape spinneret hole are arc-shaped; S3: The functional moisture-absorbing primary filament bundle enters the pre-network device for entanglement and the main network, and then enters the drawing component for stretching and high-temperature shaping, and then is rolled into a yarn roll by a winding device to obtain the multifunctional special-shaped composite nylon 6 fully drawn yarn fiber.
2. The method for preparing a multifunctional special-shaped composite nylon 6 fully drawn yarn according to claim 1, characterized in that: In step S1, the mass ratio of the alkali-soluble polyester masterbatch to the nylon 6 chips is (5-15): (85-95).
3. The method for preparing a multifunctional special-shaped composite nylon 6 fully drawn yarn according to claim 1, characterized in that: In step S1, the alkali-soluble polyester masterbatch has a relative viscosity of 1.0-1.5, a melting point of 230-240° C., and a water content of ≤500 ppm.
4. The method for preparing a multifunctional special-shaped composite nylon 6 fully drawn yarn according to claim 1, characterized in that: In step S1, the relative viscosity of the nylon 6 slice is 2.44-2.47, the melting point is 220-225° C., and the water content is ≤500 ppm.
5. The method for preparing a multifunctional special-shaped composite nylon 6 fully drawn yarn according to claim 1, characterized in that: In step S1, the processing temperature of the screw extruder is: the temperature of zone 1 is 245-252°C, the temperature of zone 2 is 251-256°C, the temperature of zone 3 is 255-261°C, the temperature of zone 4 is 261-266°C, and the temperature of zone 5 is 265-270°C. The screw extruder adopts biphenyl insulation, the temperature of the biphenyl insulation is 250-266°C, and the reduction ratio of the melt metering pump is 45-60.
6. The method for preparing a multifunctional special-shaped composite nylon 6 fully drawn yarn according to claim 1, characterized in that: In step S2, the side blowing temperature of the side blowing device is 17-24°C, the wind speed is 0.3-0.65m / s, and the relative humidity is 65-75%.
7. The method for preparing a multifunctional special-shaped composite nylon 6 fully drawn yarn according to claim 1, characterized in that: In step S2, the oiling agent model is 6352AY, the concentration is 8-12%, and the amount of oiling on the tow is 1.2-1.6%.
8. The method for preparing a multifunctional special-shaped composite nylon 6 fully drawn yarn according to claim 1, characterized in that: In step S3, the pre-network air pressure of the pre-network device is 1.60-1.70 bar; the stretching ratio of the stretching process is 1.2-1.6; during the high-temperature setting, the temperature of the hot roller is 160-170°C; the main network air pressure of the main network device is 2.60-2.65 bar; and the winding speed of the winding device is 4100-4500 m / min.
9. A multifunctional special-shaped composite nylon 6 fully drawn yarn fiber, characterized in that: The cross section of the multifunctional special-shaped composite nylon 6 fully drawn yarn fiber is in a "W" shape, and the middle part of the fiber is relatively wide and thick, showing an obvious expansion state.
10. The multifunctional special-shaped composite nylon 6 fully drawn yarn according to claim 9, characterized in that: The multifunctional special-shaped composite nylon 6 fully drawn silk fiber is prepared according to any one of the preparation methods described in claims 1-8.
Citation Information
Patent Citations
Method for producing knitted fabric having functions of strong acid resistance, strong base resistance and oil resistance
CN103215807A
Full-water-based environment-friendly superfine fiber leather manufacturing method
CN106192449A
Nylon 6 drafting yarn with bright spot effect and preparation method thereof
CN109576804A
Cool-feeling alkali-soluble chinlon 6 master batch and fiber and preparation method of application of cool-feeling alkali-soluble chinlon 6 master batch and fiber
CN118326540A
Silk coated synthetic fabrics
US20240141583A1