Polyester polyether resin water-washable moisture-absorbing quick-drying agent for polyester fiber and its blended fabrics and application method
By using block polyester polyether resin containing specific repeatability methylene chain segments on polyester fiber fabrics, the problem of poor water washing resistance is solved, and a wider and more applicable water washing resistance and moisture absorption quick drying effect is achieved. , and improves the stability and performance of finishing agents.
Patent Information
- Application Number
- CN202210818130.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-12
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-07-12
AI Technical Summary
The existing polyester polyether type moisture absorption quick-drying finishing agent has poor washing resistance on PBT fiber fabrics, and the market lacks functional finishing additives for the high-efficiency quick-drying effect of PBT and its blended fabrics.
Using block polyester polyether resin containing a specific repeatability methylene chain segment, it is prepared by transesterification and polycondensation reaction, combining specific molar feed ratios and functional monomers to adjust the melt viscosity and molecular regularity of the resin to improve the Its hydrophilicity and moisture-wicking properties on PBT and PTT fabrics.
It significantly improves the water-resistant and moisture-absorbing and quick-drying effect of PBT and PTT fabrics, expands the scope of application of finishing agents, improves the usability of products and emulsion stability, and reduces the impact on dye dispersion.
Smart Images

Figure BDA0003741664090000021 
Figure BDA0003741664090000151 
Figure BDA0003741664090000161
Abstract
Description
Technical Field
[0001] The invention belongs to the field of functional finishing of textile fabrics and is mainly used for polyester fabrics, especially for the washable, moisture-absorbing and quick-drying finishing of PBT fabrics. Background Art
[0002] The moisture absorption and quick-drying finishing of chemical fiber fabrics has become a necessary finishing process for almost all sports fabrics and underwear apparel. At present, the moisture absorption and quick-drying finishing agents used for polyester fabrics on the market are mostly polyester polyether type. This type of finishing agent has a good structural similarity with ordinary polyester fibers and is easy to finish on the fabric under high temperature conditions to achieve a washable moisture absorption and quick-drying effect. However, the washability of this conventional polyester-like finishing agent on general polyester fibers is mostly poor, especially on PBT (polybutylene terephthalate) fibers, whose commercial use has shown a significant increase in recent years, and its washable moisture absorption and quick-drying effect is even more unsatisfactory.
[0003] PBT fiber is a type of polyester fiber. Since the molecular chain contains a conjugated system formed by benzene rings and carboxyl groups similar to polyester, and contains aliphatic hydrocarbon chain segments with a length similar to nylon, it has the resilience and softness of polyamide fiber (nylon fiber) and many excellent mechanical properties of polyester fiber. Although PBT fiber has the above advantages, it has a low market share due to its high cost and late development. However, with the preference of consumers for high-end textiles and the gradual increase in domestic PBT fiber production capacity, the market share of PBT fabrics is increasing year by year; and as a high-end sports fabric, the requirements for washable and quick-drying finishing are bound to become higher and higher.
[0004] Yang Shikun pointed out in "Progress in Research on Structure and Properties of Polybutylene Terephthalate" (Polyester Industry, 1995(01):1-6) that different numbers of methylene groups in linear chain segments will lead to differences in the conformation of the macromolecular chain and the molecular chain elongation ratio in the crystal region (the ratio of the actual elongation length of the molecular chain to the theoretical elongation length). The molecular chain elongation ratio of PBT is only 86%, which is far from the 98.99% of PET (polyethylene terephthalate, commonly known as polyester); therefore, the water-resistant, moisture-absorbing and quick-drying finishing additive suitable for PBT fibers should have a chemical structure similar to that of the fiber to strengthen the intermolecular forces and the strength of hydrogen bonds and weaken the steric hindrance between the two molecules. However, the similarity between this type of finishing agent currently on the market and the chemical structure of PBT fiber is low. Moreover, due to the differences in the length and spatial configuration of the fat chain segments, its affinity with PBT fabrics is correspondingly smaller. Therefore, when used on PBT fabrics, the amount of additives treated on the fabrics is lower; the water-washing resistance, moisture absorption and quick-drying effects are also relatively poorer.
[0005] Currently, there is no functional finishing additive on the market that has a good quick-drying effect on PBT and its blended fabrics. Summary of the invention
[0006] The present invention mainly solves the deficiencies in the prior art and provides a water-resistant moisture-absorbing quick-drying agent for polyester fiber and its blended fabrics and an application method to solve the problems involved in the background technology.
[0007] The above technical problems of the present invention are mainly solved by the following technical solutions:
[0008] A polyester polyether resin water-resistant moisture-absorbing quick-drying agent for polyester fiber and its blended fabrics, characterized in that the resin is a block polyester polyether resin containing a specific repeating methylene segment, and its structure is as follows:
[0009]
[0010] Among them, AO is a structural unit of polyethylene glycol, polypropylene glycol or polytetrahydrofuran; the ranges of x, y, z and m are: 8≤x≤135, 0≤y≤10, 1≤z≤10, 1≤m≤30 respectively; n is one or more of 3, 4, 5, 6; R is H or NaSO3-.
[0011] The block polyester polyether resin containing a specific repeating methylene segment in the present invention is prepared by using a diol containing a specific repeating methylene segment, ethylene terephthalate, polyether diol, ethylene isophthalate and / or sodium 1,3-dimethyl 5-sulfonate through ester exchange and polycondensation reaction.
[0012] The diol containing methylene groups with a specific repeating degree has a methylene repeating degree of 3-6; more preferably, it is 1,4-butanediol and / or 1,3-propylene glycol.
[0013] The molar feed ratio of ethylene terephthalate to ethylene isophthalate and / or sodium dimethyl 5-sulfonate is 10:1-10:5, and more preferably 10:1-10:3.
[0014] The molar feed ratio of ethylene terephthalate to polyether diol is 5:1-5:5, and more preferably 5:1-5:3.
[0015] The polyether diol is one of polyethylene glycol, polypropylene glycol and polytetrahydrofuran or a mixture thereof, and has a molecular weight range of 600-6000, and more preferably 3000-5000.
[0016] Preferably, the block polyester polyether resin containing a methylene segment with a specific repeating degree has a melt viscosity of 3000-30000 mPa.s.
[0017] The test conditions of melt viscosity are: cone and plate viscometer; 6# rotor; 150°C; 100 rpm.
[0018] The invention discloses an application method of a polyester polyether resin water-resistant moisture-absorbing and quick-drying agent for polyester fiber and its blended fabrics. The water-resistant moisture-absorbing and quick-drying agent is used for polyester fiber and its blended fabrics.
[0019] As a preferred embodiment, the moisture absorption and quick-drying finishing process is particularly performed on PBT fibers and their blended fabrics.
[0020] Preferably, the moisture absorption and quick-drying finishing includes but is not limited to dyeing in one bath, dipping, padding and spraying related functional finishing processes.
[0021] PBT refers to polybutylene terephthalate fiber; PTT refers to polytrimethylene terephthalate.
[0022] The present invention relates to a water-resistant moisture-absorbing quick-drying agent for polyester fiber and its blended fabric and an application method thereof, which has the following beneficial effects compared with the prior art:
[0023] 1. The water-washable moisture absorption quick-drying finishing agent of the present invention uses a block polyester polyether resin containing a specific repetitive methylene segment as the main component, which can not only improve the hydrophilicity and moisture absorption and perspiration of ordinary polyester fabrics; but also can achieve water-washable moisture absorption quick-drying finishing on fabrics such as PBT, PTT, etc. that are difficult to finish with traditional quick drying, as well as various polyester blended fabrics by adjusting the repetitiveness of the methylene segments in the resin. Compared with the traditional polyester polyether finishing agent on the market, the application of the present invention is not only wider, but also its performance for special polyester fabrics is more superior through structural design.
[0024] 2. The present invention preferably uses a special organic solvent for commercialization, which, on the one hand, makes the synthesized hydrophilic resin easier to emulsify and disperse in water; at the same time, it effectively weakens the strength of the hydrogen bond network formed by the three phases in the emulsion system, avoiding excessive viscosity of the main resin with a longer soft segment during emulsification, which affects the low-temperature stability or performance of the final finishing agent, thereby improving the usability of the product.
[0025] 3. By adjusting the mass feed ratio of ethylene terephthalate to ethylene isophthalate and / or sodium dimethyl 5-sulfonate, the regularity of the block polyester polyether resin is controlled, the glass transition temperature and crystallinity of the resin are reduced, and the obtained polyester polyether resin is more easily emulsified and the emulsion stability is higher.
[0026] 4. By controlling the mass feed ratio of polyether diol to ethylene terephthalate, the ratio of hydrophilic segments to hydrophobic segments is adjusted, thereby adjusting the dispersion state and turbidity point of the resin macromolecules in the aqueous phase and improving the affinity between the finishing agent and the target fabric.
[0027] 5. By controlling the type and molecular weight of polyether diols, the hydrophilicity, fiber affinity and emulsification of block polyester polyether resins can be improved.
[0028] 6. By designing the molecules of block polyester polyether resin, excellent water-resistant and quick-drying properties are ensured, while the emulsification of the resin is improved, the stability of the emulsion is improved, and the impact on the dispersibility of the dye is reduced. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is further specifically described below through embodiments.
[0030] In the following description, a large number of specific details are provided to provide a more thorough understanding of the present invention. However, it is apparent to those skilled in the art that the present invention can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present invention, some technical features well known in the art are not described.
[0031] The present invention will be further described below in conjunction with the embodiments, and the examples of the embodiments are intended to explain the present invention and should not be construed as limiting the present invention. Where specific techniques and reaction conditions are not specified in the embodiments, the techniques or conditions described in the literature in the art or the product specifications may be used.
[0032] Example 1: 1) 0.6 mol of ethylene terephthalate, 0.3 mol of ethylene glycol, 0.24 mol of 1,3-propylene glycol, 0.18 mol of ethylene isophthalate and 0.36 mol of PEG-4000 were added to a split reactor equipped with a thermometer, a reflux condenser and a stirrer, melt-stirred in a N2 atmosphere, and heated to 150 (± 3) ° C., and then 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate was added in a mass ratio of 1:1, and the temperature was continued to be raised to 185 (± 5) ° C. The reaction was kept warm to ensure that the distillate amount was greater than 95% of the theoretical amount;
[0033] The temperature was continued to rise to 260 (± 3) °C, the introduction of N2 was stopped, and the vacuum was gradually evacuated to 10 Torr. Under this condition, the temperature and pressure were maintained for a certain period of time, and the melt viscosity of the resin was 18260 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal pressure, and a block polyester polyether hydrophilic resin 1 was obtained.
[0034] 2) Stir and cool to 170°C, add 2% tetramethyl urea by weight of the hydrophilic resin, stir thoroughly, adjust the temperature to 130°C, keep warm and stir for 1 hour, then slowly discharge into an emulsifying kettle pre-added with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus prepare a water-resistant moisture-absorbing quick-drying agent 1. Its application effect is shown in Table 1.
[0035] Example 2: 1) 0.6 mol of ethylene terephthalate, 0.3 mol of ethylene glycol, 0.24 mol of 1,4-butanediol, 0.18 mol of ethylene isophthalate and 0.36 mol of PEG-4000 were added to a split reactor equipped with a thermometer, a reflux condenser and a stirrer, melt-stirred in a N2 atmosphere, and when the temperature was raised to 150 (± 3) ° C, a total feed amount of 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate was added, the mass ratio was 1:1, and the temperature was continued to be raised to 185 (± 5) ° C, and the reaction was kept warm to ensure that the distillate amount was greater than 95% of the theoretical amount;
[0036] The temperature was continued to rise to 260 (± 3) °C, the introduction of N2 was stopped, and the vacuum was gradually evacuated to 10 Torr. Under this condition, the temperature and pressure were maintained for a certain period of time, and the melt viscosity of the resin was 18190 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal pressure, and a block polyester polyether hydrophilic resin 2 was obtained.
[0037] 2) Stir and cool to 170°C, add 2% tetramethyl urea by weight of hydrophilic resin, stir well, adjust the temperature to 130°C, keep warm and stir for 1 hour, then slowly discharge into an emulsifying kettle pre-added with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus prepare a water-resistant moisture-absorbing quick-drying agent 2. Its application effect is shown in Table 1.
[0038] Example 3: 1) 0.6 mol of ethylene terephthalate, 0.3 mol of ethylene glycol, 0.24 mol of 1,6-hexanediol, 0.18 mol of ethylene isophthalate and 0.36 mol of PEG-4000 were added to a split reactor equipped with a thermometer, a reflux condenser and a stirrer, melted and stirred in a N2 atmosphere, and when the temperature was raised to 150 (± 3) ° C, a total feed amount of 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate was added, the mass ratio was 1:1, and the temperature was continued to rise to 185 (± 5) ° C, and the reaction was kept warm to ensure that the distillate amount was greater than 95% of the theoretical amount;
[0039] The temperature was continued to rise to 260 (± 3) °C, the introduction of N2 was stopped, and the vacuum was gradually evacuated to 10 Torr. Under this condition, the temperature and pressure were maintained for a certain period of time, and the melt viscosity of the resin was 18250 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal pressure, and a block polyester polyether hydrophilic resin 3 was obtained.
[0040] 2) Stir and cool to 170°C, add 2% tetramethyl urea by weight of hydrophilic resin, stir well, adjust the temperature to 130°C, keep warm and stir for 1h, then slowly discharge into an emulsifying kettle pre-added with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus prepare a water-resistant moisture-absorbing quick-drying agent 3. Its application effect is shown in Table 1.
[0041] Example 4: 1) 0.6 mol of ethylene terephthalate, 0.3 mol of ethylene glycol, 0.13 mol of 1,4-butanediol, 0.18 mol of ethylene isophthalate and 0.36 mol of PEG-4000 were added to a split reactor equipped with a thermometer, a reflux condenser and a stirrer, melt-stirred in a N2 atmosphere, and when the temperature was raised to 150 (± 3) ° C, a total feed amount of 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate was added, the mass ratio was 1:1, and the temperature was continued to be raised to 185 (± 5) ° C, and the reaction was kept warm to ensure that the distillate amount was greater than 95% of the theoretical amount;
[0042] The temperature was continued to rise to 260 (± 3) °C, the introduction of N2 was stopped, and the vacuum was gradually evacuated to 10 Torr. Under this condition, the temperature and pressure were maintained for a certain period of time, and the melt viscosity of the resin was 18100 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal pressure, and a block polyester polyether hydrophilic resin 4 was obtained.
[0043] 2) Stir and cool to 170°C, add 2% tetramethyl urea by weight of hydrophilic resin, stir thoroughly, adjust the temperature to 130°C, keep warm and stir for 1 hour, then slowly discharge into an emulsifying kettle pre-added with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus prepare a water-resistant moisture-absorbing quick-drying agent 4. Its application effect is shown in Table 1.
[0044] Example 5: 1) 0.6 mol of ethylene terephthalate, 0.3 mol of ethylene glycol, 0.24 mol of 1,4-butanediol, 0.18 mol of ethylene isophthalate and 0.36 mol of PEG-600 were added to a split reactor equipped with a thermometer, a reflux condenser and a stirrer, melt-stirred in a N2 atmosphere, and when the temperature was raised to 150 (± 3) ° C, a total feed amount of 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate was added, the mass ratio was 1:1, and the temperature was continued to be raised to 185 (± 5) ° C, and the reaction was kept warm to ensure that the distillate amount was greater than 95% of the theoretical amount;
[0045] The temperature was continued to rise to 260 (± 3) °C, the introduction of N2 was stopped, and the vacuum was gradually evacuated to 10 Torr. Under this condition, the temperature and pressure were maintained for a certain period of time, and the melt viscosity of the resin was 18070 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal pressure, and a block polyester polyether hydrophilic resin 5 was obtained.
[0046] 2) Stir and cool to 170°C, add 2% tetramethyl urea by weight of hydrophilic resin, stir thoroughly, adjust the temperature to 130°C, keep warm and stir for 1h, then slowly discharge into an emulsifying kettle pre-added with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus prepare a water-resistant moisture-absorbing quick-drying agent 5. Its application effect is shown in Table 1.
[0047] Example 6: 1) 0.6 mol of ethylene terephthalate, 0.3 mol of ethylene glycol, 0.24 mol of 1,4-butanediol, 0.18 mol of ethylene isophthalate and 0.36 mol of PEG-3000 were added to a split reactor equipped with a thermometer, a reflux condenser and a stirrer, melted and stirred in a N2 atmosphere, and when the temperature was raised to 150 (± 3) ° C, a total feed amount of 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate (mass ratio of 1:1) was added, and the temperature was continued to be raised to 185 (± 5) ° C, and the reaction was kept warm to ensure that the distillate amount was greater than 95% of the theoretical amount;
[0048] The temperature was continued to rise to 260 (± 3) °C, the introduction of N2 was stopped, and the vacuum was gradually evacuated to 10 Torr. Under this condition, the temperature and pressure were maintained for a certain period of time, and the melt viscosity of the resin was 18110 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal pressure, and a block polyester polyether hydrophilic resin 6 was obtained.
[0049] 2) Stir and cool to 170°C, add 2% tetramethyl urea by weight of hydrophilic resin, stir well, adjust the temperature to 130°C, keep warm and stir for 1 hour, then slowly discharge into an emulsifying kettle pre-added with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus prepare a water-resistant moisture-absorbing quick-drying agent 6. Its application effect is shown in Table 1.
[0050] Example 7: 1) 0.6 mol of ethylene terephthalate, 0.3 mol of ethylene glycol, 0.24 mol of 1,4-butanediol, 0.18 mol of ethylene isophthalate and 0.36 mol of PEG-6000 were added to a split reactor equipped with a thermometer, a reflux condenser and a stirrer, melted and stirred in a N2 atmosphere, and when the temperature was raised to 150 (± 3) ° C, a total feed amount of 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate was added, the mass ratio was 1:1, and the temperature was continued to rise to 185 (± 5) ° C, and the reaction was kept warm to ensure that the distillate amount was greater than 95% of the theoretical amount;
[0051] The temperature was continued to rise to 260 (± 3) °C, the introduction of N2 was stopped, and the vacuum was gradually evacuated to 10 Torr. Under this condition, the temperature and pressure were maintained for a certain period of time, and the melt viscosity of the resin was 18220 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal pressure, and a block polyester polyether hydrophilic resin 7 was obtained.
[0052] 2) Stir and cool to 170°C, add 2% tetramethyl urea by weight of hydrophilic resin, stir well, adjust the temperature to 130°C, keep warm and stir for 1 hour, then slowly discharge into an emulsifying kettle pre-added with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus prepare a water-resistant moisture-absorbing quick-drying agent 7. Its application effect is shown in Table 1.
[0053] Example 8: 1) 0.6 mol of ethylene terephthalate, 0.3 mol of ethylene glycol, 0.24 mol of 1,4-butanediol, 0.3 mol of ethylene isophthalate and 0.36 mol of PEG-4000 were added to a split reactor equipped with a thermometer, a reflux condenser and a stirrer, melt-stirred in a N2 atmosphere, and when the temperature was raised to 150 (± 3) ° C, a total feed amount of 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate was added, the mass ratio was 1:1, and the temperature was continued to rise to 185 (± 5) ° C, and the reaction was kept warm to ensure that the distillate amount was greater than 95% of the theoretical amount;
[0054] The temperature was continued to rise to 260 (± 3) °C, the introduction of N2 was stopped, and the vacuum was gradually evacuated to 10 Torr. Under this condition, the temperature and pressure were maintained for a certain period of time, and the melt viscosity of the resin was 18280 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal pressure, and a block polyester polyether hydrophilic resin 8 was obtained.
[0055] 2) Stir and cool to 170°C, add 2% tetramethyl urea by weight of hydrophilic resin, stir thoroughly, adjust the temperature to 130°C, keep warm and stir for 1 hour, then slowly discharge into an emulsifying kettle pre-added with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus prepare a water-resistant moisture-absorbing quick-drying agent 8. Its application effect is shown in Table 1.
[0056] Example 9: 1) 0.6 mol of ethylene terephthalate, 0.3 mol of ethylene glycol, 0.24 mol of 1,4-butanediol, 0.18 mol of ethylene isophthalate and 0.36 mol of PEG-4000 were added to a split reactor equipped with a thermometer, a reflux condenser and a stirrer, melt-stirred in a N2 atmosphere, and when the temperature was raised to 150 (± 3) ° C, a total feed amount of 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate was added in a mass ratio of 1:1, and the temperature was continued to be raised to 185 (± 5) ° C, and the reaction was kept warm to ensure that the distillate amount was greater than 95% of the theoretical amount;
[0057] The temperature was continued to rise to 260 (± 3) °C, the introduction of N2 was stopped, and the vacuum was gradually evacuated to 10 Torr. Under this condition, the temperature and pressure were maintained for a certain period of time, and the melt viscosity of the resin was 4260 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal pressure, and a block polyester polyether hydrophilic resin 9 was obtained.
[0058] 2) Stir and cool to 170°C, add 2% tetramethyl urea by weight of hydrophilic resin, stir well, adjust the temperature to 130°C, keep warm and stir for 1h, then slowly discharge into an emulsifying kettle pre-added with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus prepare a water-resistant moisture-absorbing quick-drying agent 9. Its application effect is shown in Table 1.
[0059] Comparative Example 1: 1) 0.6 mol of ethylene terephthalate, 0.54 mol of ethylene glycol, 0.18 mol of ethylene isophthalate and 0.36 mol of PEG-4000 were added to a split reactor equipped with a thermometer, a reflux condenser and a stirrer, melted and stirred in a N2 atmosphere, and when the temperature was raised to 150 (± 3) ° C, a total feed amount of 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate was added, the mass ratio was 1:1, and the temperature was continued to rise to 185 (± 5) ° C, and the reaction was kept warm to ensure that the distillate amount was greater than 95% of the theoretical amount;
[0060] The temperature was continued to rise to 260 (± 3) °C, the introduction of N2 was stopped, and the vacuum was gradually evacuated to 10 Torr. Under this condition, the temperature and pressure were maintained for a certain period of time, and the melt viscosity of the resin was 18060 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal pressure, and a block polyester polyether hydrophilic resin 10 was obtained.
[0061] 2) Stir and cool to 170°C, add 2% tetramethyl urea by weight of the hydrophilic resin, stir thoroughly, adjust the temperature to 130°C, keep warm and stir for 1 hour, then slowly discharge into an emulsifying kettle pre-added with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus prepare a water-resistant moisture-absorbing quick-drying agent 10. Its application effect is shown in Table 1.
[0062] Comparative Example 2: 1) 0.6 mol of ethylene terephthalate, 0.3 mol of ethylene glycol, 0.24 mol of 1,7-heptanediol, 0.18 mol of ethylene isophthalate and 0.36 mol of PEG-4000 were added to a split reactor equipped with a thermometer, a reflux condenser and a stirrer, melted and stirred in a N2 atmosphere, and when the temperature was raised to 150 (± 3) ° C, a total feed amount of 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate was added, the mass ratio was 1:1, and the temperature was continued to rise to 185 (± 5) ° C, and the reaction was kept warm to ensure that the distillate amount was greater than 95% of the theoretical amount;
[0063] The temperature was continued to rise to 260 (± 3) °C, the introduction of N2 was stopped, and the vacuum was gradually evacuated to 10 Torr. Under this condition, the temperature and pressure were maintained for a certain period of time, and the melt viscosity of the resin was 18210 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal, and a block polyester polyether hydrophilic resin 11 was obtained.
[0064] 2) Stir and cool to 170°C, add 2% tetramethyl urea by weight of hydrophilic resin, stir thoroughly, adjust the temperature to 130°C, keep warm and stir for 1 hour, then slowly discharge into an emulsifying kettle pre-added with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus prepare a water-resistant moisture-absorbing quick-drying agent 11. Its application effect is shown in Table 1.
[0065] Comparative Example 3: 1) 0.6 mol of ethylene terephthalate, 0.3 mol of ethylene glycol, 0.24 mol of 1,4-butanediol, 0.18 mol of ethylene isophthalate and 0.06 mol of PEG-4000 were added to a split reactor equipped with a thermometer, a reflux condenser and a stirrer, melted and stirred in a N2 atmosphere, and when the temperature was raised to 150 (± 3) ° C, a total feed amount of 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate was added, the mass ratio was 1:1, and the temperature was continued to rise to 185 (± 5) ° C, and the reaction was kept warm to ensure that the distillate amount was greater than 95% of the theoretical amount;
[0066] The temperature was continued to rise to 260 (± 3) °C, the introduction of N2 was stopped, and the vacuum was gradually evacuated to 10 Torr. Under this condition, the temperature and pressure were maintained for a certain period of time, and the melt viscosity of the resin was 18090 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal pressure, and a block polyester polyether hydrophilic resin 12 was obtained.
[0067] 2) Stir and cool to 170°C, add 2% tetramethyl urea by weight of hydrophilic resin, stir thoroughly, adjust the temperature to 130°C, keep warm and stir for 1 hour, then slowly discharge into an emulsifying kettle pre-added with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus prepare a water-resistant moisture-absorbing quick-drying agent 12. Its application effect is shown in Table 1.
[0068] Comparative Example 4: 1) 0.6 mol of ethylene terephthalate, 0.3 mol of ethylene glycol, 0.24 mol of 1,4-butanediol, 0.18 mol of ethylene isophthalate and 6 mol of PEG-4000 were added to a split reactor equipped with a thermometer, a reflux condenser and a stirrer, melted and stirred in a N2 atmosphere, and when the temperature was raised to 150 (± 3) ° C, a total feed amount of 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate was added, the mass ratio was 1:1, and the temperature was continued to rise to 185 (± 5) ° C, and the reaction was kept warm to ensure that the distillate distillate was greater than 95% of the theoretical amount;
[0069] The temperature was continued to rise to 260 (± 3) °C, and the introduction of N2 was stopped. The vacuum was gradually evacuated to 10 Torr, and the temperature and pressure were maintained under this condition for a certain period of time. The melt viscosity of the resin was 18030 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal pressure, and a block polyester polyether hydrophilic resin 13 was obtained.
[0070] 2) Stir and cool to 170°C, add 2% tetramethyl urea by weight of the hydrophilic resin, stir thoroughly, adjust the temperature to 130°C, keep warm and stir for 1 hour, then slowly discharge into an emulsifying kettle pre-added with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus prepare a water-resistant moisture-absorbing quick-drying agent 13. Its application effect is shown in Table 1.
[0071] Comparative Example 5: 1) 0.6 mol of ethylene terephthalate, 0.3 mol of ethylene glycol, 0.24 mol of 1,4-butanediol, 0.18 mol of ethylene isophthalate and 0.36 mol of PEG-400 were added to a split reactor equipped with a thermometer, a reflux condenser and a stirrer, melted and stirred in a N2 atmosphere, and when the temperature was raised to 150 (± 3) ° C, a total feed amount of 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate was added, the mass ratio was 1:1, and the temperature was continued to rise to 185 (± 5) ° C, and the reaction was kept warm to ensure that the distillate amount was greater than 95% of the theoretical amount;
[0072] The temperature was continued to rise to 260 (± 3) °C, the introduction of N2 was stopped, and the vacuum was gradually evacuated to 10 Torr. Under this condition, the temperature and pressure were maintained for a certain period of time, and the melt viscosity of the resin was 18290 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal pressure, and a block polyester polyether hydrophilic resin 14 was obtained.
[0073] 2) Stir and cool to 170°C, add 2% tetramethyl urea by weight of the hydrophilic resin, stir thoroughly, adjust the temperature to 130°C, keep warm and stir for 1 hour, then slowly discharge into an emulsifying kettle pre-added with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus obtain a water-resistant moisture-absorbing quick-drying agent 14. The application effect is shown in Table 1.
[0074] Comparative Example 6: 1) 0.6 mol of ethylene terephthalate, 0.3 mol of ethylene glycol, 0.24 mol of 1,4-butanediol, 0.18 mol of ethylene isophthalate and 0.36 mol of PEG-8000 were added to a split reactor equipped with a thermometer, a reflux condenser and a stirrer, melted and stirred in a N2 atmosphere, and when the temperature was raised to 150 (± 3) ° C, a total feed amount of 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate was added, the mass ratio was 1:1, and the temperature was continued to rise to 185 (± 5) ° C, and the reaction was kept warm to ensure that the distillate amount was greater than 95% of the theoretical amount;
[0075] The temperature was continued to rise to 260 (± 3) °C, the introduction of N2 was stopped, and the vacuum was gradually evacuated to 10 Torr. Under this condition, the temperature and pressure were maintained for a certain period of time, and the melt viscosity of the resin was 18120 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal, and a block polyester polyether hydrophilic resin 15 was obtained.
[0076] 2) Stir and cool to 170°C, add 2% tetramethyl urea by weight of the hydrophilic resin, stir thoroughly, adjust the temperature to 130°C, keep warm and stir for 1 hour, then slowly discharge into an emulsifying kettle pre-added with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus obtain a water-resistant moisture-absorbing quick-drying agent 15. The application effect is shown in Table 1.
[0077] Comparative Example 7: 1) 0.6 mol of ethylene terephthalate, 0.3 mol of ethylene glycol, 0.24 mol of 1,4-butanediol, and 0.36 mol of PEG-4000 were added to a split reactor equipped with a thermometer, a reflux condenser, and a stirrer, melted and stirred in a N2 atmosphere, and when the temperature was raised to 150 (± 3) ° C, a total feed amount of 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate was added, the mass ratio was 1:1, and the temperature was continued to be raised to 185 (± 5) ° C, and the reaction was kept warm to ensure that the distillate amount was greater than 95% of the theoretical amount;
[0078] The temperature was continued to rise to 260 (± 3) °C, the introduction of N2 was stopped, and the vacuum was gradually evacuated to 10 Torr. Under this condition, the temperature and pressure were maintained for a certain period of time, and the melt viscosity of the resin was 18130 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal pressure, and a block polyester polyether hydrophilic resin 16 was obtained.
[0079] 2) Stir and cool to 170°C, add 2% tetramethyl urea by weight of the hydrophilic resin, stir thoroughly, adjust the temperature to 130°C, keep warm and stir for 1 hour, then slowly discharge into an emulsifying kettle pre-added with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus obtain a water-resistant moisture-absorbing quick-drying agent 16. The application effect is shown in Table 1.
[0080] Comparative Example 8: 1) 0.6 mol of ethylene terephthalate, 0.3 mol of ethylene glycol, 0.24 mol of 1,4-butanediol, 0.18 mol of ethylene isophthalate and 0.36 mol of PEG-4000 were added to a split reactor equipped with a thermometer, a reflux condenser and a stirrer, melted and stirred in a N2 atmosphere, and when the temperature was raised to 150 (± 3) ° C, a total feed amount of 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate was added, the mass ratio was 1:1, and the temperature was continued to rise to 185 (± 5) ° C, and the reaction was kept warm to ensure that the distillate amount was greater than 95% of the theoretical amount;
[0081] The temperature was continued to rise to 260 (± 3) °C, and the introduction of N2 was stopped. The vacuum was gradually evacuated to 10 Torr, and the temperature and pressure were maintained under this condition for a certain period of time. The melt viscosity of the resin was 2090 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal pressure, and a block polyester polyether hydrophilic resin 17 was obtained.
[0082] 2) Stir and cool to 170°C, add 2% tetramethyl urea by weight of hydrophilic resin, stir thoroughly, adjust the temperature to 130°C, keep warm and stir for 1 hour, then slowly discharge into an emulsifying kettle pre-added with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus prepare a water-resistant moisture-absorbing quick-drying agent 17. Its application effect is shown in Table 1.
[0083] Comparative Example 9: 1) 0.6 mol of ethylene terephthalate, 0.3 mol of ethylene glycol, 0.24 mol of 1,4-butanediol, 0.18 mol of ethylene isophthalate and 0.36 mol of PEG-4000 were added to a split reactor equipped with a thermometer, a reflux condenser and a stirrer, melted and stirred in a N2 atmosphere, and when the temperature was raised to 150 (± 3) ° C, a total feed amount of 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate was added, the mass ratio was 1:1, and the temperature was continued to rise to 185 (± 5) ° C, and the reaction was kept warm to ensure that the distillate amount was greater than 95% of the theoretical amount;
[0084] The temperature was continued to rise to 260 (± 3) °C, and the introduction of N2 was stopped. The vacuum was gradually evacuated to 10 Torr, and the temperature and pressure were maintained under this condition for a certain period of time. The melt viscosity of the resin was 35160 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal pressure, and a block polyester polyether hydrophilic resin 18 was obtained.
[0085] 2) Stir and cool to 170°C, add 2% tetramethyl urea by weight of hydrophilic resin, stir thoroughly, adjust the temperature to 130°C, keep warm and stir for 1 hour, then slowly discharge into an emulsifying kettle pre-added with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus prepare a water-resistant moisture-absorbing quick-drying agent 18. Its application effect is shown in Table 1.
[0086] Comparative Example 10: 1) 0.6 mol of ethylene terephthalate, 0.3 mol of ethylene glycol, 0.24 mol of 1,4-butanediol, 0.18 mol of ethylene isophthalate and 0.36 mol of PEG-4000 were added to a split reactor equipped with a thermometer, a reflux condenser and a stirrer, melted and stirred in a N2 atmosphere, and when the temperature was raised to 150 (± 3) ° C, a total feed amount of 0.15‰ of a composite catalyst of zinc acetate and tetrabutyl titanate was added, the mass ratio was 1:1, and the temperature was continued to rise to 185 (± 5) ° C, and the reaction was kept warm to ensure that the distillate amount was greater than 95% of the theoretical amount;
[0087] The temperature was continued to rise to 260 (± 3) °C, the introduction of N2 was stopped, and the vacuum was gradually evacuated to 10 Torr. Under this condition, the temperature and pressure were maintained for a certain period of time, and the melt viscosity of the resin was 18190 mPa.s. After the reaction was completed, N2 was introduced to restore the pressure to normal pressure, and a block polyester polyether hydrophilic resin 2 was obtained.
[0088] 2) Stir and cool to 170°C, add ethylene glycol (2% by weight of the hydrophilic resin), stir thoroughly, adjust the temperature to 130°C, keep warm and stir for 1 hour, then slowly discharge into an emulsifying kettle pre-filled with 65°C hot water, stir and disperse, complete the emulsification of the synthetic resin, and thus obtain a water-resistant moisture-absorbing quick-drying agent 19. The application effect is shown in Table 1.
[0089] Test example:
[0090] The quick-drying performance of the water-washable moisture-absorbing quick-drying finishing agents prepared in the above embodiments and comparative examples was evaluated according to the diffusive moisture residual rate test method.
[0091] The specific operation method of the diffusive moisture residual rate (residual water rate) test method is as follows: take a 10cm×10cm size of the test fabric (avoid the edges, defects and wrinkles), and adjust the humidity for at least 4 hours under the conditions of T=20±2℃, RH=65±2%; accurately absorb 0.3mL of distilled water and drop it on the surface of the test fabric sample (skin-friendly surface), test the mass of the fabric sample after each equal interval, and calculate the moisture residual rate of the fabric surface after 60 minutes according to the following formula:
[0092] Residual moisture rate (%) = (W0-W') / (W 60 -W′)×100
[0093] Where: W0 is the initial mass of the test fabric sample after water is added;
[0094] W t To test the mass of the fabric sample 60 minutes after water is added;
[0095] W' is the weight of the cloth.
[0096] The test of drip diffusion time is carried out according to the specific method in GBT 21655.1-2008 Evaluation of moisture absorption and quick-drying properties of textiles Part 1 Single item combination test method;
[0097] The low temperature stability test method of the water-washable moisture-absorbing quick-drying finishing agent prepared in the above embodiments and comparative examples is as follows: 200 g of the sample is placed in a glass bottle with a sealed lid and placed in a -5°C low temperature constant temperature box for 7 days; after 7 days, the fluidity of the emulsion is observed. If the emulsion can still flow normally, it is judged that its low temperature stability is good; if the emulsion freezes or forms a jelly and loses fluidity, it is judged that its low temperature stability is poor.
[0098] The PBT fabric is a PBT / PET (blending ratio: 50 / 50) blended knitted fabric, the PTT fabric is a PTT / PET (blending ratio: 70 / 30) blended knitted fabric, and the PET fabric is a 100% pure polyester knitted fabric.
[0099] The washing process of the finished fabric was carried out according to JIS L 0217103 method.
[0100] The model of the commercially available product is NICEPOLE PR-9000 (produced by Nichia Chemical (China) Co., Ltd.)
[0101] The application properties, unless otherwise specified, are all the application results of the invented finishing agent in the dyeing one-bath process.
[0102]
[0103]
[0104]
[0105] Compared with conventional moisture absorbing and quick-drying agents, Examples 1 to 3 have better water-resistant moisture absorbing and quick-drying effects on PBT and PTT fabrics. Compared with Example 2, Examples 4-9 provide possible changes in various monomers, raw materials and specifications in the present invention, and point out the influence of various factors on the final resin application effect. By comparing Examples 2, 8 and Comparative Example 7, it can be seen that by controlling the molar feed ratio of ethylene terephthalate to ethylene isophthalate, the molecular regularity of the block polyester polyether resin can be adjusted, and the emulsification can be significantly improved; Examples 1 and 2 show that the finishing agents synthesized using two different functional monomers: 1,4-butanediol and 1,3-propylene glycol have outstanding performance on PBT and PTT fabrics, respectively, and have obvious advantages over conventional finishing agents.
[0106] By comparing Example 2 and Comparative Example 10, it can be seen that the selection of a solvent with relatively weak hydrogen bonding ability can significantly improve the emulsion stability problem of the synthetic resin during the water-based process, fundamentally reduce the emulsion viscosity, and improve the low-temperature storage stability of the emulsion.
[0107] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
Claims
1. A polyester polyether resin water-resistant moisture-absorbing quick-drying agent for polyester fiber and its blended fabrics, characterized in that: The resin is a block polyester polyether resin containing a predetermined repeating methylene segment. Its structure is as follows: Wherein, AO is a structural unit of polyethylene glycol, polypropylene glycol or polytetrahydrofuran; the ranges of x, y, z and m are: 8≤x≤135, 0≤y≤10, 1≤z≤10, 1≤m≤30; n is one or more of 3, 4, 5 and 6; R is H or NaSO3-; The polyester fiber and the blended fabrics thereof are PBT fiber and the blended fabrics thereof.
2. The polyester polyether resin water-resistant moisture-absorbing quick-drying agent for polyester fiber and its blended fabrics according to claim 1, characterized in that: The block polyester polyether resin contains a predetermined repeating methylene segment and has a melt viscosity of 3000-30000 mPa.s.
3. The application method of the polyester polyether resin water-resistant moisture-absorbing and quick-drying agent for polyester fiber and its blended fabrics according to claim 1, characterized in that: The water-washable moisture-absorbing and quick-drying agent is used for moisture-absorbing and quick-drying finishing processing on PBT fiber and its blended fabrics.
4. The application method of the polyester polyether resin water-resistant moisture-absorbing quick-drying agent for polyester fiber and its blended fabrics according to claim 3, characterized in that: The moisture absorption and quick-drying finishing includes dyeing in one bath, dipping, padding and spraying related functional finishing processes.