Double-layer mouth rehabilitation membrane material and preparation method thereof

By adopting a double-layer structure design in GBR membrane materials, combining polylactic acid microspheres and piezoelectric fiber layers, the problems of inabsorbability and insufficient mechanical properties of existing GBR membrane materials in bone regeneration are solved, and high-quality bones are achieved Regeneration and bone remodeling, reconstruction improves osteogenesis efficiency and reduces risk of gingival atrophy/membrane exposure.

CN119015516AActive Publication Date: 2024-11-26CHENGDU MEIYI BOYA MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411114769.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The existing GBR membrane materials have problems of inabsorbability and insufficient mechanical properties during bone regeneration, which leads to the need for secondary surgery and the advance growth of fibrous tissue that interferes with bone regeneration, and lacks hydrophilicity and piezoelectric activity, which limits its clinical application. .

Method used

Using the preparation method of a double-layer oral restoration membrane material, a protein membrane is formed by mixing polylactic acid microspheres containing bone-forming active materials with aqueous methacrylylated protein solution, and piezoelectric inorganic is formed on its surface by electrospinning technology. The fiber layer combines nano-scale bioactive materials and surface modifiers to enhance the hydrophilicity and piezoelectric properties of the material.

Benefits of technology

A double-layer oral restoration membrane material based on resorption and degradation is achieved, with good hydrophilicity, piezoelectric properties and softness, which promotes bone regeneration, reduces the risk of gingival atrophy/membrane exposure, and improves osteogenesis efficiency .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119015516A_ABST
    Figure CN119015516A_ABST
Patent Text Reader

Abstract

The invention discloses a double-layer oral repair membrane material and a preparation method thereof, and the preparation method comprises the following steps: 1) dispersing polylactic acid microspheres containing an osteogenic active material in a methylacryloylated protein aqueous solution to obtain a first mixture; spreading, ultrasonically vibrating and drying the first mixture to obtain a protein film; (2) putting the nanoscale osteogenesis active material powder and a nano piezoelectric inorganic substance into a surface modifier aqueous solution, and carrying out ultrasonic treatment to obtain surface-modified nano powder; mixing the surface modified nano powder, poly-L-lactic acid and a second solvent, and performing ultrasonic vibration to obtain an electrospinning solution; and 3) forming a layer of fibrous membrane on the protein membrane through electrostatic spinning by using the electrospinning solution, and then washing and freeze-drying to obtain the double-layer oral cavity restoration membrane material. The obtained double-layer oral cavity repairing film material has good hydrophilicity, piezoelectric property and softness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a double-layer oral repair membrane material and a preparation method thereof. Background Art

[0002] In the field of orthopedics and dentistry, treatment of bone defects caused by congenital malformations, trauma, tumors, inflammation, etc. usually requires the use of means to promote bone tissue healing, repair and regeneration. In the early 1980s, the concept of guided tissue regeneration (GTR) was first proposed internationally. Based on the inference of the GTR concept, tissue barrier membrane guided bone regeneration technology is defined as guided bone regeneration (GBR) technology. Its core is to establish and maintain a local closed space on the surface of the bone defect by applying tissue barrier membrane materials (also known as GBR membranes) to block the growth of fibrous connective tissue, thereby avoiding competitive inhibition between different cells, so that bone cells and bone tissue can fully mobilize their own healing ability, and complete high-quality bone regeneration and bone remodeling in a closed space without adverse external interference. Therefore, the GBR membrane is the key to the success of the GBR technology, and its own performance will directly affect the bone regeneration effect.

[0003] In the current clinical operation of oral restoration, this technology mainly uses natural bone powder or artificial bone powder as filling, supplemented by GBR membrane covering. GBR membrane materials are mainly divided into two types: absorbable and non-absorbable. Non-absorbable GBR membrane materials are mainly polytetrafluoroethylene (e-PTFE) and titanium metal, which have good mechanical strength and provide stable bone regeneration and repair space. However, due to its non-absorbability, it requires secondary surgery to remove after implantation, which will increase the patient's pain and surgical costs. Absorbable GBR membrane materials are represented by collagen membranes, which can be completely degraded and absorbed after implantation, so the damage caused by secondary surgery can be avoided. However, the mechanical properties of collagen membranes are weak and the degradation rate in the body is fast. The premature absorption of the membrane leads to the loss of its mechanical strength and the ability to support and maintain the bone forming space, which easily causes the fibrous tissue to grow in advance, thereby interfering with bone regeneration in the surgical area. Although the GBR membranes prepared by absorbable synthetic materials (including polylactic acid, polycaprolactone, polyglycolic acid, etc.) degrade more slowly, they are still limited in clinical use due to the presence of piezoelectric activity, membrane adhesion, and adhesion lower than collagen membranes.

[0004] CN107029293A discloses a pericardial collagen membrane for guiding bone regeneration and its preparation method and use. The pericardial membrane is cross-linked after being compounded with chitosan by a unique decellularization technology. The preparation method of the pericardial collagen membrane is: taking the pig pericardium to remove large pieces of fat, then defatting, alkali soaking, de-alkali, enzymolysis, compounding, cross-linking, and disinfection. The biocompatibility of the pericardium in this patent document is good, and the degradation time can be extended, but glutaraldehyde needs to be used as a cross-linking agent, and the introduction of chemical cross-linking agents has the risk of potential toxic side effects on the human body.

[0005] CN114732962A discloses a degradable antibacterial guided bone regeneration membrane and its preparation method and application. The preparation method comprises the following steps: (1) mixing hydroxyapatite, porogen and loaded Cu 2+ The ZIF-8 nanoparticles are added to the polyester solution and mixed evenly to obtain a casting solution; (2) the casting solution is formed by casting, immersed in deionized water, taken out and dried to obtain a degradable antibacterial guided bone regeneration membrane. The guided bone regeneration membrane obtained in this patent document focuses on antibacterial properties, and does not involve hydrophilicity and piezoelectric activity.

[0006] CN115814170A discloses a preparation method and application of a cross-scale bionic composite restoration that guides periodontal tissue regeneration, the preparation method comprising: firstly, a polymer solution and a nano-enhancement solution are blended to prepare a blended sol, and a composite film with a bionic structure is constructed by assembly; then a polyethylene glycol / polymer mixed layer is deposited on one side of the film, and a sufficient chemical modification is performed after drying; the polyethylene glycol is removed with hot water to obtain a rough surface, an inert polymer solution is sprayed on the rough surface, and a heterogeneous bionic structure material is obtained after mineralization treatment. The hydrophilicity of the restoration obtained in this patent document still needs to be improved, and it does not involve piezoelectric activity.

[0007] CN118267538A discloses an oral repair membrane and a preparation method thereof, the oral repair membrane comprising: a substrate, the substrate is formed by overlapping and winding fibers with a diameter of 10nm-100μm, and has a porous structure; and active particles, the active particles are loaded on the surface and / or inside of the substrate, and the active particles are derived from piezoelectric materials (polyhydroxyalkanoates) and / or hydrophilic polymer materials. Although the oral repair membrane of the patent document has a low softness, its hydrophilicity and piezoelectric activity still need to be further improved.

[0008] CN117919520A discloses a nanocomposite membrane for guiding bone tissue regeneration and its preparation method and application, the composite membrane comprises a polymer (one or more of polyvinyl alcohol, sodium alginate, chitosan and polylactic acid), a bioactive ceramic material (one or more of hydroxyapatite, β-tricalcium phosphate, bioactive glass and zirconium oxide toughened alumina ceramic) and a two-dimensional nanomaterial (one or more of MXene, graphene oxide, reduced graphene oxide and MoS2); hydrogen bonds are formed between the polymer, the bioactive ceramic material and the two-dimensional nanomaterial. The composite membrane of this patent document has good toughness, but its hydrophilicity still needs to be further improved, and piezoelectric activity is not involved. Summary of the invention

[0009] In view of this, one object of the present invention is to provide a method for preparing a double-layer oral repair membrane material, wherein the double-layer oral repair membrane material obtained by the preparation method has good hydrophilicity, piezoelectric properties, and good softness on the basis of being absorbable and degradable. Another object of the present invention is to provide a double-layer oral repair membrane material prepared by the preparation method as described above.

[0010] The present invention adopts the following technical solutions to achieve the above-mentioned purpose.

[0011] In one aspect, the present invention provides a method for preparing a double-layer oral repair membrane material, comprising the following steps:

[0012] 1) dispersing polylactic acid microspheres containing osteogenic active materials in a methacrylylated protein aqueous solution to obtain a first mixture; spreading the first mixture and performing ultrasonic vibration to obtain a polymerized protein film; and drying the polymerized protein film to obtain a protein film;

[0013] 2) placing nano-scale osteogenic active material powder and nano-piezoelectric inorganic substance in a surface modifier aqueous solution and subjecting it to ultrasonic treatment to obtain surface-modified nano-powder; mixing the surface-modified nano-powder, poly-L-lactic acid and a second solvent, subjecting them to ultrasonic vibration to obtain an electrospinning solution; wherein the nano-piezoelectric inorganic substance is selected from nano-barium titanate or nano-zinc oxide; and the surface modifier aqueous solution is selected from one of a polyethylene glycol aqueous solution, a polyglycolic acid aqueous solution and a sodium citrate aqueous solution;

[0014] 3) electrospinning the electrospinning solution to form a fiber membrane on the protein membrane, followed by washing and freeze-drying to obtain a double-layer oral repair membrane material;

[0015] There is no particular order between step 1) and step 2).

[0016] According to the preparation method of the present invention, preferably, in step 1), nano-scale osteogenic active material powder, polylactic acid and a pore-forming agent are mixed and heated to form a melt; the melt is sprayed into a first solvent to form microspheres, thereby obtaining polylactic acid microspheres containing osteogenic active material;

[0017] Wherein, the nano-scale osteogenic active material powder is selected from one or more of nano-scale bioactive glass, nano-scale hydroxyapatite and nano-scale β-tricalcium phosphate;

[0018] Wherein, the polylactic acid is selected from one or more of poly-L-lactic acid and poly-D-lactic acid, and must contain poly-L-lactic acid;

[0019] Wherein, the pore-forming agent is selected from one or more of polyethylene glycol, polyglycolic acid, tributyl citrate and polyhydroxybutyric acid;

[0020] The mass ratio of nano-scale osteogenic active material powder, polylactic acid and pore-forming agent is 5-15:80-120:5-25.

[0021] According to the preparation method of the present invention, preferably:

[0022] The first solvent is selected from one or more of water, ethanol and dimethyl sulfoxide;

[0023] The polylactic acid is a mixture of poly (dextrorotatory) lactic acid and poly (l-lactic acid); the mass ratio of the nano-scale osteogenic active material powder, poly (dextrorotatory) lactic acid, poly (l-lactic acid) and pore-forming agent is 5-15:40-60:40-60:5-25.

[0024] According to the preparation method of the present invention, preferably, the methacrylylated protein aqueous solution is a solution obtained by mixing methacrylylated protein and water in a mass ratio of 1:3 to 1:10; wherein the methacrylylated protein is selected from one of methacrylylated type I collagen, methacrylylated type II collagen, methacrylylated silk fibroin, methacrylylated recombinant collagen and methacrylylated gelatin.

[0025] According to the preparation method of the present invention, preferably, in the first mixture, the concentration of the polylactic acid microspheres containing the osteogenic active material is 1-10 wt %.

[0026] According to the preparation method of the present invention, preferably, in step 2), the nano-scale osteogenic active material powder and the nano-piezoelectric inorganic substance are placed in an aqueous solution of a surface modifier for ultrasonic treatment, solid-liquid separation, and drying to obtain a surface-modified nano-powder; wherein the nano-scale osteogenic active material powder is selected from one or more of nano-scale bioactive glass, nano-scale hydroxyapatite and nano-scale β-tricalcium phosphate; the mass ratio of the nano-scale osteogenic active material powder to the nano-piezoelectric inorganic substance is 1 to 1.05:1.

[0027] According to the preparation method of the present invention, preferably, in step 2), the mass volume concentration of the surface modifier aqueous solution is 2-8% (w / v); the mass ratio of the surface modified nanopowder to poly-L-lactic acid is 1:10-1:100.

[0028] According to the preparation method of the present invention, preferably, the second solvent is selected from one of hexafluoroisopropanol, N,N-dimethylformamide, trifluoroethanol, tetrahydrofuran and dichloromethane.

[0029] According to the preparation method of the present invention, preferably, the electrospinning parameters include: the rate of the microinjection pump is 5-10 mL / h, the high voltage is 18-30 kV, and the distance between the receiver and the injection pump needle is 20-25 cm.

[0030] On the other hand, the present invention further provides a double-layer oral repair membrane material, which is prepared according to the preparation method described above.

[0031] The double-layer oral repair membrane material prepared by the present invention has good hydrophilicity, piezoelectric properties and softness on the basis of being absorbable and degradable; among them, good hydrophilicity is conducive to soft tissue adhesion and reduces the risk of gingival atrophy / membrane exposure; good piezoelectric properties are conducive to promoting osteogenesis, achieving high-quality bone regeneration and bone remodeling and reconstruction, and improving osteogenesis efficiency; good softness is conducive to the attachment of the entire membrane. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is the SEM image of the first layer of the protein film in Example 1.

[0033] Figure 2 This is the SEM image of the fiber membrane of the second layer of Example 1. DETAILED DESCRIPTION

[0034] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0035] The method for preparing a double-layer oral repair membrane material of the present invention comprises the following steps: 1) preparing a protein membrane; 2) preparing an electrospinning solution; 3) forming a double-layer oral repair membrane material. There is no particular order between step 1) and step 2), and the two can be performed simultaneously. A detailed description is given below.

[0036] <Steps for preparing protein film>

[0037] In the present invention, polylactic acid microspheres containing osteogenic active materials are dispersed in a methacryloyl protein aqueous solution to obtain a first mixture; the first mixture is spread and subjected to ultrasonic vibration to obtain a polymerized protein film; the polymerized protein film is dried to obtain a protein film. This is conducive to improving the hydrophilicity and piezoelectric properties of the obtained double-layer oral repair membrane material, and it can be absorbed and degraded, and the degradation time is longer than that of a simple collagen membrane.

[0038] In the present invention, the polylactic acid microspheres containing osteogenic active materials are prepared by the following steps: mixing nano-scale osteogenic active material powder, polylactic acid and a pore-forming agent, and heating to form a melt; spraying the melt into a first solvent to form microspheres, thereby obtaining polylactic acid microspheres containing osteogenic active materials. This is conducive to forming uniform microspheres.

[0039] In this step, the mass ratio of nano-scale osteogenic active material powder, polylactic acid and pore-forming agent is 5-15:80-120:5-25, preferably 5-12:80-110:8-20, more preferably 5-10:80-100:10-15. This is conducive to taking into account both hydrophilicity and piezoelectric properties.

[0040] In this step, the nano-scale osteogenic active material powder is selected from one or more of nano-scale bioactive glass, nano-scale hydroxyapatite and nano-scale β-tricalcium phosphate, preferably nano-scale bioactive glass. The particle size range is 20 to 150 nm. Bioactive glass is a silicate material, and its main components include SiO2, Na2O, CaO, and P2O5. The source of bioactive glass is not particularly limited and can be purchased commercially.

[0041] In this step, the polylactic acid is selected from one or more of poly-L-lactic acid (PLLA) and poly-D-lactic acid (PDLA), and must contain poly-L-lactic acid. In some specific embodiments, polylactic acid is a mixture of poly-D-lactic acid and poly-L-lactic acid, and the mass ratio of poly-D-lactic acid and poly-L-lactic acid can be 40-60:40-60, preferably 40-55:40-55, more preferably 40-50:40-50, and the amount of poly-L-lactic acid is greater than or equal to the amount of poly-D-lactic acid. The molecular weight of polylactic acid is 5w-20w g / mol (can be recorded as 5w-20wDa). The optical purity of poly-D-lactic acid and poly-L-lactic acid can be greater than 95%.

[0042] According to one embodiment of the present invention, the mass ratio of the nano-scale osteogenic active material powder, poly (D-lactic acid), poly (L-lactic acid) and pore-forming agent may be 5-15:40-60:40-60:5-25.

[0043] In the present invention, the pore-forming agent can be selected from one or more of polyethylene glycol, polyglycolic acid, tributyl citrate and polyhydroxybutyric acid, preferably polyethylene glycol, and the molecular weight of polyethylene glycol is greater than or equal to 800 and less than or equal to 4000. For example, it can be polyethylene glycol 800 (denoted as PEG 800 ), polyethylene glycol 1000 (denoted as PEG 1000 ). The first solvent is selected from one or more of water, ethanol and dimethyl sulfoxide, preferably water.

[0044] According to one embodiment of the present invention, nano-scale osteogenic active material powder, polylactic acid and a pore-forming agent are mixed, and then heated and blended at 190-220° C. for 10-20 minutes in a torque rheometer to form a melt; the melt is sprayed into a first solvent through a microfluidic extrusion device to form microspheres, and stirring is continued for 30 minutes to 1 hour, followed by washing with 35-45° C. water for multiple times to remove residual pore-forming agent, and vacuum drying is performed after washing to obtain polylactic acid microspheres containing osteogenic active material.

[0045] In the present invention, the aperture of the nozzle used in the microfluidic extrusion device is 20 to 50 μm.

[0046] In the present invention, the methacrylylated protein aqueous solution is a solution obtained by mixing methacrylylated protein and water in a mass ratio of 1:3 to 1:10. The mixture may be stirred until completely dissolved. The mass ratio of methacrylylated protein to water is preferably 1:6 to 1:10, and more preferably 1:8 to 1:9.

[0047] The methacrylylated protein is selected from the group consisting of methacrylylated type I collagen, methacrylylated type II collagen, methacrylylated silk fibroin, methacrylylated recombinant collagen and methacrylylated gelatin, preferably methacrylylated gelatin.

[0048] In the first mixture of the present invention, the concentration of the polylactic acid microspheres containing the osteogenic active material is 1 to 10 wt %, preferably 3 to 9 wt %, and more preferably 5 to 8 wt %.

[0049] In the present invention, the first mixture can be spread on a mold by solution casting, then left to stand for 15 to 30 minutes, and then subjected to ultrasonic vibration in an ultrasonic oscillator to obtain a polymerized protein film. The frequency of the ultrasonic vibration is 50 to 300 kHz, preferably 150 to 300 kHz, and more preferably 240 to 300 kHz. In this way, the porous surface of the microspheres can be used to react with water and air under the action of ultrasonic vibration to generate a large number of free radicals, thereby catalyzing free radical polymerization of carbon-carbon double bonds on the side chains of methacrylylated proteins.

[0050] In the present invention, the polymerized protein film is placed in a vacuum oven and dried at 45 to 55° C. for 2 to 4 hours to obtain the protein film. The thickness of the protein film can be 200 to 500 μm.

[0051] <Steps for preparing electrospinning solution>

[0052] In the present invention, nano-scale osteogenic active material powder and nano-piezoelectric inorganic material are placed in a surface modifier aqueous solution and ultrasonically treated to obtain surface-modified nano-powder; the surface-modified nano-powder, poly-L-lactic acid and a second solvent are mixed and ultrasonically vibrated to obtain an electrospinning solution. This is conducive to obtaining a double-layer oral repair membrane material with good softness and good piezoelectric properties.

[0053] In the present invention, the nano-piezoelectric inorganic material is selected from nano-barium titanate or nano-zinc oxide, preferably nano-barium titanate. The particle size of the nano-piezoelectric inorganic material is 50-150 nm.

[0054] In the present invention, the surface modifier aqueous solution is selected from one of polyethylene glycol aqueous solution, polyglycolic acid aqueous solution and sodium citrate aqueous solution, preferably polyethylene glycol aqueous solution. The molecular weight of polyethylene glycol in the polyethylene glycol aqueous solution is 1000 to 4000. For example, it can be polyethylene glycol 2000 (denoted as PEG 2000 The mass volume concentration of the surface modifier aqueous solution is 2 to 8% (w / v), preferably 3 to 8% (w / v), and more preferably 4 to 8% (w / v).

[0055] In this step, the nano-scale osteogenic active material powder is selected from one or more of nano-scale bioactive glass, nano-scale hydroxyapatite and nano-scale β-tricalcium phosphate, preferably nano-scale bioactive glass. The particle size range is 20 to 150 nm. Bioactive glass is a silicate material, and its main components include SiO2, Na2O, CaO, and P2O5. The source of bioactive glass is not particularly limited and can be purchased commercially. The mass ratio of the nano-scale osteogenic active material powder to the nano-piezoelectric inorganic substance is 1 to 1.05:1.

[0056] According to one embodiment of the present invention, nano-scale osteogenic active material powder and nano-piezoelectric inorganic material are placed in a surface modifier aqueous solution for ultrasonic treatment, solid-liquid separation, and drying to obtain surface-modified nano-powder. The ratio of the sum of the mass of the nano-scale osteogenic active material powder and the nano-piezoelectric inorganic material to the volume of the surface modifier aqueous solution can be 1g:8-12mL, preferably 1g:9-12mL, for example, 1g:10mL. In the present invention, the frequency of ultrasonic treatment can be 30-80kHz, preferably 45-80kHz, and more preferably 60-80kHz. The temperature during ultrasonic treatment can be 60-85°C, preferably 65-85°C, and more preferably 75-80°C. The time of ultrasonic treatment can be 10-40min, preferably 15-40min, and more preferably 20-30min. After ultrasonic treatment, solid-liquid separation is performed, and solid-liquid separation can be filtration. After solid-liquid separation, the solid is dried, and the drying temperature can be 55-85°C.

[0057] In some embodiments, the surface-modified nanopowder and poly-L-lactic acid are mixed, the mixture is added to the second solvent, ultrasonically vibrated for 1 to 3 hours, and then stirred in a closed container for 4 to 8 hours to obtain an electrospinning solution. The frequency of the ultrasonic vibration can be 30 to 80 kHz, preferably 45 to 80 kHz, and more preferably 60 to 80 kHz.

[0058] In the present invention, the mass ratio of the surface modified nano powder to the poly-L-lactic acid is 1:10 to 1:100, preferably 1:10 to 1:50, and more preferably 1:10 to 1:25. The concentration of the poly-L-lactic acid in the electrospinning solution is 5 to 20 wt%, preferably 5 to 15 wt%, and more preferably 5 to 10 wt%. In this step, the molecular weight of the poly-L-lactic acid can be 5w to 10w g / mol.

[0059] In the present invention, the second solvent is selected from one of hexafluoroisopropanol, N,N-dimethylformamide, trifluoroethanol, tetrahydrofuran and dichloromethane, preferably hexafluoroisopropanol.

[0060] <Steps for forming a double-layer oral restoration film material>

[0061] The electrospinning solution is electrospun to form a fiber membrane on the protein membrane, which is then washed and freeze-dried to obtain a double-layer oral repair membrane material. This is conducive to obtaining a repair membrane with a thickness within a specific range and is conducive to improving the hydrophilicity and piezoelectric properties of the obtained repair membrane material.

[0062] The electrospinning parameters include: the rate of the microinjection pump is 5-10 mL / h, the high voltage is 18-30 kV, and the distance between the receiver and the syringe pump needle is 20-25 cm. The receiver can be a plate-type receiver.

[0063] In certain specific embodiments, the protein film can be fixed on a plate-type receiver, and the electrospinning solution can be electrospun on the protein film to form a fiber film. After electrospinning, washing can be performed by multiple washings with injection water to remove the residual second solvent, and then vacuum freeze drying at below -30°C for 20 to 36 hours.

[0064] The present invention also provides a double-layer oral repair membrane material, which is prepared according to the preparation method as described above. The thickness of the double-layer oral repair membrane material is 400 μm to 1 mm, preferably 500 to 900 μm, and more preferably 500 to 890 μm.

[0065] The first layer of the double-layer oral repair membrane material of the present invention is a cross-linked protein membrane containing polylactic acid / osteoblastic active material composite microspheres, which contacts the gums when used. The protein membrane has good hydrophilicity, which is conducive to the adhesion and growth of tissue cells, and reduces the risk of gum atrophy or membrane exposure; the second layer of the membrane is an irregular polylactic acid fiber layer containing piezoelectric / osteoblastic active material powder, which contacts the bone defect site filled with bone powder when used, has a good piezoelectric effect, and is conducive to promoting osteogenesis. In addition, the double-layer oral repair membrane material of the present invention has good softness and good overall adhesion.

[0066] The test methods used in the following examples are described as follows:

[0067] SEM test: ZEISS GeminiSEM 300 was used for testing.

[0068] The raw materials used in the following examples are described as follows:

[0069] Methacrylated gelatin, nano-scale bioactive glass powder, poly-L-lactic acid (PLLA), and poly-D-lactic acid (PDLA) were from Chengdu Meiyi Boya Material Technology Co., Ltd. Nano-barium titanate was purchased from Nanjing Hongde Nanomaterials Co., Ltd.

[0070] Preparation Example 1

[0071] Nano-scale bioactive glass powder, PDLA, PLLA and PEG 1000 The materials were weighed according to a mass ratio of 10:40:40:10, and then added to the rheometer, heated to 200°C and blended for 20 minutes to obtain a uniform melt, wherein the particle size of the nanoscale bioactive glass powder was 20 nm, and the molecular weights of PDLA and PLLA were both 10 wDa. The melt was sprayed into purified water (the first solvent) through a microfluidic extruder with a diameter of 10 μm, stirred for 1 hour, and then repeatedly rinsed with purified water for 5 times to remove residual PEG. 1000 , and then vacuum dried at 50°C for 8 hours to obtain polylactic acid microspheres containing osteogenic active materials.

[0072] Example 1

[0073] 1) Disperse the polylactic acid microspheres containing osteogenic active materials obtained in Preparation Example 1 in a methacryloyl protein aqueous solution (an aqueous solution formed by mixing methacryloyl gelatin and water in a ratio of 1:8 and stirring at 37°C to completely dissolve them), the concentration of the polylactic acid microspheres being 8wt%, and magnetically stirring at room temperature for 15 minutes until the microspheres are dispersed to obtain a first mixture; spread the first mixture on a mold using a solution casting method, let it stand at room temperature for 20 minutes, and then ultrasonically vibrate it in an ultrasonic oscillator for 15 minutes at a vibration frequency of 240kHz to obtain a polymerized protein film; place the polymerized protein film in a vacuum drying oven and dry it at 50°C for 3 hours to obtain a protein film, which is the first layer of protein film. Its thickness is 450μm. The SEM results of the first layer of protein film are shown in Figure 1 .

[0074] 2) Mix the nano-scale bioactive glass powder and nano-barium titanate in a mass ratio of 1:1 and place them in a polyethylene glycol aqueous solution (8% (w / v), PEG 2000 ), ultrasonically treated at 80°C for 30 minutes, filtered, washed with purified water, and dried to obtain surface-modified nanopowder. The surface-modified nanopowder was mixed with PLLA at a mass ratio of 1:25, then added to hexafluoroisopropanol (the second solvent) and mixed, ultrasonically vibrated for 1 hour, and then stirred for 6 hours in a closed container at room temperature to form an electrospinning solution with a PLLA concentration of 10wt%; wherein the particle size of nano-barium titanate is 50nm, the particle size of nano-scale bioactive glass powder is 20nm, the molecular weight of PLLA is 7wDa, and the optical purity is greater than 95%. wherein the ratio of the sum of the mass of nano-scale bioactive glass powder and nano-barium titanate to the volume of polyethylene glycol aqueous solution is 1g:10mL.

[0075] 3) The protein film was fixed on a plate-type receiver, and the electrospinning solution was electrospinned to form a fiber membrane on the protein film, and then washed with injection water for 3 times to remove the residual solvent, and freeze-dried at -30°C for 24 hours to obtain a double-layer oral repair membrane material. The thickness was 890μm. The parameters of electrospinning were as follows: the rate of the microinjection pump was 8mL / h, the high voltage was 25kV, and the distance between the receiver and the injection pump needle was 23cm. The SEM results of the second layer of fiber membrane are shown in Figure 2 .

[0076] Preparation Example 2

[0077] Nano-scale bioactive glass powder, PDLA, PLLA and PEG 1000The materials were weighed according to a mass ratio of 5:40:40:15, and then added to the rheometer, heated to 210°C and blended for 15 minutes to obtain a uniform melt, wherein the particle size of the nanoscale bioactive glass powder was 20 nm, and the molecular weights of PDLA and PLLA were both 10 wDa. The melt was sprayed into purified water (the first solvent) through a microfluidic extruder with a diameter of 10 μm, stirred for 1 hour, and then repeatedly rinsed with purified water for 5 times to remove residual PEG. 1000 , and then vacuum dried at 50°C for 8 hours to obtain polylactic acid microspheres containing osteogenic active materials.

[0078] Example 2

[0079] 1) The polylactic acid microspheres containing osteogenic active materials prepared in Preparation Example 2 are dispersed in a methacrylated protein aqueous solution (an aqueous solution formed by mixing methacrylated gelatin and water in a ratio of 1:9 and stirring at 37°C to completely dissolve the mixture), the concentration of the polylactic acid microspheres is 5wt%, and the mixture is magnetically stirred at room temperature for 15 minutes until the microspheres are dispersed to obtain a first mixture; the first mixture is spread on a mold by a solution casting method, allowed to stand at room temperature for 20 minutes, and then ultrasonically vibrated in an ultrasonic oscillator for 15 minutes at a vibration frequency of 240kHz to obtain a polymerized protein film; the polymerized protein film is placed in a vacuum drying oven and dried at 50°C for 3 hours to obtain a protein film. Its thickness is 330μm.

[0080] 2) Mix the nano-scale bioactive glass powder and nano-barium titanate in a mass ratio of 1:1 and place them in a polyethylene glycol aqueous solution (8% (w / v), PEG 2000 ), ultrasonically treated at 80°C for 40 minutes, filtered, washed with purified water, and dried to obtain surface-modified nanopowder. The surface-modified nanopowder was mixed with PLLA at a mass ratio of 1:10, then added to hexafluoroisopropanol (the second solvent) for mixing, ultrasonically vibrated for 1 hour, and then stirred for 6 hours in a closed container at room temperature to form an electrospinning solution with a PLLA concentration of 5wt%; wherein the particle size of nano-barium titanate is 50nm, the particle size of nano-scale bioactive glass powder is 20nm, the molecular weight of PLLA is 7wDa, and the optical purity is greater than 95%. wherein the ratio of the sum of the mass of nano-scale bioactive glass powder and nano-barium titanate to the volume of polyethylene glycol aqueous solution is 1g:10mL.

[0081] 3) The protein film was fixed on a plate-type receiver, and the electrospinning solution was electrospinned to form a fiber film on the protein film, and then washed with injection water for 3 times to remove the residual solvent, and freeze-dried at -30°C for 24 hours to obtain a double-layer oral repair membrane material. The thickness was 820 μm. The parameters of electrospinning were: the rate of the microinjection pump was 8 mL / h, the high voltage was 25 kV, and the distance between the receiver and the injection pump needle was 23 cm.

[0082] Example 3

[0083] The procedure of Example 1 was followed. The thickness of the obtained protein film was 210 μm.

[0084] The thickness of the obtained double-layer oral restoration membrane material is 830 μm.

[0085] Example 4

[0086] The procedure of Example 1 was followed. The thickness of the obtained protein film was 210 μm.

[0087] The thickness of the obtained double-layer oral repair membrane material is 500 μm.

[0088] Comparative Example 1

[0089] The only difference from Example 1 is that step 2) is different. In this comparative example, nano-barium titanate and nano-scale bioactive glass powder are not added, and PLLA is used to form an electrospinning solution. The thickness of the obtained double-layer membrane is 860 μm.

[0090] Comparative Example 2

[0091] The only difference from Example 1 is that step 1) is not included. In this comparative example, only a fiber membrane is formed, and no protein membrane is involved.

[0092] Experimental example

[0093] 1. Dielectric constant test

[0094] The present invention uses a quasi-static d33 tester to directly measure the piezoelectric constants of the membrane materials of Examples 1 to 4 and the comparative example, and the membrane materials are not polarized. Five points are taken for each sample to measure and the average is taken. The results are shown in Table 1.

[0095] Table 1

[0096] Serial number Piezoelectric constant d33 (pC / N) Example 1 2.25±0.31 Example 2 2.17±0.26 Example 3 2.23±0.18 Example 4 2.18±0.23 Comparative Example 1 0.91±0.05 Comparative Example 2 1.31±0.07 Pure PLLA electrospun membrane 0.75±0.09

[0097] As shown in Table 1, the piezoelectric constant of the double-layer repair membrane material obtained by the present invention is relatively high without polarization, reaching above 2.1 pC / N, which is significantly improved, which is beneficial to promote osteogenesis and improve osteogenesis efficiency.

[0098] 2. Hydrophilicity test

[0099] The present invention uses a contact angle tester to measure the surface contact angles of the double-layer repair membranes (protein membranes on the gum side) obtained in Examples 1 to 4 and the pure PLLA electrospun membrane prepared by the electrospinning process at room temperature. Three samples are tested in each group of samples, and three positions are tested for each sample. The average value is calculated. The test results are shown in Table 2 below.

[0100] Table 2

[0101] Serial number Contact Angle Example 1 43.18°±2.95° Example 2 45.26°±2.78° Example 3 43.95°±2.57° Example 4 44.09°±2.36° Pure PLLA electrospun membrane 91.53°±3.71°

[0102] It can be seen from Table 2 that the protein film on the gingival side of the double-layer repair membrane material of the present invention has good hydrophilicity and shows good adhesion effect on the surface of endothelial cells. Therefore, the inventors believe that the repair membrane prepared by the present invention is conducive to endothelial cell adhesion, thereby reducing the risk of gingival atrophy / membrane exposure.

[0103] 3. Softness test

[0104] The present invention measured the softness of Examples 1 to 4 according to the method of GB / T 8942-2002. The softness value is the sum of the bending resistance of the film material and the maximum vector of the friction force at the gap, expressed in millinewton (mN). The smaller the softness value, the softer the film material, and the better the corresponding adhesion. When the softness of the film material is less than 1000mN, it has good adhesion. The results are shown in Table 3.

[0105] Table 3

[0106] Serial number Softness(mN) Example 1 753 Example 2 740 Example 3 894 Example 4 761

[0107] As shown in Table 3, the double-layer repair membrane materials of the present invention have good softness. However, when the fiber membrane of the second layer accounts for a higher proportion, its softness becomes worse, which may be because the fiber membrane of the second layer has a higher proportion of polylactic acid, which has a certain brittleness and affects the softness of the finished product.

[0108] In addition, the average pore size of the fiber membrane of comparative example 2 was measured to be 1.2 μm, and the porosity was 93%. The present invention controls the electrospinning parameters to obtain a fiber membrane with irregular pores and a sufficiently small average pore size (1.2 μm) to achieve a better physical barrier effect and maintain the stability of the osteogenic space.

[0109] In summary, the piezoelectric constant of the double-layer oral repair membrane material prepared by the present invention can be improved without polarization; in addition, it has good hydrophilicity and low softness. The double-layer oral repair membrane material prepared by the present invention has good piezoelectric properties, which is beneficial to promote osteogenesis and achieve high-quality bone regeneration and bone remodeling and reconstruction; it has good hydrophilicity and good softness, which is beneficial to soft tissue adhesion, reduces the risk of gingival atrophy / membrane exposure, and is beneficial to the attachment of the overall membrane.

[0110] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.

Claims

1. A method for preparing a double-layer oral repair membrane material, characterized in that: The steps include: 1) dispersing polylactic acid microspheres containing osteogenic active materials in a methacrylylated protein aqueous solution to obtain a first mixture; spreading the first mixture, ultrasonically vibrating, to obtain a polymerized protein film; and drying the polymerized protein film to obtain a protein film; 2) placing nano-scale osteogenic active material powder and nano-piezoelectric inorganic substance in a surface modifier aqueous solution and subjecting it to ultrasonic treatment to obtain surface-modified nano-powder; mixing the surface-modified nano-powder, poly-L-lactic acid and a second solvent, subjecting them to ultrasonic vibration to obtain an electrospinning solution; wherein the nano-piezoelectric inorganic substance is selected from nano-barium titanate or nano-zinc oxide; and the surface modifier aqueous solution is selected from one of a polyethylene glycol aqueous solution, a polyglycolic acid aqueous solution and a sodium citrate aqueous solution; 3) electrospinning the electrospinning solution to form a fiber membrane on the protein membrane, followed by washing and freeze-drying to obtain a double-layer oral repair membrane material; There is no particular order between step 1) and step 2).

2. The preparation method according to claim 1, characterized in that: In step 1), nano-scale osteogenic active material powder, polylactic acid and a pore-forming agent are mixed and heated to form a melt; the melt is sprayed into a first solvent to form microspheres, thereby obtaining polylactic acid microspheres containing osteogenic active material; Wherein, the nano-scale osteogenic active material powder is selected from one or more of nano-scale bioactive glass, nano-scale hydroxyapatite and nano-scale β-tricalcium phosphate; Wherein, the polylactic acid is selected from one or more of poly-L-lactic acid and poly-D-lactic acid, and must contain poly-L-lactic acid; Wherein, the pore-forming agent is selected from one or more of polyethylene glycol, polyglycolic acid, tributyl citrate and polyhydroxybutyric acid; The mass ratio of nano-scale osteogenic active material powder, polylactic acid and pore-forming agent is 5-15:80-120:5-25.

3. The preparation method according to claim 2, characterized in that: The first solvent is selected from one or more of water, ethanol and dimethyl sulfoxide; The polylactic acid is a mixture of poly (dextrorotatory) lactic acid and poly (l-lactic acid); the mass ratio of the nano-scale osteogenic active material powder, poly (dextrorotatory) lactic acid, poly (l-lactic acid) and pore-forming agent is 5-15:40-60:40-60:5-25.

4. The preparation method according to claim 1, characterized in that: The methacrylylated protein aqueous solution is a solution obtained by mixing methacrylylated protein and water in a mass ratio of 1:3 to 1:10; wherein the methacrylylated protein is selected from one of methacrylylated type I collagen, methacrylylated type II collagen, methacrylylated silk fibroin, methacrylylated recombinant collagen and methacrylylated gelatin.

5. The preparation method according to claim 1, characterized in that: In the first mixture, the concentration of the polylactic acid microspheres containing the osteogenic active material is 1-10 wt %.

6. The preparation method according to claim 1, characterized in that: In step 2), the nano-scale osteogenic active material powder and the nano-piezoelectric inorganic substance are placed in an aqueous solution of a surface modifier for ultrasonic treatment, solid-liquid separation, and drying to obtain a surface-modified nano-powder; wherein the nano-scale osteogenic active material powder is selected from one or more of nano-scale bioactive glass, nano-scale hydroxyapatite and nano-scale β-tricalcium phosphate; the mass ratio of the nano-scale osteogenic active material powder to the nano-piezoelectric inorganic substance is 1 to 1.05:

1.

7. The preparation method according to claim 6, characterized in that: In step 2), the mass volume concentration of the surface modifier aqueous solution is 2 to 8% (w / v); the mass ratio of the surface modified nanopowder to the poly-L-lactic acid is 1:10 to 1:

100.

8. The preparation method according to claim 1, characterized in that: The second solvent is selected from one of hexafluoroisopropanol, N,N-dimethylformamide, trifluoroethanol, tetrahydrofuran and dichloromethane.

9. The preparation method according to claim 1, characterized in that: The parameters of the electrospinning include: the rate of the microinjection pump is 5-10 mL / h, the high voltage is 18-30 kV, and the distance between the receiver and the injection pump needle is 20-25 cm.

10. A double-layer oral repair membrane material, characterized in that: It is prepared according to the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Guided bone regeneration pericardial collagen membrane as well as preparation method and application thereof

    CN107029293A

  • Degradable antibacterial guided bone regeneration membrane as well as preparation method and application thereof

    CN114732962A

  • Preparation method and application of cross-scale bionic composite restoration for guiding periodontal tissue regeneration

    CN115814170A

  • Nano-composite membrane for guiding bone tissue regeneration as well as preparation method and application of nano-composite membrane

    CN117919520A

  • Oral cavity repairing film and preparation method thereof

    CN118267538A

Cited By

  • Bacteriostatic oral rehabilitation composite film and preparation method thereof

    CN120094000A

  • Antibacterial oral repair composite film and preparation method thereof

    CN120094000B

  • Oral cavity repairing film as well as preparation method and application thereof

    CN120586161A