Preparation method and manufacturing device of short carbon fibers

By removing the glue and reapplying the thermoplastic coating, the problem of chopped carbon fibers not tolerate high temperature and poor bonding properties is solved. Chopped carbon fibers that are resistant to high temperature and are well combined with the thermoplastic matrix material are prepared, which improves its in composite materials. performance and application potential.

CN118979389AActive Publication Date: 2024-11-19ZHONGFU SHENYING CARBON FIBER
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411049003.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

In the existing chopped carbon fiber preparation process, the thermoset coating on the surface of the carbon fiber bundle is not resistant to high temperatures and is difficult to firmly combine with the thermoplastic matrix material, which limits its application range.

Method used

By degluing the carbon fiber bundle, the included epoxy resin-based thermosetting coating is removed, and the thermoplastic resin coating is reapplied to the surface, so the chopped carbon fibers produced can withstand high temperatures and are firmly combined with the thermoplastic matrix material.

Benefits of technology

The high temperature stability of chopped carbon fibers and good combination with thermoplastic matrix materials have been achieved, improving its performance and application potential in composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979389A_ABST
    Figure CN118979389A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and a manufacturing device of short carbon fibers, and belongs to the technical field of short carbon fiber manufacturing. The preparation method of the short carbon fiber comprises the following steps: providing a continuous finished carbon fiber bundle, wherein the surface of the carbon fiber bundle is a thermosetting coating; sequentially carrying out twisting treatment, degumming treatment, sizing treatment, pre-drying treatment, slitting treatment and drying treatment on the carbon fiber bundles to obtain short carbon fibers; wherein in the step of sizing treatment, a sizing agent is thermoplastic resin, and the chopped carbon fiber prepared by the method can resist high temperature and can be firmly combined with a thermoplastic matrix material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of chopped carbon fiber manufacturing, and in particular to a preparation method and a manufacturing device for chopped carbon fiber. Background Art

[0002] Carbon fiber reinforced thermoplastic composites (CFRTP for short) have the advantages of good toughness, fatigue resistance, high temperature resistance, short molding cycle and easy recycling and reuse. They are widely used in aerospace, military industry, automobiles, sporting goods and other fields. From the perspective of reinforcement, CFRTP is divided into long-cut carbon fiber reinforced thermoplastic composites, short-cut carbon fiber reinforced thermoplastic composites and continuous carbon fiber reinforced composites. Among them, short-cut carbon fiber is made by bundling carbon fiber filaments with high strength and high modulus and then cutting them according to the specified length. Compared with carbon fiber filaments, it has the advantage of more uniform distribution in the matrix material. At the same time, short-cut carbon fiber also has the advantages of higher mechanical strength and lower density. However, the short-cut carbon fiber prepared by the existing preparation process has the problem of not being resistant to high temperature and difficult to firmly combine with the thermoplastic matrix material, which affects the application and promotion of short-cut carbon fiber. Summary of the invention

[0003] The purpose of the present application is to provide a method and a manufacturing device for chopped carbon fibers, wherein the chopped carbon fibers prepared are resistant to high temperatures and can be firmly combined with a thermoplastic matrix material.

[0004] The embodiment of the present application is implemented as follows:

[0005] In a first aspect, an embodiment of the present application provides a method for preparing chopped carbon fibers, comprising the following steps: providing a continuous finished carbon fiber bundle, the surface of the carbon fiber bundle being a thermosetting coating; sequentially performing twisting treatment, degumming treatment, sizing treatment, pre-drying treatment, slitting treatment and drying treatment on the carbon fiber bundle to obtain chopped carbon fibers; wherein, in the sizing treatment step, the sizing agent is a thermoplastic resin.

[0006] At present, the surface of commercially available carbon fiber bundles is usually a thermosetting coating (i.e., cured after coating with an epoxy resin sizing agent), and chopped carbon fibers are cut from corresponding commercially available carbon fiber bundles. On the one hand, since the coating formed by the epoxy resin sizing agent is not resistant to high temperatures, the corresponding chopped carbon fibers are difficult to meet the high-temperature processing requirements; on the other hand, although the coating formed by the epoxy resin sizing agent can be stably combined with the epoxy resin matrix, it is difficult to stably combine with the thermoplastic resin matrix. In this application, the researchers first de-glue the carbon fiber bundle after the twisting treatment to remove the epoxy resin thermosetting coating on the surface of the carbon fiber material, and then re-apply the thermoplastic coating on the surface of the carbon fiber material through the sizing treatment. The chopped carbon fibers prepared by this preparation method are resistant to high temperatures and can be firmly combined with the thermoplastic matrix material.

[0007] In some optional embodiments, the degumming step includes: soaking the twisted carbon fiber bundle in a degumming agent, the degumming agent includes acetone; or, placing the twisted carbon fiber bundle in a pyrolysis furnace for heat treatment, the heat treatment temperature is 250-450°C.

[0008] In the above technical scheme, the epoxy resin thermosetting coating on the surface of the carbon fiber material can be effectively removed by immersing the carbon fiber bundle in a degumming agent or heat-treating it in a pyrolysis furnace. Among them, limiting the composition of the degumming agent and limiting the temperature of the heat treatment are both helpful to improve the degumming effect.

[0009] In some alternative embodiments, the debonding agent includes acetone and methylene chloride.

[0010] Optionally, the volume ratio of acetone to dichloromethane is (2-4):1.

[0011] In the above technical solution, a mixed system of acetone and dichloromethane is used as a degumming agent, which can achieve a better degumming effect.

[0012] Furthermore, limiting the volume ratio of acetone to dichloromethane within a specific range is more helpful to improve the debonding effect of the debonding agent.

[0013] In some optional embodiments, the temperature of the heat treatment is 300-400°C.

[0014] In the above technical solution, the temperature of the heat treatment is further limited to a more excellent range, which can achieve a better debonding effect in the process of debonding by pyrolysis.

[0015] In some optional embodiments, the solid content of the sizing agent is 1-10%.

[0016] Optionally, the solid content of the sizing agent is 4-8%.

[0017] In the above technical solution, the solid content of the sizing agent is limited within a specific range, which can achieve a better bundling effect. At the same time, a thermoplastic coating with suitable thickness and good thickness uniformity can be obtained after curing.

[0018] In some optional embodiments, in the twisting step, the twisting specification is 10 to 50 pieces / m.

[0019] Optionally, in the twisting step, the twisting specification is 20 to 40 pieces / m.

[0020] In the above technical solution, the twisting specifications are gradually limited within a specific range, which helps the degumming agent and the sizing agent to infiltrate the carbon fiber bundles, thereby achieving better degumming and sizing effects, and at the same time, it can also achieve a better bundling effect.

[0021] In some optional embodiments, in the slitting step, the slitting method is gantry type or rotary type.

[0022] Optionally, the cutting method is gantry type.

[0023] Optionally, the slitting speed is 0.1-2 m / min.

[0024] In the above technical solution, the gantry type or rotary type slitting method can achieve a better slitting effect, among which the gantry type slitting method can achieve a better slitting effect than the rotary type slitting method.

[0025] Furthermore, controlling the slitting speed within a specific range can enable the corresponding production line to have an appropriate production rate, thereby enabling each work section to have a more appropriate processing time to obtain chopped carbon fibers of better quality.

[0026] In some optional embodiments, in the pre-drying step, the pre-drying equipment is a steam-heated drying roller, and the treatment temperature is 100-250° C. and the treatment pressure is 0.3-0.6 MPa.

[0027] Optionally, the treatment temperature is 180-220° C., and the treatment pressure is 0.5-0.6 MPa.

[0028] In the above technical scheme, the processing temperature and processing pressure in the pre-drying treatment are limited within a specific range step by step, so that the slurry on the surface of the carbon fiber bundle has an appropriate degree of solidification after pre-drying, which is convenient for subsequent slitting treatment and can also obtain high-quality chopped carbon fibers (if the degree of solidification is low, the coating is easy to adhere to the slitting equipment during slitting, affecting the slitting efficiency and slitting effect; if the degree of solidification is too high, the coating is easy to break during slitting, resulting in a decrease in product yield).

[0029] In some optional embodiments, in the drying step, the drying equipment is a tunnel-type pyrolysis furnace, and the treatment temperature is 200-300° C., and the conveying speed is 0.1-5 m / min.

[0030] Optionally, the processing temperature is 250-300° C. and the conveying speed is 0.5-2 m / min.

[0031] In the above technical solution, the processing temperature and the conveying speed in the drying process are limited step by step within a specific range to provide more suitable drying conditions, thereby achieving a better drying effect.

[0032] In the second aspect, an embodiment of the present application provides a manufacturing device for chopped carbon fiber, which is suitable for the preparation method provided in the embodiment of the first aspect, and includes a wire withdrawal rack, a degumming tank or a pyrolysis furnace, a glue application tank, a drying roller, a slitting machine and a drying furnace arranged in sequence along the conveying direction of the carbon fiber bundle.

[0033] In the above technical solution, a specific form of chopped carbon fiber manufacturing device is used, which can be combined with the preparation method provided in the first aspect embodiment to prepare chopped carbon fibers that are resistant to high temperatures and can be firmly combined with a thermoplastic matrix material. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0035] Figure 1 A process flow chart of a method for preparing chopped carbon fibers provided in an embodiment of the present application;

[0036] Figure 2 A schematic structural diagram of a device for manufacturing chopped carbon fibers provided in an embodiment of the present application.

[0037] Icons: 10- manufacturing device for chopped carbon fiber; 100- defilament withdrawal rack; 200- pyrolysis furnace; 300- glue tank; 400- drying roller; 500- slitting machine; 600- drying furnace; 700- vibrating screen. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0039] It should be noted that “and / or” in this application, such as “Feature 1 and / or Feature 2”, refers to the three situations of “Feature 1” alone, “Feature 2” alone, or “Feature 1” plus “Feature 2”.

[0040] In addition, in the description of the present application, unless otherwise specified, the meaning of "multiple" in "one or more" refers to two or more; the range of "value a ~ value b" includes the two end values ​​"a" and "b", and the "unit" in "value a ~ value b + unit of measurement" represents the "unit of measurement" of both "value a" and "value b".

[0041] The preparation method and manufacturing device of the chopped carbon fiber according to the embodiment of the present application are described in detail below.

[0042] In a first aspect, an embodiment of the present application provides a method for preparing chopped carbon fibers, comprising the following steps: providing a continuous finished carbon fiber bundle, the surface of the carbon fiber bundle being a thermosetting coating; sequentially performing twisting treatment, degumming treatment, sizing treatment, pre-drying treatment, slitting treatment and drying treatment on the carbon fiber bundle to obtain chopped carbon fibers; wherein, in the sizing treatment step, the sizing agent is a thermoplastic resin.

[0043] At present, the surface of commercially available carbon fiber bundles is usually a thermosetting coating (i.e., cured after coating with an epoxy resin sizing agent), and chopped carbon fibers are cut from corresponding commercially available carbon fiber bundles. On the one hand, since the coating formed by the epoxy resin sizing agent is not resistant to high temperatures, the corresponding chopped carbon fibers are difficult to meet the high-temperature processing requirements; on the other hand, although the coating formed by the epoxy resin sizing agent can be stably combined with the epoxy resin matrix, it is difficult to stably combine with the thermoplastic resin matrix. In this application, the researchers first de-glue the carbon fiber bundle after the twisting treatment to remove the epoxy resin thermosetting coating on the surface of the carbon fiber material, and then re-apply the thermoplastic coating on the surface of the carbon fiber material through the sizing treatment. The chopped carbon fibers prepared by this preparation method are resistant to high temperatures and can be firmly combined with the thermoplastic matrix material.

[0044] It should be noted that the type of the finished carbon fiber bundle is not limited, and the currently mainstream commercially available carbon fiber bundle can be selected as long as the coating on its surface is a thermosetting coating, such as T700-12K.

[0045] It should be noted that the current preparation process of chopped carbon fiber usually uses waste silk or tail yarn as preparation raw materials. The embodiment of the present application uses continuous finished carbon fiber bundles, and the prepared chopped carbon fiber also has the properties of continuous defect-free and better mechanical properties.

[0046] It should be noted that the specific type of thermoplastic resin is not limited and can be selected according to conventional methods in the art, such as polyimide or polyaryletherketone.

[0047] As an example, the degumming step includes: immersing the twisted carbon fiber bundle in a degumming agent, the degumming agent includes acetone; or, placing the twisted carbon fiber bundle in a pyrolysis furnace for heat treatment, the heat treatment temperature is 250-450°C, for example but not limited to any one of 250°C, 300°C, 350°C, 400°C and 450°C or a range between any two of them.

[0048] In this embodiment, the epoxy resin thermosetting coating on the surface of the carbon fiber material can be effectively removed by immersing the carbon fiber bundle in a degumming agent or heat treating it in a pyrolysis furnace. Among them, limiting the composition of the degumming agent and limiting the temperature of the heat treatment are both helpful to improve the degumming effect.

[0049] As an example, the adhesive stripping agent includes acetone and methylene chloride.

[0050] In this embodiment, a mixed system of acetone and dichloromethane is used as a degumming agent, which can achieve a better degumming effect.

[0051] As an example, the volume ratio of acetone to dichloromethane is (2-4):1, such as but not limited to any one of 2:1, 2.5:1, 3:1, 3.5:1 and 4:1 or a range between any two of the volume ratios.

[0052] In this embodiment, the volume ratio of acetone to dichloromethane is further limited within a specific range, which is more helpful to improve the debonding effect of the debonding agent.

[0053] As an example, the heat treatment temperature is 300-400°C, for example but not limited to any one of 300°C, 320°C, 340°C, 360°C, 380°C and 400°C or a range between any two of them.

[0054] In this embodiment, the temperature of the heat treatment is further limited to a more excellent range, which can achieve a better debonding effect during the debonding process by the pyrolysis method.

[0055] As an example, the solid content of the sizing agent is 1-10%, such as but not limited to any one of 1%, 2%, 4%, 6%, 8% and 10% or a range between any two of the solid content.

[0056] As an example, the solid content of the sizing agent is 4-8%, such as but not limited to any one of 4%, 5%, 6%, 7% and 8% or a range between any two of the solid content.

[0057] In this embodiment, the solid content of the sizing agent is limited within a specific range, so that a better bundling effect can be achieved. At the same time, a thermoplastic coating with a suitable thickness and good thickness uniformity can be obtained after curing.

[0058] As an example, in the twisting step, the twisting specification is 10 to 50 pieces / m, for example but not limited to any one of 10 pieces / m, 20 pieces / m, 30 pieces / m, 40 pieces / m and 50 pieces / m or a range between any two of them.

[0059] As an example, in the twisting step, the twisting specification is 20 to 40 pieces / m, for example but not limited to any one of 10 pieces / m, 15 pieces / m, 20 pieces / m, 25 pieces / m, 30 pieces / m, 35 pieces / m and 40 pieces / m or a range value between any two of them.

[0060] In this embodiment, the twisting specifications are gradually limited within a specific range, which helps the degumming agent and the sizing agent to infiltrate the carbon fiber bundle, thereby achieving better degumming and sizing effects, and at the same time, it can also achieve a better bundling effect.

[0061] As an example, in the slitting process step, the slitting method is a gantry type or a rotary type.

[0062] As an example, the cutting method is gantry type.

[0063] In this embodiment, the gantry type or rotary type slitting method can achieve a better slitting effect, among which the gantry type slitting method can achieve a better slitting effect than the rotary type slitting method.

[0064] As an example, the slitting speed is 0.1-2 m / min, for example but not limited to, the slitting speed is any one of 0.1 m / min, 0.5 m / min, 1 m / min, 1.5 m / min and 2 m / min or a range between any two of them.

[0065] It should be noted that, usually, twisting, degumming, sizing, pre-drying and slitting are all on the same production line, so the slitting speed also determines the processing speed of the front-end process.

[0066] In this embodiment, the slitting speed is further controlled within a specific range, so that the corresponding production line can have a suitable production rate, and then each section has a more suitable processing time to obtain short-cut carbon fibers with better quality.

[0067] As an example, in the pre-drying treatment step, the pre-drying equipment is a steam-heated drying roller, and the treatment temperature is 100-250°C, for example but not limited to the temperature being any one of 100°C, 150°C, 200°C and 250°C or a range between any two of them; the treatment pressure is 0.3-0.6MPa, for example but not limited to the treatment pressure being any one of 0.3MPa, 0.4MPa, 0.5MPa and 0.6MPa or a range between any two of them.

[0068] As an example, the processing temperature is 180-220°C, for example but not limited to the temperature being any point value among 180°C, 190°C, 200°C, 210°C and 220°C or the range value between any two thereof; the processing pressure is 0.5-0.6MPa, for example but not limited to the processing pressure being any point value among 0.52MPa, 0.54MPa, 0.56MPa, 0.58MPa and 0.6MPa or the range value between any two thereof.

[0069] In this embodiment, the processing temperature and processing pressure in the pre-drying treatment are limited step by step within a specific range, so that the slurry on the surface of the carbon fiber bundle has an appropriate degree of solidification after pre-drying, thereby facilitating the subsequent slitting process and obtaining higher-quality chopped carbon fibers (if the degree of solidification is too low, the coating is likely to adhere to the slitting equipment during slitting, affecting the slitting efficiency and slitting effect; if the degree of solidification is too high, the coating is likely to break during slitting, resulting in a reduction in product yield).

[0070] As an example, in the drying treatment step, the drying equipment is a tunnel pyrolysis furnace, and the treatment temperature is 200-300°C, for example but not limited to the temperature of any one of 200°C, 220°C, 240°C, 260°C, 280°C and 300°C or a range between any two of them; the conveying speed is 0.1-5m / min, for example but not limited to the conveying speed of any one of 0.1m / min, 0.5m / min, 1m / min, 2m / min, 3m / min, 4m / min and 5m / min or a range between any two of them.

[0071] As an example, the processing temperature is 250-300°C, for example but not limited to the temperature being any one of 250°C, 260°C, 270°C, 280°C, 290°C and 300°C or a range between any two thereof; the conveying speed is 0.5-2m / min, for example but not limited to the conveying speed being any one of 0.5m / min, 1m / min, 1.5m / min and 2m / min or a range between any two thereof.

[0072] In this embodiment, the processing temperature and the conveying speed in the drying process are limited step by step within specific ranges to provide more suitable drying conditions, thereby achieving better drying effects.

[0073] It should be noted that any process or step not specifically described or limited in the preparation process of chopped carbon fibers may be arranged according to conventional selections in the art.

[0074] As an example, in the slitting step, the length of the chopped carbon fibers after slitting is 2 to 10 mm, the volume density of the chopped carbon fibers is greater than 400 g / L, and the contour shape of the chopped carbon fibers is flat or columnar.

[0075] As an example, the process flow chart of the preparation method of chopped carbon fiber is shown as follows: Figure 1 shown.

[0076] See also Figure 2 In the second aspect, the embodiment of the present application provides a manufacturing device 10 for chopped carbon fiber, which is suitable for the preparation method provided in the embodiment of the first aspect, and includes a wire withdrawal rack 100, a degumming tank or a pyrolysis furnace 200, a glue application tank 300, a drying roller 400, a slitting machine 500 and a drying furnace 600 arranged in sequence along the conveying direction of the carbon fiber bundle.

[0077] In the present application, a manufacturing device 10 for chopped carbon fibers in a specific form can be used in combination with the preparation method provided in the first embodiment to prepare chopped carbon fibers that are resistant to high temperatures and can be firmly bonded to a thermoplastic matrix material. Among them, the wire withdrawal rack 100 is used for twisting treatment, the degumming tank or pyrolysis furnace 200 is used for degumming treatment, the glue tank 300 is used for glue application treatment, the drying roller 400 is used for pre-drying treatment, the slitting machine 500 is used for slitting treatment, and the drying furnace 600 is used for drying treatment.

[0078] It should be noted that since each device in the manufacturing apparatus for chopped carbon fiber is a common type of device in the art, the embodiments of the present application do not further introduce the devices, and the devices can be arranged in a conventional manner in the art.

[0079] As an example, along the conveying direction of the carbon fiber bundle, the downstream of the drying furnace further includes a vibrating screen 700, and the vibrating screen 700 is a linear vibrating screen with three outlets and a length of 1.5 to 2 m.

[0080] In this embodiment, the provision of the vibrating screen 700 is beneficial to improving the specification consistency of the chopped carbon fibers.

[0081] As an example, the length of the glue tank 300 is 0.8-1.2 m, and the conveying roller in the glue tank has a groove for accommodating the carbon fiber bundle.

[0082] The features and performance of the present application are further described in detail below in conjunction with the embodiments.

[0083] Example 1

[0084] The present invention provides a method for preparing chopped carbon fibers, comprising the following steps:

[0085] A continuous finished carbon fiber bundle is provided, the surface of the carbon fiber bundle is a thermosetting coating, and the specific model of the finished carbon fiber bundle is T700-12K; the carbon fiber bundle is subjected to twisting treatment, degumming treatment, sizing treatment, pre-drying treatment, slitting treatment, drying treatment and vibration powder screening treatment in sequence to obtain short-cut carbon fiber.

[0086] Specifically, in the twisting treatment step, the twisting specification is 25 pieces / m; in the degumming treatment step, the degumming agent is immersed in the degumming tank, and the degumming agent is a mixed system of acetone and dichloromethane, and the volume ratio of the two is 3:1 respectively; in the sizing treatment step, the sizing agent is a polyimide thermoplastic resin, and the solid content of the sizing agent is 6%; in the pre-drying treatment step, the pre-drying equipment is a steam-heated drying roller, the treatment temperature is 200°C, and the treatment pressure is 0.5MPa; in the drying treatment step, the drying equipment is a tunnel pyrolysis furnace, the treatment temperature is 250°C, and the conveying speed is 2.5m / min; in the slitting treatment step, the slitting method is a gantry type, and the slitting speed is 0.1-2m / min.

[0087] Example 2

[0088] The embodiment of the present application provides a method for preparing chopped carbon fibers, which differs from Embodiment 1 only in that, in the degumming step, heat treatment is performed in a pyrolysis furnace at a temperature of 350°C.

[0089] Example 3

[0090] The embodiment of the present application provides a method for preparing chopped carbon fibers, which is different from the embodiment 1 only in that the debonding agent is only acetone.

[0091] Example 4

[0092] The embodiment of the present application provides a method for preparing chopped carbon fibers, which is different from the embodiment 1 only in that the debonding agent is only dichloromethane.

[0093] Example 5

[0094] The embodiment of the present application provides a method for preparing chopped carbon fibers, which differs from Embodiment 1 only in that the debonding agent is a mixed system of acetone and dichloromethane, and the volume ratio of the two is 2:1 respectively.

[0095] Example 6

[0096] The embodiment of the present application provides a method for preparing chopped carbon fibers, which differs from Embodiment 1 only in that the debonding agent is a mixed system of acetone and dichloromethane, and the volume ratio of the two is 4:1 respectively.

[0097] Example 7

[0098] The embodiment of the present application provides a method for preparing chopped carbon fibers, which differs from Embodiment 1 only in that the debonding agent is a mixed system of acetone and dichloromethane, and the volume ratio of the two is 1:1.

[0099] Example 8

[0100] The embodiment of the present application provides a method for preparing chopped carbon fibers, which differs from Embodiment 1 only in that the debonding agent is a mixed system of acetone and dichloromethane, and the volume ratio of the two is 5:1.

[0101] Example 9

[0102] The embodiment of the present application provides a method for preparing chopped carbon fibers, which differs from Embodiment 2 only in that, in the degumming step, heat treatment is performed in a pyrolysis furnace at a temperature of 300°C.

[0103] Example 10

[0104] The embodiment of the present application provides a method for preparing chopped carbon fibers, which differs from Embodiment 2 only in that, in the degumming step, heat treatment is performed in a pyrolysis furnace at a temperature of 400°C.

[0105] Embodiment 11

[0106] The embodiment of the present application provides a method for preparing chopped carbon fibers, which differs from Embodiment 2 only in that, in the degumming step, heat treatment is performed in a pyrolysis furnace at a temperature of 250°C.

[0107] Example 12

[0108] The embodiment of the present application provides a method for preparing chopped carbon fibers, which differs from Embodiment 2 only in that, in the degumming step, heat treatment is performed in a pyrolysis furnace at a temperature of 450°C.

[0109] Comparative Example 1

[0110] The comparative example of the present application provides a method for preparing chopped carbon fibers, which differs from Example 1 only in that no degumming treatment is performed.

[0111] Test example

[0112] Performance test of chopped carbon fiber

[0113] Test method:

[0114] The chopped carbon fibers prepared in Examples 1 to 12 and Comparative Example 1 were numbered respectively, and then each sample was compounded with a bismaleimide thermoplastic resin matrix, and then the interlaminar interface bonding strength of the composite material at room temperature and after high temperature treatment (treated at 180°C for 48h) was tested. Specifically, the interlaminar shear strength was determined according to JC / T 773-2010 and GB / T 30969.

[0115] Table 1 Performance statistics of each sample

[0116]

[0117] Referring to Table 1, it can be seen from the test results of Examples 1 to 12 and Comparative Example 1 that after the twisting treatment, the carbon fiber bundle is first debonded to remove the epoxy resin thermosetting coating on the surface of the carbon fiber material, and then the thermoplastic coating is re-applied to the surface of the carbon fiber material through a sizing treatment. Compared with the sizing treatment directly after the twisting treatment, the short carbon fiber reinforced thermoplastic composite material corresponding to the former has a better interlayer interface bonding strength at room temperature and after high temperature treatment, that is, it has a better high temperature resistance.

[0118] From the test results of Example 1 and Examples 3 to 8, it can be seen that when a mixed system of acetone and dichloromethane is used as a degumming agent and the volume ratio of the two is limited to a specific range, compared with using a single degumming agent or not limiting the volume ratio of the two within a specific range, the short-cut carbon fiber reinforced thermoplastic composite material corresponding to the former has better interlayer interface bonding strength at room temperature and after high temperature treatment, that is, has better high temperature resistance.

[0119] It can be seen from the test results of Examples 2 and 9 to 12 that in the step of degumming using a pyrolysis furnace, the temperature of the heat treatment is limited to a specific range. Compared with not limiting the treatment temperature to a specific range, the short carbon fiber reinforced thermoplastic composite material corresponding to the former has better interlayer interface bonding strength at room temperature and after high temperature treatment, that is, it has better high temperature resistance.

[0120] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

Claims

1. A method for preparing chopped carbon fiber, It is characterized in that The following steps are involved: Providing a continuous finished carbon fiber bundle, wherein the surface of the carbon fiber bundle is a thermosetting coating; The carbon fiber bundle is subjected to twisting treatment, degumming treatment, sizing treatment, pre-drying treatment, slitting treatment and drying treatment in sequence to obtain chopped carbon fiber; wherein, in the sizing treatment step, the sizing agent is a thermoplastic resin.

2. The preparation method according to claim 1, It is characterized in that The degumming step comprises: soaking the twisted carbon fiber bundle in a degumming agent, wherein the degumming agent comprises acetone; Alternatively, the carbon fiber bundle after twisting is placed in a pyrolysis furnace for heat treatment, and the heat treatment temperature is 250-450°C.

3. The preparation method according to claim 2, It is characterized in that The debonding agent includes acetone and dichloromethane; Optionally, the volume ratio of the acetone to the dichloromethane is (2-4):

1.

4. The preparation method according to claim 2, It is characterized in that The temperature of the heat treatment is 300-400°C.

5. The preparation method according to any one of claims 1 to 4, It is characterized in that The solid content of the sizing agent is 1 to 10%; Optionally, the solid content of the sizing agent is 4-8%.

6. The preparation method according to any one of claims 1 to 4, It is characterized in that In the twisting step, the twisting specification is 10 to 50 pieces / m; Optionally, in the twisting step, the twisting specification is 20 to 40 pieces / m.

7. The preparation method according to any one of claims 1 to 4, It is characterized in that In the step of slitting, the slitting method is gantry type or rotary type; Optionally, the slitting method is gantry type; Optionally, the slitting speed is 0.1-2 m / min.

8. The preparation method according to any one of claims 1 to 4, It is characterized in that In the step of pre-drying treatment, the pre-drying equipment is a steam-heated drying roller, and the treatment temperature is 100-250° C. and the treatment pressure is 0.3-0.6 MPa; Optionally, the treatment temperature is 180-220° C., and the treatment pressure is 0.5-0.6 MPa.

9. The preparation method according to any one of claims 1 to 4, It is characterized in that In the drying step, the drying equipment is a tunnel-type pyrolysis furnace, and the treatment temperature is 200-300°C, and the conveying speed is 0.1-5m / min; Optionally, the processing temperature is 250-300° C., and the conveying speed is 0.5-2 m / min.

10. A device for producing chopped carbon fibers, It is characterized in that The preparation method according to any one of claims 1 to 9 comprises a defilament rack, a debonding tank or a pyrolysis furnace, a sizing tank, a drying roller, a slitting machine and a drying furnace arranged in sequence along the conveying direction of the carbon fiber bundle.

Citation Information

Patent Citations

  • Method for preparing phenolic resin system Z-pin by using twisted carbon fibers

    CN104029401A

  • Nano-material enhanced high-temperature-resistant type carbon fiber thermoplastic sizing agent and preparing method and application thereof

    CN109826013A

  • Chopped fiber bundle of carbon fibers

    CN111020782A

  • Method and device for producing chopped carbon fibers for thermoplastic

    CN115404697A