Battery cell and electric equipment

By optimizing the adhesion and structural design of the electrode components in the battery cell, the problem of easy cracking of the outer shell or tearing of the electrode components when the steel-cased battery cell is subjected to stress has been solved, achieving efficient protection and extended service life of the battery cell.

CN118983494APending Publication Date: 2024-11-19NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411073604.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

When a steel-cased battery cell is subjected to stress, the adhesive force of the adhesive tape is difficult to balance, which can easily cause the casing to crack or the electrode components to tear, resulting in a higher possibility of battery cell failure.

Method used

By setting the adhesion force between the first negative electrode and the first end wall in the electrode assembly to be greater than or equal to 10 N/m, the adhesion force between the first negative electrode and the first diaphragm to be less than the adhesion force between the first positive electrode and the first diaphragm, and setting the negative electrode on the outermost side of the electrode assembly, and by combining the design of the negative electrode active material layer and the diaphragm, the content of the adhesive layer and the adhesive is optimized in order to control the adhesion force and the adhesion area.

Benefits of technology

This reduces the likelihood of the casing cracking and electrode assembly tearing when the battery cell is subjected to stress, extends the battery cell's lifespan, and reduces the risk of electrode damage or short circuits caused by collisions between the electrode and the casing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983494A_ABST
    Figure CN118983494A_ABST
Patent Text Reader

Abstract

The invention provides a battery cell and electric equipment, a battery cell shell comprises a shell and an electrode assembly, the electrode assembly is accommodated in the shell, and the shell comprises a first end wall and a second end wall which are oppositely arranged along the thickness direction of the electrode assembly; the electrode assembly comprises a first positive pole piece, a first negative pole piece and a first diaphragm, the first negative pole piece is bonded to the first end wall through a first bonding layer, the first positive pole piece is located on the side, opposite to the first end wall, of the first negative pole piece, and the first diaphragm is arranged between the first positive pole piece and the first negative pole piece; wherein the bonding force of the first bonding layer is F1, and F1 is larger than or equal to 10 N / m; the adhesive force between the first negative pole piece and the first diaphragm is F2, the adhesive force between the first positive pole piece and the first diaphragm is F3, and F2 is smaller than F3. The possibility that the shell cracks when the battery cell is stressed can be reduced, and the possibility that the electrode assembly is torn when the battery cell is stressed can also be reduced, so that the possibility that the battery cell loses efficacy after being stressed is relatively low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a battery cell and an electrical device. Background Art

[0002] With the rapid development of new energy technologies, batteries have been widely used in electronic equipment, electric vehicles, electric two-wheelers, power tools, etc. The requirements for battery quality, safety, and miniaturization are becoming increasingly higher.

[0003] The electrode assemblies in steel-shell batteries are generally bonded to the outer shell with adhesive tape. If the adhesive force of the adhesive tape is large, when the steel-shell battery is subjected to stress, the impulse of the external force transmitted to the electrode assembly through the adhesive tape is large, and the electrode assembly is easily torn; if the adhesive force of the adhesive tape is small, the impulse of the external force transmitted to the electrode assembly through the adhesive tape is small, and the outer shell is easily cracked. The above two failure modes are difficult to balance, resulting in a higher possibility of failure of the steel-shell battery when subjected to stress. Summary of the invention

[0004] The present application provides a battery cell and electrical equipment, which can reduce the possibility of failure of the battery cell due to stress.

[0005] In a first aspect, the present application provides a battery cell, which includes a shell and an electrode assembly, wherein the electrode assembly is accommodated in the shell, and the shell includes a first end wall and a second end wall arranged opposite to each other along the thickness direction of the electrode assembly; the electrode assembly includes a first positive electrode sheet, a first negative electrode sheet and a first separator, the first negative electrode sheet is bonded to the first end wall through a first adhesive layer, the first positive electrode sheet is located on the side of the first negative electrode sheet facing away from the first end wall, and the first separator is arranged between the first positive electrode sheet and the first negative electrode sheet; wherein the adhesion force of the first adhesive layer is F1, satisfying F1≥10N / m; the adhesion force between the first negative electrode sheet and the first separator is F2, and the adhesion force between the first positive electrode sheet and the first separator is F3, satisfying F2<F3.

[0006] In the above technical solution, the battery cell includes a shell and an electrode assembly, and the electrode assembly is accommodated in the shell, so that the shell can protect the electrode assembly; by making the adhesion force F1 of the first adhesive layer between the first negative electrode plate and the first end wall ≥ 10N / m, the adhesion force between the electrode assembly and the first end wall can be made larger, the external force can be more transmitted to the electrode assembly through the first adhesive layer, and more impulse is absorbed. The impulse of the external force on the battery cell transmitted to the electrode assembly through the first adhesive layer is larger, and the possibility of cracking of the shell is smaller; by making the adhesion force F2 between the first negative electrode plate and the first diaphragm and the adhesion force F3 between the first positive electrode plate and the first diaphragm satisfy F2 < F3, so that the bonding force between the first negative electrode plate and the first diaphragm is relatively small, and the impulse transmitted to the first positive electrode plate can be reduced. Because in general, the thickness of the negative electrode plate is greater than that of the positive electrode plate, when the battery cell is subjected to force, the negative electrode plate is less likely to tear than the positive electrode plate. Therefore, by setting the first negative electrode plate at the outermost side of the electrode assembly, and transmitting more impulse of the external force to the first negative electrode plate, and less impulse to the first positive electrode plate and other plates, it is possible to make each plate of the electrode assembly less likely to tear, thereby reducing the possibility of tearing of the electrode assembly, making the possibility of failure of the battery cell under force lower, which is conducive to extending the service life of the battery cell. Therefore, in the above scheme, it can be ensured that in the case of large bonding force, the problem of electrode plate tearing and causing failure of the battery cell under force can be avoided.

[0007] In some embodiments of the present application, F3-F2≥5N / m.

[0008] In the above technical solution, by making F3-F2≥5N / m, the first negative electrode plate and the first diaphragm can be separated more evenly, thereby further reducing the impulse transmitted to the first positive electrode plate, further reducing the possibility of tearing of the electrode assembly, and making the possibility of stress failure of the battery cell lower, which is beneficial to extending the service life of the battery cell.

[0009] In some embodiments of the present application, 10 N / m ≤ F2 ≤ 95 N / m, 15 N / m ≤ F3 ≤ 100 N / m.

[0010] In the above technical scheme, when F2 is greater than or equal to 10N / m, the possibility of the first negative electrode sheet being separated from the first diaphragm is reduced, thereby reducing the possibility of the outer shell receiving an excessive impulse and cracking, and reducing the possibility of other electrode sheets except the first negative electrode sheet colliding with the outer shell and being damaged or even short-circuiting; when F2 is less than or equal to 95N / m, the impulse transmitted to the first positive electrode sheet by the external force is reduced, thereby further reducing the possibility of the electrode assembly tearing; therefore, when 10N / m≤F2≤95N / m, it can reduce the possibility of the first negative electrode sheet being separated from the first diaphragm, thereby reducing the possibility of the outer shell receiving an excessive impulse and cracking, and reducing the possibility of other electrode sheets except the first negative electrode sheet colliding with the outer shell and being damaged or even short-circuiting, and reducing the impulse transmitted to the first positive electrode sheet by the external force, thereby further reducing the possibility of the electrode assembly tearing.

[0011] When F3 is greater than or equal to 15N / m, the first diaphragm is less likely to be separated from the first positive electrode sheet, thereby reducing the possibility of the outer shell receiving an excessive impulse and cracking, and reducing the possibility of the other electrodes except the first negative electrode sheet colliding with the outer shell and being damaged or even short-circuiting; when F3 is less than or equal to 100N / m, the impulse transmitted to the first positive electrode sheet by the external force is less, thereby reducing the possibility of the electrode assembly tearing; therefore, when 15N / m≤F3≤100N / m, the first diaphragm is less likely to be separated from the first positive electrode sheet, thereby reducing the possibility of the outer shell receiving an excessive impulse and cracking, and reducing the possibility of the other electrodes except the first negative electrode sheet colliding with the outer shell and being damaged or even short-circuiting, and reducing the impulse transmitted to the first positive electrode sheet by the external force, thereby reducing the possibility of the electrode assembly tearing.

[0012] In some embodiments of the present application, the first negative electrode plate includes a negative electrode collector and a negative electrode active material layer, the negative electrode active material layer is arranged on the side of the negative electrode collector facing the first positive electrode plate, and a groove is arranged on the side of the negative electrode active material layer facing the first separator.

[0013] In the above technical solution, by providing the negative electrode active material layer on the side of the negative electrode current collector facing the first positive electrode plate, and providing a groove on the side of the negative electrode active material layer facing the first diaphragm, the bonding area between the negative electrode active material layer and the first diaphragm can be made smaller, thereby making the bonding force between the negative electrode active material layer and the first diaphragm smaller, and reducing the impulse transmitted to the first positive electrode plate, thereby reducing the possibility of tearing of the electrode assembly, making the possibility of failure of the battery cell due to force lower, which is beneficial to extending the service life of the battery cell.

[0014] In some embodiments of the present application, the projection area of ​​the groove in the thickness direction of the first negative electrode sheet is S1, and the projection area of ​​the negative active material layer in the thickness direction of the first negative electrode sheet is S2, satisfying 5%≤S1 / S2≤35%.

[0015] In the above technical solution, when S1 / S2 is greater than or equal to 5%, the bonding area between the negative electrode active material layer and the first diaphragm can be smaller, so that the bonding force between the negative electrode active material layer and the first diaphragm is smaller, and the impulse transmitted to the first positive electrode plate can be reduced, thereby reducing the possibility of tearing the electrode assembly; when S1 / S2 is less than or equal to 35%, the bonding area between the negative electrode active material layer and the first diaphragm can be larger, so that the bonding force between the negative electrode active material layer and the first diaphragm is larger, and the possibility of the first negative electrode plate being separated from the first diaphragm is smaller, thereby It can reduce the possibility that the outer shell receives an excessive impulse and cracks, and can also reduce the possibility that the other pole pieces except the first negative pole piece collide with the outer shell and are damaged or even short-circuited; therefore, when 5%≤S1 / S2≤35%, it can not only reduce the impulse transmitted to the first positive pole piece, thereby reducing the possibility of tearing of the electrode assembly, but also reduce the possibility that the first negative pole piece separates from the first diaphragm, thereby reducing the possibility that the outer shell receives an excessive impulse and cracks, and can also reduce the possibility that the other pole pieces except the first negative pole piece collide with the outer shell and are damaged or even short-circuited.

[0016] In some embodiments of the present application, the groove extends along the first direction, the width of the groove along the second direction is W1, the width of the negative electrode active material layer along the second direction is W2, satisfying 5%≤W1 / W2≤35%; the thickness direction, the first direction, and the second direction of the electrode assembly are perpendicular to each other.

[0017] In the above technical solution, when W1 / W2 is greater than or equal to 5%, the bonding area between the negative electrode active material layer and the first diaphragm can be smaller, thereby making the bonding force between the negative electrode active material layer and the first diaphragm smaller, which can reduce the impulse transmitted to the first positive electrode plate, thereby reducing the possibility of tearing the electrode assembly; when W1 / W2 is less than or equal to 35%, the bonding area between the negative electrode active material layer and the first diaphragm can be larger, thereby making the bonding force between the negative electrode active material layer and the first diaphragm larger, which can reduce the possibility of the first negative electrode plate detaching from the first diaphragm, thereby reducing the possibility of the shell receiving too much impulse and cracking, and can also reduce the possibility of tearing the first positive electrode plate. The possibility of other pole pieces other than the first negative pole piece colliding with the outer shell and being damaged or even short-circuiting is small, and the possibility of the first diaphragm extending into the groove and adhering to the side wall of the groove can be reduced; therefore, when 5%≤W1 / W2≤35%, it can not only reduce the impulse transmitted to the first positive pole piece, thereby reducing the possibility of tearing of the electrode assembly, but also make the possibility of the first negative pole piece detaching from the first diaphragm small, thereby making the possibility of the outer shell receiving excessive impulse and cracking small, and also make the possibility of other pole pieces other than the first negative pole piece colliding with the outer shell and being damaged or even short-circuiting is small, and the possibility of the first diaphragm extending into the groove and adhering to the side wall of the groove can be reduced.

[0018] In some embodiments of the present application, the first positive electrode plate includes a positive electrode collector, a first positive electrode active material layer and a second positive electrode active material layer. The first positive electrode active material layer is arranged on the side of the positive electrode collector facing the first negative electrode plate, and the second positive electrode active material layer is arranged on the side of the positive electrode collector facing away from the first negative electrode plate; the first positive electrode active material layer is arranged in a plane on the side facing the first diaphragm.

[0019] In the above technical solution, by making the first positive electrode active material layer be arranged in a plane on the side facing the first diaphragm, the bonding area between the first positive electrode active material layer and the first diaphragm can be made larger, thereby making the bonding force between the first positive electrode active material layer and the first diaphragm larger, and making it less likely that the first negative electrode plate and the first diaphragm will separate from the first positive electrode plate, thereby making it less likely that the outer shell will receive an excessive impulse and crack, and also making it less likely that other plates except the first negative electrode plate will collide with the outer shell and be damaged or even short-circuited.

[0020] In some embodiments of the present application, the first negative electrode plate includes a negative electrode collector and a negative electrode active material layer, the negative electrode active material layer is arranged on the side of the negative electrode collector facing the first positive electrode plate, the negative electrode active material layer includes a first adhesive, and the content of the first adhesive in the negative electrode active material layer is 0.3% to 0.8%.

[0021] In the above technical solution, when the content of the first binder in the negative electrode active material layer is greater than or equal to 0.3%, the bonding force between the negative electrode active material layer and the first diaphragm can be relatively large, and the possibility of the first negative electrode plate being separated from the first diaphragm can be relatively small, thereby reducing the possibility of the shell receiving an excessive impulse and cracking, and reducing the possibility of other plates except the first negative electrode plate colliding with the shell and being damaged or even short-circuited; when the content of the first binder in the negative electrode active material layer is less than or equal to 0.8%, the bonding force between the negative electrode active material layer and the first diaphragm can be relatively small, and the impulse transmitted to the first positive electrode plate can be reduced. Since in general, the thickness of the negative electrode plate is greater than that of the positive electrode plate, when the battery cell is subjected to force, the negative electrode plate is thicker than the positive electrode plate. It is less likely to tear, so by arranging the first negative electrode plate at the outermost side of the electrode assembly and transferring more impulse of the external force to the first negative electrode plate, and transferring less impulse to the first positive electrode plate and other plates, it is possible that each plate of the electrode assembly is not easily torn, thereby reducing the possibility of tearing of the electrode assembly; therefore, when the content of the first adhesive in the negative electrode active material layer is 0.3% to 0.8%, it can reduce the possibility of the first negative electrode plate detaching from the first diaphragm, thereby reducing the possibility of the outer shell receiving excessive impulse and cracking, and can reduce the possibility of other plates except the first negative electrode plate colliding with the outer shell and being damaged or even short-circuited, and can reduce the impulse transferred to the first positive electrode plate, thereby reducing the possibility of tearing of the electrode assembly.

[0022] In some embodiments of the present application, the first positive electrode plate includes a positive electrode collector, a first positive electrode active material layer and a second positive electrode active material layer, the first positive electrode active material layer is arranged on the side of the positive electrode collector facing the first negative electrode plate, and the second positive electrode active material layer is arranged on the side of the positive electrode collector facing away from the first negative electrode plate; the first positive electrode active material layer includes a second adhesive, and the content of the second adhesive in the first positive electrode active material layer is 0.8% to 2%.

[0023] In the above technical scheme, when the content of the second adhesive in the first positive electrode active material layer is greater than or equal to 0.8%, the bonding force between the first positive electrode active material layer and the first diaphragm can be greater, the possibility of the first positive electrode plate being separated from the first diaphragm can be reduced, and the possibility of other plates except the first negative electrode plate colliding with the outer shell and being damaged or even short-circuited can be reduced; when the content of the second adhesive in the first positive electrode active material layer is less than or equal to 2%, the bonding force between the first positive electrode active material layer and the first diaphragm can be smaller, the impulse transmitted to the first positive electrode plate can be reduced, thereby reducing the possibility of tearing of the electrode assembly; therefore, when the content of the second adhesive in the first positive electrode active material layer is 0.8% to 2%, it can not only reduce the possibility of the first positive electrode plate being separated from the first diaphragm, thereby reducing the possibility of other plates except the first negative electrode plate colliding with the outer shell and being damaged or even short-circuited, but also reduce the impulse transmitted to the first positive electrode plate, thereby reducing the possibility of tearing of the electrode assembly.

[0024] In some embodiments of the present application, the first diaphragm includes a base layer, a second adhesive layer and a third adhesive layer, the second adhesive layer is arranged on the side of the base layer facing the first negative electrode sheet, the third adhesive layer is arranged on the side of the base layer facing the first positive electrode sheet, the second adhesive layer includes a third adhesive, the content of the third adhesive in the second adhesive layer is a, the third adhesive layer includes a fourth adhesive, the content of the fourth adhesive in the third adhesive layer is b, satisfying a<b.

[0025] In the above technical solution, by making the content a of the third adhesive in the second adhesive layer and the content b of the fourth adhesive in the third adhesive layer satisfy a<b, the bonding force between the first diaphragm and the first negative electrode plate can be made smaller than the bonding force between the first diaphragm and the first positive electrode plate, and the impulse transmitted to the first positive electrode plate can be reduced, thereby reducing the possibility of tearing of the electrode assembly, making the possibility of stress failure of the battery cell lower, which is beneficial to extending the service life of the battery cell.

[0026] In some embodiments of the present application, 45%≤a≤85%.

[0027] In the above technical scheme, when a is greater than or equal to 45%, the bonding force between the first diaphragm and the first negative electrode sheet can be relatively large, so that the possibility of the first negative electrode sheet being separated from the first diaphragm is relatively small, thereby reducing the possibility that the outer shell receives an excessively large impulse and cracks, and also reducing the possibility that other electrodes except the first negative electrode sheet collide with the outer shell and are damaged or even short-circuited; when a is less than or equal to 85%, the bonding force between the first diaphragm and the first negative electrode sheet can be relatively small, so that the impulse transmitted by the external force to the first positive electrode sheet is relatively small, thereby reducing the possibility that the electrode assembly is torn; therefore, when 45%≤a≤85%, it is not only possible that the first negative electrode sheet is less likely to be separated from the first diaphragm, thereby reducing the possibility that the outer shell receives an excessively large impulse and cracks, but also reducing the possibility that other electrodes except the first negative electrode sheet collide with the outer shell and are damaged or even short-circuited, and also reducing the impulse transmitted by the external force to the first positive electrode sheet, thereby reducing the possibility that the electrode assembly is torn.

[0028] In some embodiments of the present application, the first diaphragm includes a base layer, a second bonding layer and a third bonding layer, the second bonding layer is arranged on the side of the base layer facing the first negative electrode plate, the third bonding layer is arranged on the side of the base layer facing the first positive electrode plate, the second bonding layer includes a first ceramic material, the content of the first ceramic material in the second bonding layer is c, the third bonding layer includes a second ceramic material, the content of the second ceramic material in the third bonding layer is d, and c>d is satisfied.

[0029] In the above technical solution, by making the content c of the first ceramic material in the second bonding layer and the content d of the second ceramic material in the third bonding layer satisfy c>d, the bonding force between the first diaphragm and the first negative electrode plate can be made smaller than the bonding force between the first diaphragm and the first positive electrode plate, thereby reducing the impulse transmitted to the first positive electrode plate, thereby reducing the possibility of tearing of the electrode assembly, making the possibility of stress failure of the battery cell lower, which is beneficial to extending the service life of the battery cell.

[0030] In some embodiments of the present application, 10%≤c≤50%.

[0031] In the above technical solution, when c is greater than or equal to 10%, the adhesion force between the first diaphragm and the first negative electrode sheet can be smaller, so that the impulse transmitted by the external force to the first positive electrode sheet is smaller, thereby reducing the possibility of tearing of the electrode assembly; when c is less than or equal to 50%, the adhesion force between the first diaphragm and the first negative electrode sheet can be larger, so that the possibility of the first negative electrode sheet being separated from the first diaphragm is smaller, thereby reducing the possibility of the outer shell receiving an excessive impulse and cracking, and reducing the possibility of other electrode sheets other than the first negative electrode sheet colliding with the outer shell and being damaged or even short-circuiting; therefore, when 10%≤c≤50%, the impulse transmitted by the external force to the first positive electrode sheet can be smaller, thereby reducing the possibility of tearing of the electrode assembly, and reducing the possibility of the first negative electrode sheet being separated from the first diaphragm, thereby reducing the possibility of the outer shell receiving an excessive impulse and cracking, and reducing the possibility of other electrode sheets other than the first negative electrode sheet colliding with the outer shell and being damaged or even short-circuiting.

[0032] In some embodiments of the present application, the electrode assembly also includes a second positive electrode sheet, a second negative electrode sheet and a second diaphragm, the second negative electrode sheet is bonded to the second end wall through a fourth adhesive layer, the second positive electrode sheet is located on the side of the second negative electrode sheet facing away from the second end wall, and the second diaphragm is arranged between the second positive electrode sheet and the second negative electrode sheet; wherein, the bonding force of the fourth adhesive layer is F4, satisfying F4≥10N / m; the bonding force between the second negative electrode sheet and the second diaphragm is F5, and the bonding force between the second positive electrode sheet and the second diaphragm is F6, satisfying F5<F6.

[0033] In the above technical solution, by making the adhesion force F4 of the fourth adhesive layer between the second negative electrode sheet and the second end wall ≥ 10N / m, the adhesion force between the electrode assembly and the second end wall can be made larger, the impulse of the external force applied to the battery cell transmitted to the electrode assembly through the fourth adhesive layer is larger, and the possibility of cracking of the outer shell is smaller; by making the adhesion force F5 between the second negative electrode sheet and the second diaphragm and the adhesion force F6 between the second positive electrode sheet and the second diaphragm satisfy F5<F6, the adhesion force between the second negative electrode sheet and the second diaphragm is smaller, the impulse transmitted to the second positive electrode sheet can be reduced, thereby reducing the possibility of tearing of the electrode assembly, making the possibility of failure of the battery cell due to force lower, which is beneficial to extending the service life of the battery cell.

[0034] In some embodiments of the present application, the shell also includes a side wall, which is arranged around the first end wall and connects the first end wall and the second end wall; the electrode assembly includes multiple side surfaces connected end to end, and a fifth bonding layer is arranged between at least one side surface and the side wall, and the electrode assembly is bonded to the side wall through the fifth bonding layer.

[0035] In the above technical solution, by arranging a fifth adhesive layer between at least one side of the electrode assembly and the side wall of the outer shell, the electrode assembly is bonded to the side wall through the fifth adhesive layer, which can further reduce the possibility of displacement of the electrode assembly relative to the outer shell and causing damage to the electrode assembly and the outer shell or even short circuit. It can also facilitate the assembly of the electrode assembly and the outer shell. When the battery cell is subjected to force, the fifth adhesive layer can absorb part of the impulse, thereby making the bonding force range of the first adhesive layer larger.

[0036] In some embodiments of the present application, the adhesive force of the fifth adhesive layer is F7, satisfying F7 ≥ 50 N / m.

[0037] In the above technical solution, by ensuring that the adhesion force F7 of the fifth adhesive layer satisfies F7 ≥ 50 N / m, the adhesion force between the electrode assembly and the side wall of the outer shell can be higher, which can further reduce the possibility of displacement of the electrode assembly relative to the outer shell, causing damage to the electrode assembly and the outer shell or even a short circuit.

[0038] In some embodiments of the present application, the ratio of the length of each fifth adhesive layer to the length of the side surface where the fifth adhesive layer is located is between 40% and 80%.

[0039] In the above technical scheme, when the ratio of the length of each fifth adhesive layer to the length of the side where the fifth adhesive layer is located is greater than or equal to 40%, the bonding area between the electrode assembly and the side wall of the outer shell can be larger, and the bonding force between the electrode assembly and the side wall of the outer shell can be higher, which can further reduce the possibility of displacement of the electrode assembly relative to the outer shell, causing damage to the electrode assembly and the outer shell by collision or even short circuit; when the ratio of the length of each fifth adhesive layer to the length of the side where the fifth adhesive layer is located is less than or equal to 80%, the influence on the penetration of the electrolyte can be reduced, and the possibility of low process quality of the battery cell caused by curling of the fifth adhesive layer can be reduced; therefore, when the ratio of the length of each fifth adhesive layer to the length of the side where the fifth adhesive layer is located is between 40% and 80%, it can not only further reduce the possibility of displacement of the electrode assembly relative to the outer shell, causing damage to the electrode assembly and the outer shell by collision or even short circuit, but also reduce the influence on the penetration of the electrolyte, and the possibility of low process quality of the battery cell caused by curling of the fifth adhesive layer can be reduced.

[0040] In some embodiments of the present application, the outer shell is a hard shell.

[0041] In the above technical solution, the outer shell is a hard shell, which can prevent external force from directly acting on the electrode assembly, so that the outer shell can better protect the electrode assembly.

[0042] In some embodiments of the present application, the electrode assembly is a laminated structure.

[0043] In a second aspect, an embodiment of the present application provides an electrical device, including a battery cell as described above, and the battery cell is used to provide electrical energy. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can also be obtained based on these drawings.

[0045] Figure 1 A schematic cross-sectional view of a battery cell provided in some embodiments of the present application;

[0046] Figure 2 A schematic cross-sectional view of a battery cell provided in some other embodiments of the present application;

[0047] Figure 3 A schematic diagram of the structure of a first diaphragm of a battery cell provided in some other embodiments of the present application;

[0048] Figure 4 A schematic cross-sectional structure diagram of a first diaphragm of a battery cell provided in some embodiments of the present application;

[0049] Figure 5 A schematic cross-sectional structure diagram of a battery cell from another perspective provided in some embodiments of the present application;

[0050] Figure 6 Schematic diagram of the cross-sectional structure of the battery cell provided in some other embodiments of the present application.

[0051] Icon: 10-battery core; 100-housing; 110-first end wall; 120-second end wall; 130-side wall; 200-electrode assembly; 210-first positive electrode plate; 211-positive electrode current collector; 212-first positive electrode active material layer; 213-second positive electrode active material layer; 220-first negative electrode plate; 221-negative electrode current collector; 222-negative electrode active material layer; 222a-groove; 230-first separator Membrane; 231-base layer; 232-second bonding layer; 233-second bonding layer; 240-second positive electrode sheet; 250-second negative electrode sheet; 260-second diaphragm; 270-third positive electrode sheet; 280-third negative electrode sheet; 290-third diaphragm; 310-first bonding layer; 320-fourth bonding layer; 330-fifth bonding layer; X-thickness direction of the electrode assembly; Y-first direction; Z-second direction. DETAILED DESCRIPTION

[0052] In order to make the purpose, technical solutions and advantages of the present application clearer, the technical solutions in the embodiments of the present application will be clearly described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of this application.

[0053] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by technicians in the technical field to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0054] The terms "first", "second", etc. in the specification and claims of this application or the above-mentioned drawings are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship.

[0055] Reference to "embodiment" in this application means that a particular feature, structure, or characteristic described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments.

[0056] In the embodiments of the present application, the same reference numerals represent the same components, and for the sake of brevity, detailed descriptions of the same components are omitted in different embodiments. It should be understood that the thickness, length, width and other dimensions of various components in the embodiments of the present application shown in the drawings, as well as the overall thickness, length, width and other dimensions of the integrated device are only exemplary descriptions and should not constitute any limitation to the present application.

[0057] With the development of the new energy industry, batteries are gradually developing in the direction of high energy density and high power density. When the battery cell is subjected to external force, the battery cell shell and electrode assembly are more likely to be damaged and fail. The electrode assembly in the steel shell battery cell is generally bonded to the shell with adhesive tape. If the adhesive force of the adhesive tape is large, when the steel shell battery cell is subjected to force, the external force is transmitted to the electrode assembly through the adhesive tape with a large impulse, and the shell is not easy to crack, but the electrode assembly is easy to tear; if the adhesive force of the adhesive tape is small, the external force is transmitted to the electrode assembly through the adhesive tape with a small impulse, and the electrode assembly is not easy to tear, but the shell is easy to crack. The above two failure modes are difficult to balance, resulting in a higher possibility of failure of the steel shell battery cell when it is subjected to force.

[0058] In order to reduce the possibility of failure of a battery cell due to stress, the present application provides a battery cell, which includes a shell and an electrode assembly, wherein the electrode assembly is accommodated in the shell, and the shell includes a first end wall and a second end wall arranged opposite to each other along the thickness direction of the electrode assembly; the electrode assembly includes a first positive electrode sheet, a first negative electrode sheet and a first diaphragm, wherein the first negative electrode sheet is bonded to the first end wall through a first adhesive layer, the first positive electrode sheet is located on the side of the first negative electrode sheet facing away from the first end wall, and the first diaphragm is arranged between the first positive electrode sheet and the first negative electrode sheet; wherein the adhesive force of the first adhesive layer is F1, satisfying F1≥10N / m; the adhesive force between the first negative electrode sheet and the first diaphragm is F2, and the adhesive force between the first positive electrode sheet and the first diaphragm is F3, satisfying F2<F3. It should be noted that the adhesive force included in the first adhesive layer is divided into three types: ① the adhesive force between the first end wall and the first adhesive layer; ② the cohesive force of the first adhesive layer; ③ the adhesive force between the first adhesive layer and the first negative electrode sheet. Here, the bonding force of the first bonding layer refers to the lowest bonding force of the first bonding layer, that is, the bonding force corresponding to the earliest separated interface.

[0059] In a battery cell of this structure, the battery cell includes a shell and an electrode assembly, and the electrode assembly is accommodated in the shell so that the shell can protect the electrode assembly; by making the adhesion force F1 of the first adhesive layer between the first negative electrode plate and the first end wall ≥ 10N / m, the adhesion force between the electrode assembly and the first end wall can be made larger, the impulse of the external force applied to the battery cell transmitted to the electrode assembly through the first adhesive layer is larger, and the possibility of cracking of the shell is smaller; by making the adhesion force F2 between the first negative electrode plate and the first diaphragm and the adhesion force F3 between the first positive electrode plate and the first diaphragm satisfy F2<F3, the adhesion force between the first negative electrode plate and the first diaphragm is smaller, the impulse transmitted to the first positive electrode plate can be reduced, thereby reducing the possibility of tearing of the electrode assembly, making the possibility of failure of the battery cell due to force lower, which is beneficial to extending the service life of the battery cell.

[0060] The battery cell provided in the embodiment of the present application can be a secondary battery or a primary battery, for example, a lithium ion battery, a sodium ion battery or a magnesium ion battery, etc., which is not limited in the embodiment of the present application. The electrochemical device can be cylindrical, flat, rectangular or other shapes, etc., which is not limited in the embodiment of the present application.

[0061] The embodiments of the present application provide an electrical device that uses a battery cell as a power source. The electrical device may be, but is not limited to, a mobile phone, a tablet, a laptop computer, an electric toy, an electric tool, an electric vehicle, an electric car, a ship, a spacecraft, and the like.

[0062] See also Figure 1 , Figure 1 A schematic diagram of the cross-sectional structure of a battery cell provided in some embodiments of the present application.

[0063] The embodiment of the present application provides a battery cell 10, which includes a housing 100 and an electrode assembly 200. The electrode assembly 200 is accommodated in the housing 100, and the housing 100 includes a first end wall 110 and a second end wall 120 that are arranged opposite to each other along the thickness direction X of the electrode assembly 200. The electrode assembly 200 includes a first positive electrode sheet 210, a first negative electrode sheet 220, and a first separator 230. The first negative electrode sheet 220 is bonded to the first end wall 110 through a first adhesive layer 310. The first positive electrode sheet 210 is located on a side of the first negative electrode sheet 220 that faces away from the first end wall 110, and the first separator 230 is arranged between the first positive electrode sheet 210 and the first negative electrode sheet 220.

[0064] By accommodating the electrode assembly 200 in the housing 100 , the housing 100 can protect the electrode assembly 200 .

[0065] In some embodiments, the battery cell 10 is arranged in a square shape.

[0066] In some embodiments, the adhesion force of the first adhesive layer 310 is F1, satisfying F1≥10N / m. The adhesion force between the first negative electrode plate 220 and the first separator 230 is F2, and the adhesion force between the first positive electrode plate 210 and the first separator 230 is F3, satisfying F2<F3. For example, F1 can be 10N / m, 20N / m or 50N / m, etc. For example, F2 can be 0.9*F3, 0.7*F3 or 0.5*F3, etc.

[0067] By ensuring that the bonding force F1 of the first bonding layer 310 between the first negative electrode plate 220 and the first end wall 110 is ≥10 N / m, the bonding force between the electrode assembly 200 and the first end wall 110 can be made larger, and the external force can be transmitted to the electrode assembly 200 through the first bonding layer 310 to absorb more impulse. The external force applied to the battery cell 10 has a larger impulse transmitted to the electrode assembly 200 through the first bonding layer 310, and the possibility of cracking of the outer shell 100 is smaller. By making the adhesion force F2 between the first negative electrode sheet 220 and the first diaphragm 230, and the adhesion force F3 between the first positive electrode sheet 210 and the first diaphragm 230 satisfy F2<F3, the adhesion force between the first negative electrode sheet 220 and the first diaphragm 230 is made smaller, so that the impulse transmitted to the first positive electrode sheet 210 can be reduced. Since in general, the thickness of the negative electrode sheet is greater than that of the positive electrode sheet, when the battery cell 10 is subjected to force, the negative electrode sheet is less likely to tear than the positive electrode sheet. Therefore, by setting the first negative electrode sheet 220 at the outermost side of the electrode assembly 200, and making more impulse of the external force be transmitted to the first negative electrode sheet 220, and less impulse be transmitted to the first positive electrode sheet 210 and other sheets, it is possible that each sheet of the electrode assembly 200 is not easily torn, thereby reducing the possibility of tearing of the electrode assembly 200. Therefore, by making F1 ≥ 10 N / m and F2 < F3, the possibility of cracking of the shell 100 when the battery cell 10 is subjected to force can be reduced, and the possibility of tearing of the electrode assembly 200 when the battery cell 10 is subjected to force can be reduced, so that the possibility of failure of the battery cell 10 due to force is low, which is conducive to extending the service life of the battery cell 10. Therefore, in the above scheme, it can be ensured that when the bonding force is large, the problem of electrode tearing and causing failure of the battery cell due to force can be avoided.

[0068] In some embodiments, F3-F2≥5N / m. For example, F3-F2 may be 5N / m, 8N / m, or 10N / m.

[0069] By making F3-F2≥5N / m, the first negative electrode plate 220 and the first separator 230 can be separated more evenly, thereby further reducing the impulse transmitted to the first positive electrode plate 210, further reducing the possibility of tearing of the electrode assembly 200, and making the possibility of stress failure of the battery cell 10 lower, which is beneficial to extending the service life of the battery cell 10.

[0070] In some embodiments, 10 N / m≤F2≤95 N / m. For example, F2 may be 10 N / m, 50 N / m, or 95 N / m.

[0071] When F2 is greater than or equal to 10N / m, the first negative electrode sheet 220 is less likely to separate from the first diaphragm 230, thereby reducing the possibility of the outer shell 100 receiving an excessively large impulse and cracking, and reducing the possibility that the other sheets except the first negative electrode sheet 220 collide with the outer shell 100 to be damaged or even short-circuited; when F2 is less than or equal to 95N / m, the impulse transmitted to the first positive electrode sheet 210 by the external force is less, thereby further reducing the possibility of the electrode assembly 200 being torn; therefore, when 10N / m≤F2≤95N / m, the first negative electrode sheet 220 is less likely to separate from the first diaphragm 230, thereby reducing the possibility of the outer shell 100 receiving an excessively large impulse and cracking, and reducing the possibility that the other sheets except the first negative electrode sheet 220 collide with the outer shell 100 to be damaged or even short-circuited, and reducing the impulse transmitted to the first positive electrode sheet 210 by the external force, thereby further reducing the possibility of the electrode assembly 200 being torn.

[0072] In some embodiments, 15 N / m≤F3≤100 N / m. For example, F3 may be 15 N / m, 60 N / m, or 100 N / m.

[0073] When F3 is greater than or equal to 15 N / m, the first diaphragm 230 is less likely to separate from the first positive electrode sheet 210, thereby reducing the possibility that the outer shell 100 receives an excessively large impulse and cracks, and also reducing the possibility that the other sheets except the first negative electrode sheet 220 collide with the outer shell 100 to be damaged or even short-circuited; when F3 is less than or equal to 100 N / m, the impulse transmitted to the first positive electrode sheet 210 by the external force is less, thereby reducing the possibility that the electrode assembly 200 is torn; therefore, when 15 N / m≤F3≤100 N / m, the first diaphragm 230 is less likely to separate from the first positive electrode sheet 210, thereby reducing the possibility that the outer shell 100 receives an excessively large impulse and cracks, and also reducing the possibility that the other sheets except the first negative electrode sheet 220 collide with the outer shell 100 to be damaged or even short-circuited, and also reducing the impulse transmitted to the first positive electrode sheet 210 by the external force, thereby reducing the possibility that the electrode assembly 200 is torn.

[0074] See also Figure 2 and Figure 3 , Figure 2 A schematic cross-sectional view of a battery cell provided in some other embodiments of the present application; Figure 3 A schematic structural diagram of the first diaphragm of a battery cell provided in some other embodiments of the present application.

[0075] In other embodiments, the first negative electrode plate 220 includes a negative electrode collector 221 and a negative electrode active material layer 222 , the negative electrode active material layer 222 is arranged on the side of the negative electrode collector 221 facing the first positive electrode plate 210 , and a groove 222 a is provided on the side of the negative electrode active material layer 222 facing the first separator 230 .

[0076] By disposing the negative electrode active material layer 222 on the side of the negative electrode collector 221 facing the first positive electrode plate 210, and providing a groove 222a on the side of the negative electrode active material layer 222 facing the first separator 230, the bonding area between the negative electrode active material layer 222 and the first separator 230 can be made smaller, thereby making the bonding force between the negative electrode active material layer 222 and the first separator 230 smaller, and reducing the impulse transmitted to the first positive electrode plate 210, thereby reducing the possibility of tearing of the electrode assembly 200, and reducing the possibility of force failure of the battery cell 10, which is beneficial to extending the service life of the battery cell 10.

[0077] In some embodiments, the projection area of ​​the groove 222a in the thickness direction of the first negative electrode sheet 220 is S1, and the projection area of ​​the negative active material layer 222 in the thickness direction of the first negative electrode sheet 220 is S2, which satisfies 5%≤S1 / S2≤35%. For example, S1 / S2 can be 5%, 15%, or 35%.

[0078] When S1 / S2 is greater than or equal to 5%, the bonding area between the negative electrode active material layer 222 and the first separator 230 can be smaller, so that the bonding force between the negative electrode active material layer 222 and the first separator 230 is smaller, which can reduce the impulse transmitted to the first positive electrode plate 210, thereby reducing the possibility of tearing of the electrode assembly 200; when S1 / S2 is less than or equal to 35%, the bonding area between the negative electrode active material layer 222 and the first separator 230 can be larger, so that the bonding force between the negative electrode active material layer 222 and the first separator 230 is larger, which can reduce the possibility of the first negative electrode plate 220 detaching from the first separator 230, thereby The possibility of the outer shell 100 receiving an excessive impulse and cracking is reduced, and the possibility of other pole pieces except the first negative pole piece 220 colliding with the outer shell 100 to be damaged or even short-circuited is reduced; therefore, when 5%≤S1 / S2≤35%, it can not only reduce the impulse transmitted to the first positive pole piece 210, thereby reducing the possibility of the electrode assembly 200 being torn, but also reduce the possibility of the first negative pole piece 220 being separated from the first diaphragm 230, thereby reducing the possibility of the outer shell 100 receiving an excessive impulse and cracking, but also reduce the possibility of other pole pieces except the first negative pole piece 220 colliding with the outer shell 100 to be damaged or even short-circuited.

[0079] In some embodiments, the groove 222a extends along the first direction Y, the width of the groove 222a along the second direction Z is W1, and the width of the negative active material layer 222 along the second direction Z is W2, which satisfies 5%≤W1 / W2≤35%. For example, W1 / W2 can be 5%, 15% or 35%.

[0080] In some embodiments, the thickness direction X, the first direction Y, and the second direction Z of the electrode assembly 200 are perpendicular to each other.

[0081] In some embodiments, a plurality of grooves 222 a are disposed on the first diaphragm 222 , and W1 is the sum of the widths of the plurality of grooves 222 a along the second direction Z.

[0082] When W1 / W2 is greater than or equal to 5%, the bonding area between the negative electrode active material layer 222 and the first diaphragm 230 can be smaller, so that the bonding force between the negative electrode active material layer 222 and the first diaphragm 230 is smaller, and the impulse transmitted to the first positive electrode plate 210 can be reduced, thereby reducing the possibility of tearing of the electrode assembly 200; when W1 / W2 is less than or equal to 35%, the bonding area between the negative electrode active material layer 222 and the first diaphragm 230 can be larger, so that the bonding force between the negative electrode active material layer 222 and the first diaphragm 230 is larger, and the possibility of the first negative electrode plate 220 being separated from the first diaphragm 230 is smaller, so that the possibility of the outer shell 100 receiving an excessively large impulse and cracking is smaller, and the outer shell 100 other than the first negative electrode plate 220 can be The possibility of other pole pieces colliding with the shell 100 and being damaged or even short-circuited is small, and the possibility of the first diaphragm 230 extending into the groove 222a and adhering to the side wall of the groove 222a can be reduced; therefore, when 5%≤W1 / W2≤35%, it is possible to reduce the impulse transmitted to the first positive pole piece 210, thereby reducing the possibility of tearing of the electrode assembly 200, and the possibility of the first negative pole piece 220 being separated from the first diaphragm 230 is small, thereby reducing the possibility of the shell 100 receiving excessive impulse and cracking, and the possibility of other pole pieces except the first negative pole piece 220 colliding with the shell 100 and being damaged or even short-circuited is small, and the possibility of the first diaphragm 230 extending into the groove 222a and adhering to the side wall of the groove 222a can be reduced.

[0083] In some embodiments, the first positive electrode plate 210 includes a positive electrode current collector 211, a first positive electrode active material layer 212, and a second positive electrode active material layer 213. The first positive electrode active material layer 212 is disposed on the side of the positive electrode current collector 211 facing the first negative electrode plate 220, and the second positive electrode active material layer 213 is disposed on the side of the positive electrode current collector 211 facing away from the first negative electrode plate 220. The first positive electrode active material layer 212 is disposed in a plane on the side facing the first separator 230.

[0084] By arranging the first positive electrode active material layer 212 in a plane facing the side of the first separator 230, the bonding area between the first positive electrode active material layer 212 and the first separator 230 can be made larger, thereby increasing the bonding force between the first positive electrode active material layer 212 and the first separator 230, and reducing the possibility of the first negative electrode plate 220 and the first separator 230 being separated from the first positive electrode plate 210, thereby reducing the possibility of the outer shell 100 receiving an excessive impulse and cracking, and reducing the possibility of other plates except the first negative electrode plate 220 colliding with the outer shell 100 to be damaged or even short-circuited.

[0085] See also Figure 1 In some embodiments, the first negative electrode plate 220 includes a negative electrode current collector 221 and a negative electrode active material layer 222. The negative electrode active material layer 222 is disposed on the side of the negative electrode current collector 221 facing the first positive electrode plate 210. The negative electrode active material layer 222 includes a first adhesive, and the content of the first adhesive in the negative electrode active material layer 222 is 0.3% to 0.8%. For example, the content of the first adhesive in the negative electrode active material layer 222 may be 0.3%, 0.5% or 0.8%.

[0086] When the content of the first binder in the negative electrode active material layer 222 is greater than or equal to 0.3%, the bonding force between the negative electrode active material layer 222 and the first diaphragm 230 can be greater, and the possibility of the first negative electrode plate 220 being separated from the first diaphragm 230 can be reduced, so that the possibility of the outer shell 100 receiving an excessive impulse and cracking is reduced, and the possibility of other plates except the first negative electrode plate 220 colliding with the outer shell 100 and being damaged or even short-circuited can be reduced; when the content of the first binder in the negative electrode active material layer 222 is less than or equal to 0.8%, the bonding force between the negative electrode active material layer 222 and the first diaphragm 230 can be smaller, and the impulse transmitted to the first positive electrode plate 210 can be reduced. Because in general, the thickness of the negative electrode plate is greater than that of the positive electrode plate, when the battery cell is subjected to force, the negative electrode plate is less likely to tear than the positive electrode plate. By arranging the first negative electrode plate 220 at the outermost side of the electrode assembly 200, and transmitting more impulse of the external force to the first negative electrode plate 220, and transmitting less impulse to the first positive electrode plate 210 and other plates, it is possible to prevent each plate of the electrode assembly 200 from being easily torn, thereby reducing the possibility of tearing of the electrode assembly 200; therefore, when the content of the first adhesive in the negative electrode active material layer 222 is 0.3% to 0.8%, it is possible to reduce the possibility of the first negative electrode plate 220 being separated from the first diaphragm 230, thereby reducing the possibility of the outer shell 100 receiving excessive impulse and cracking, and it is possible to reduce the possibility of other plates except the first negative electrode plate 220 colliding with the outer shell 100 and being damaged or even short-circuited, and it is possible to reduce the impulse transmitted to the first positive electrode plate 210, thereby reducing the possibility of tearing of the electrode assembly 200.

[0087] In some embodiments, the first positive electrode plate 210 includes a positive electrode current collector 211, a first positive electrode active material layer 212, and a second positive electrode active material layer 213. The first positive electrode active material layer 212 is disposed on the side of the positive electrode current collector 211 facing the first negative electrode plate 220, and the second positive electrode active material layer 213 is disposed on the side of the positive electrode current collector 211 facing away from the first negative electrode plate 220. The first positive electrode active material layer 212 includes a second adhesive, and the content of the second adhesive in the first positive electrode active material layer 212 is 0.8% to 2%. For example, the content of the second adhesive in the first positive electrode active material layer 212 may be 0.8%, 1.2%, or 2%, etc.

[0088] When the content of the second adhesive in the first positive electrode active material layer 212 is greater than or equal to 0.8%, the bonding force between the first positive electrode active material layer 212 and the first separator 230 can be greater, the possibility of the first positive electrode plate 210 being separated from the first separator 230 can be reduced, and the possibility of other plates except the first negative electrode plate 220 being damaged by collision with the shell 100 or even short-circuited can be reduced; when the content of the second adhesive in the first positive electrode active material layer 212 is less than or equal to 2%, the bonding force between the first positive electrode active material layer 212 and the first separator 230 can be greater. The smaller the adhesive force, the less impulse transmitted to the first positive electrode sheet 210 can be, thereby reducing the possibility of tearing of the electrode assembly 200; therefore, when the content of the second adhesive in the first positive electrode active material layer 212 is 0.8% to 2%, it can reduce the possibility of the first positive electrode sheet 210 being separated from the first diaphragm 230, thereby reducing the possibility of other sheets except the first negative electrode sheet 220 being damaged by collision with the outer shell 100 or even short-circuiting, and can reduce the impulse transmitted to the first positive electrode sheet 210, thereby reducing the possibility of tearing of the electrode assembly 200.

[0089] In some embodiments, the first separator 230 includes a base layer 231, a second adhesive layer 232 and a third adhesive layer 233, the second adhesive layer 232 is disposed on the side of the base layer 231 facing the first negative electrode sheet 220, the third adhesive layer 233 is disposed on the side of the base layer 231 facing the first positive electrode sheet 210, the second adhesive layer 232 includes a third adhesive, the content of the third adhesive in the second adhesive layer 232 is a, the third adhesive layer 233 includes a fourth adhesive, the content of the fourth adhesive in the third adhesive layer 233 is b, and a<b is satisfied. For example, a can be 0.9*b, 0.7*b or 0.5*b, etc.

[0090] By ensuring that the content a of the third adhesive in the second adhesive layer 232 and the content b of the fourth adhesive in the third adhesive layer 233 satisfy a<b, the bonding force between the first diaphragm 230 and the first negative electrode plate 220 can be made smaller than the bonding force between the first diaphragm 230 and the first positive electrode plate 210, thereby reducing the impulse transmitted to the first positive electrode plate 210 and reducing the possibility of tearing of the electrode assembly 200, thereby reducing the possibility of stress failure of the battery cell 10 and helping to extend the service life of the battery cell 10.

[0091] In some embodiments, 45%≤a≤85%. For example, a may be 45%, 65%, or 85%.

[0092] When a is greater than or equal to 45%, the bonding force between the first diaphragm 230 and the first negative electrode sheet 220 can be relatively large, so that the first negative electrode sheet 220 is less likely to be separated from the first diaphragm 230, thereby reducing the possibility that the shell 100 receives an excessively large impulse and cracks, and also reducing the possibility that other sheets except the first negative electrode sheet 220 collide with the shell 100 and are damaged or even short-circuited; when a is less than or equal to 85%, the bonding force between the first diaphragm 230 and the first negative electrode sheet 220 can be relatively small, so that the external force is transmitted to the first positive electrode sheet The impulse of 210 is small, so that the possibility of tearing of the electrode assembly 200 is small; therefore, when 45%≤a≤85%, it can not only reduce the possibility of the first negative electrode plate 220 separating from the first diaphragm 230, but also reduce the possibility of the outer shell 100 receiving too much impulse and cracking, but also reduce the possibility of other plates except the first negative electrode plate 220 colliding with the outer shell 100 and being damaged or even short-circuited, and can also reduce the impulse transmitted to the first positive electrode plate 210 by the external force, so that the possibility of tearing of the electrode assembly 200 is small.

[0093] See also Figure 1 and Figure 4 , Figure 4 A schematic diagram of the cross-sectional structure of the first diaphragm of the battery cell provided in some embodiments of the present application.

[0094] In some embodiments, the first separator 230 includes a base layer 231, a second adhesive layer 232 and a third adhesive layer 233, the second adhesive layer 232 is disposed on the side of the base layer 231 facing the first negative electrode sheet 220, the third adhesive layer 233 is disposed on the side of the base layer 231 facing the first positive electrode sheet 210, the second adhesive layer 232 includes a first ceramic material, the content of the first ceramic material in the second adhesive layer 232 is c, the third adhesive layer 233 includes a second ceramic material, the content of the second ceramic material in the third adhesive layer 233 is d, and c>d is satisfied. For example, c can be 1.1*d, 1.5*d or 2*d, etc.

[0095] By ensuring that the content c of the first ceramic material in the second adhesive layer 232 and the content d of the second ceramic material in the third adhesive layer 233 satisfy c>d, the bonding force between the first diaphragm 230 and the first negative electrode plate 220 can be made smaller than the bonding force between the first diaphragm 230 and the first positive electrode plate 210, thereby reducing the impulse transmitted to the first positive electrode plate 210 and reducing the possibility of tearing of the electrode assembly 200, thereby reducing the possibility of stress failure of the battery cell 10 and helping to extend the service life of the battery cell 10.

[0096] In other embodiments, the first diaphragm 230 may also only include the second adhesive layer 232 and the third adhesive layer 233 .

[0097] In some embodiments, 10%≤c≤50%. For example, c can be 10%, 30%, or 50%.

[0098] When c is greater than or equal to 10%, the bonding force between the first diaphragm 230 and the first negative electrode sheet 220 can be small, so that the impulse transmitted to the first positive electrode sheet 210 by the external force is small, so that the possibility of tearing of the electrode assembly 200 is small; when c is less than or equal to 50%, the bonding force between the first diaphragm 230 and the first negative electrode sheet 220 can be large, so that the possibility of the first negative electrode sheet 220 being separated from the first diaphragm 230 is small, so that the possibility of the shell 100 receiving an excessive impulse and cracking is small, and the first negative electrode sheet 210 can be small. The possibility that other pole pieces other than the first positive pole piece 220 collide with the outer shell 100 and are damaged or even short-circuited is small; therefore, when 10%≤c≤50%, the impulse transmitted by the external force to the first positive pole piece 210 can be reduced, thereby reducing the possibility of tearing of the electrode assembly 200, and the possibility that the first negative pole piece 220 is separated from the first diaphragm 230 can be reduced, thereby reducing the possibility that the outer shell 100 receives excessive impulse and cracks, and the possibility that other pole pieces other than the first negative pole piece 220 collide with the outer shell 100 and are damaged or even short-circuited is reduced.

[0099] See also Figure 1 In some embodiments, the electrode assembly 200 further includes a second positive electrode sheet 240, a second negative electrode sheet 250 and a second separator 260, the second negative electrode sheet 250 is bonded to the second end wall 120 through a fourth adhesive layer 320, the second positive electrode sheet 240 is located on the side of the second negative electrode sheet 250 facing away from the second end wall 120, and the second separator 260 is disposed between the second positive electrode sheet 240 and the second negative electrode sheet 250; wherein the bonding force of the fourth adhesive layer 320 is F4, satisfying F4≥10N / m. The bonding force between the second negative electrode sheet 250 and the second separator 260 is F5, and the bonding force between the second positive electrode sheet 240 and the second separator 260 is F6, satisfying F5<F6. For example, F4 may be 10N / m, 20N / m or 50N / m, etc. For example, F5 may be 0.9*F6, 0.7*F6 or 0.5*F6, etc.

[0100] By making the adhesive force F4 of the fourth adhesive layer 320 between the second negative electrode sheet 250 and the second end wall 120 ≥ 10 N / m, the adhesive force between the electrode assembly 200 and the second end wall 120 can be made larger, the impulse of the external force on the battery cell 10 transmitted to the electrode assembly 200 through the fourth adhesive layer 320 is larger, and the possibility of the shell 100 cracking is smaller. By making the adhesive force F5 between the second negative electrode sheet 250 and the second diaphragm 260 and the adhesive force F6 between the second positive electrode sheet 240 and the second diaphragm 260 satisfy F5 < F6, the adhesive force between the second negative electrode sheet 250 and the second diaphragm 260 is smaller, the impulse transmitted to the second positive electrode sheet 240 can be reduced, and thus the possibility of the electrode assembly 200 tearing can be reduced. Therefore, by making F4 ≥ 10 N / m and F5 < F6, the possibility of cracking of the outer casing 100 when the battery cell 10 is subjected to stress can be reduced, and the possibility of tearing of the electrode assembly 200 when the battery cell 10 is subjected to stress can be reduced, so that the possibility of failure of the battery cell 10 due to stress is lower, which is beneficial to extending the service life of the battery cell 10.

[0101] See also Figure 1 and Figure 5 , Figure 5 A schematic diagram of a cross-sectional structure of a battery cell from another perspective provided in some embodiments of the present application.

[0102] In some embodiments, the housing 100 further includes a side wall 130, which is disposed around the first end wall 110, and the side wall 130 connects the first end wall 110 and the second end wall 120. The electrode assembly 200 includes a plurality of side surfaces 270 connected end to end, and a fifth adhesive layer 330 is disposed between at least one side surface 270 and the side wall 130, and the electrode assembly 200 is bonded to the side wall 130 through the fifth adhesive layer 330.

[0103] By setting a fifth adhesive layer 330 between at least one side surface 270 of the electrode assembly 200 and the side wall 130 of the outer shell 100, the electrode assembly 200 is bonded to the side wall 130 through the fifth adhesive layer 330, which can further reduce the possibility of displacement of the electrode assembly 200 relative to the outer shell 100 and causing damage to the electrode assembly 200 and the outer shell 100 or even a short circuit. It can also facilitate the assembly of the electrode assembly 200 and the outer shell 100, and when the battery cell 10 is subjected to force, the fifth adhesive layer 330 can absorb part of the impulse, thereby making the bonding force range of the first adhesive layer 310 larger.

[0104] In some embodiments, the adhesive force of the fifth adhesive layer 330 is F7, satisfying F7 ≥ 50 N / m. For example, F7 may be 50 N / m, 80 N / m, or 1000 N / m.

[0105] By ensuring that the adhesion force F7 of the fifth adhesive layer 330 satisfies F7 ≥ 50 N / m, the adhesion force between the electrode assembly 200 and the side wall 130 of the outer shell 100 can be increased, which can further reduce the possibility of displacement of the electrode assembly 200 relative to the outer shell 100, causing collision damage or even short circuit between the electrode assembly 200 and the outer shell 100.

[0106] In some embodiments, the ratio of the length of each fifth adhesive layer 330 to the length of the side surface 270 where the fifth adhesive layer 330 is located is between 40% and 80%. For example, the ratio of the length of each fifth adhesive layer 330 to the length of the side surface 270 where the fifth adhesive layer 330 is located can be 40%, 60% or 80%.

[0107] When the ratio of the length of each fifth adhesive layer 330 to the length of the side surface 270 where the fifth adhesive layer 330 is located is greater than or equal to 40%, the bonding area between the electrode assembly 200 and the side wall 130 of the housing 100 can be larger, and the bonding force between the electrode assembly 200 and the side wall 130 of the housing 100 is higher, which can further reduce the possibility of the electrode assembly 200 being displaced relative to the housing 100 and causing the electrode assembly 200 to collide with the housing 100, be damaged, or even short-circuit. When the ratio of the length of each fifth adhesive layer 330 to the length of the side surface 270 where the fifth adhesive layer 330 is located is less than or equal to 80%, the bonding area between the electrode assembly 200 and the side wall 130 of the housing 100 can be larger, and the bonding force between the electrode assembly 200 and the side wall 130 of the housing 100 can be higher, and the possibility of the electrode assembly 200 being displaced relative to the housing 100 and causing the electrode assembly 200 to collide with the housing 100, be damaged, or even short-circuit can be further reduced. %, can reduce the influence on the penetration of the electrolyte, and can reduce the possibility of the fifth adhesive layer 330 curling up and causing the process quality rate of the battery cell 10 to be low; therefore, when the ratio of the length of each fifth adhesive layer 330 to the length of the side 270 where the fifth adhesive layer 330 is located is between 40% and 80%, it can not only further reduce the possibility of the electrode assembly 200 being displaced relative to the outer shell 100 and causing the electrode assembly 200 to collide with the outer shell 100 and be damaged or even short-circuited, but also reduce the influence on the penetration of the electrolyte, and can reduce the possibility of the fifth adhesive layer 330 curling up and causing the process quality rate of the battery cell 10 to be low.

[0108] See also Figure 1 In some embodiments, the battery cell 10 further includes a plurality of third positive electrode sheets 270, a plurality of third negative electrode sheets 280 and a plurality of third diaphragms 290. The plurality of third positive electrode sheets 270 and the plurality of third negative electrode sheets 280 are alternately arranged between the first positive electrode sheet 210 and the second positive electrode sheet 220, and the third diaphragm 290 is arranged between the third positive electrode sheet 270 and the third negative electrode sheet 280.

[0109] See also Figure 5In some embodiments, the battery cell 10 includes a first electrode terminal 410 and a second electrode terminal 420, and the first electrode terminal 410 and the second electrode terminal 420 are arranged on one of the side walls 130, the first electrode terminal 410 is connected to the first positive electrode sheet 210, the second positive electrode sheet 240 and the third positive electrode sheet 270, and the second electrode terminal 420 is connected to the first negative electrode sheet 220, the second negative electrode sheet 250 and the third negative electrode sheet 280, and the fifth adhesive layer 330 is not arranged between the side wall 130 where the first electrode terminal 410 and the second electrode terminal 420 are arranged and the electrode assembly 200, which can avoid the first electrode terminal 410 and the second electrode terminal 410, reduce the impact on the electrical connection between the first electrode terminal 410 and the positive electrode sheet, the second electrode terminal 420 and the negative electrode sheet, and reduce the impact on the electrical connection between the first electrode terminal 410 and the second electrode terminal 420 and the load.

[0110] See also Figure 6 , Figure 6 Schematic diagram of the cross-sectional structure of the battery cell provided in some other embodiments of the present application.

[0111] In other embodiments, the battery cell 10 may also be arranged in a special shape, such as an L shape. A first adhesive layer 310 is arranged between the first end wall 110 of the housing 100 and the electrode assembly 200, a second adhesive layer 320 is arranged between the second end wall 120 and the electrode assembly 200, and a fifth adhesive layer 330 is arranged between the plurality of side walls 130 of the housing 100 and the electrode assembly 200.

[0112] In some embodiments, housing 100 is a hard shell.

[0113] In the above technical solution, the outer shell 100 is a hard shell, which can prevent external force from directly acting on the electrode assembly 200, so that the outer shell 100 can better protect the electrode assembly 200.

[0114] In some embodiments, the electrode assembly 200 is a laminated structure.

[0115] Referring to Table 1, in Table 1, F1 is the bonding strength of the first bonding layer, F2 is the bonding strength between the first negative electrode plate and the first separator, and F3 is the bonding strength between the first positive electrode plate and the first separator.

[0116] The test method for adhesion is:

[0117] (1) Take a cell sample and charge it to the state of charge (SOC) = 100%;

[0118] (2) Disassemble the battery cell, cut off the excess shell around the battery cell, and place the battery cell in the test electrolyte, soak it in an oven at 85°C for 4 hours, and then take it out and air-dry it at room temperature;

[0119] (3) Connect the two sides of the tensile testing machine to the two parts of the battery cell whose adhesion is to be tested (for example, when testing the adhesion of the first adhesive layer, the two sides of the tensile testing machine are connected to the first negative electrode sheet and the first end wall respectively), the tensile speed is 50 mm / min, and the two sides are in a 90° direction to test the tensile force;

[0120] (4) Record and analyze the original FX (tension-displacement) data of the tensile testing machine, and record the average tension in the stable area / test sample width as the bonding force.

[0121] The test method for drop pass rate is:

[0122] (1) Fully charge the cell sample at 23±2°C, measure and record the open circuit voltage and battery impedance of the cell;

[0123] (2) The battery cell is dropped freely from a height of 1.5 m (measured from the lowest point of the battery cell to the falling surface) onto concrete for 30 rounds of drop test. The order of one round of drop is: front-back-bottom-top-left-right, upper left corner-upper right corner-lower left corner-lower right corner;

[0124] (3) Count and observe the appearance of the battery cells. The criteria for judging whether the battery cells have passed the drop test are as follows: the battery cells should not explode, emit smoke, catch fire or leak liquid within 1 hour after being dropped; the difference between the open circuit voltage of the battery cells and the initial value before the drop should not be greater than 50mV 24 hours after the drop.

[0125] Table 1

[0126]

[0127] The test method for pole piece tearing is:

[0128] (1) Fully charge the cell sample at 23±2°C, measure and record the open circuit voltage and battery impedance of the cell;

[0129] (2) The battery cell is dropped freely from a height of 1.5 m (measured from the lowest point of the battery cell to the falling surface) onto concrete for 30 rounds of drop test. The order of one round of drop is: front-back-bottom-top-left-right, upper left corner-upper right corner-lower left corner-lower right corner;

[0130] (3) Discharge the battery cell at a constant current of 0.2C to 3V;

[0131] (4) Disassemble the battery cell and determine whether there are cracks greater than or equal to 2 mm in the electrode. If the number of cracks exceeds one, it is determined that the electrode of the battery cell is torn. The electrode tear rate = the number of battery cells with torn electrode sheets / the total number of battery cells.

[0132] The test method for weld punching is:

[0133] (1) Fully charge the cell sample at 23±2°C, measure and record the open circuit voltage and battery impedance of the cell;

[0134] (2) The battery cell is dropped freely from a height of 1.5 m (measured from the lowest point of the battery cell to the falling surface) onto concrete for 30 rounds of drop test. The order of one round of drop is: front-back-bottom-top-left-right, upper left corner-upper right corner-lower left corner-lower right corner;

[0135] (3) Check the appearance of the battery cell to see if there are cracks larger than 1 mm on the battery cell shell. If there are more than one crack, it is considered that the weld of the battery cell has been broken.

[0136] (4) Use an organic volatile gas tester to test whether the organic volatile gas concentration around the battery cell exceeds a threshold value. If it exceeds the threshold value, it is determined that the weld of the battery cell has been broken; weld break rate = number of battery cells with broken welds / total number of battery cells.

[0137] The test method for the number of cycles is:

[0138] (1) Place the battery cell in an environment of 25±2℃, charge the battery cell at a constant current of 0.2C to the battery cell's charge cut-off voltage (e.g., 4.5V), charge the battery cell at a constant voltage of 0.025C, and then discharge the battery cell at a constant current of 0.2C to the battery cell's discharge cut-off voltage (e.g., 3.0V), which is recorded as one cycle of the battery cell;

[0139] (2) Record the number of cycles before black spots first appear on the battery cell.

[0140] According to Table 1, the following conclusions can be drawn:

[0141] 1. Referring to Comparative Example 1 and Examples 1-3, when the adhesion F1 of the first adhesive layer is greater than or equal to 10 N / m, the drop pass rate and the number of cycles of the battery cell are high, and the electrode tear rate and the weld open rate are low; when the adhesion F1 of the first adhesive layer is less than 10 N / m, the drop pass rate of the battery cell is low, the weld open rate is high, the battery cell is easily damaged by force, affecting the service life of the battery cell.

[0142] 2. Referring to Comparative Example 2 and Examples 4-7, when F2 is between 10 N / m and 95 N / m, the drop pass rate and cycle number of the battery cell are high, and the electrode tear rate and weld open rate are low; when F2 is less than 10 N / m, the drop pass rate and cycle number of the battery cell are low, the weld open rate is high, the battery cell is easily damaged by force, and the cycle life of the battery cell is affected; when F2 is greater than 95 N / m, the drop pass rate of the battery cell drops sharply, the electrode tear rate increases sharply, the battery cell is easily damaged by force, and the service life of the battery cell is affected.

[0143] 3. Referring to Comparative Example 4 and Examples 8-11, when F3 is between 15 N / m and 100 N / m, the drop pass rate and cycle number of the battery cell are high, and the electrode tear rate and weld open rate are low; when F3 is less than 15 N / m, the drop pass rate of the battery cell drops sharply, the electrode tear rate increases sharply, the battery cell is easily damaged by force, affecting the service life of the battery cell; when F3 is greater than 100 N / m, the cycle number of the battery cell drops sharply, affecting the cycle life of the battery cell.

[0144] 4. Referring to Comparative Examples 2-5 and Examples 12-14, when F3-F2 is greater than 0 N / m, the drop pass rate and cycle number of the battery cell are high, and the electrode tear rate and weld open rate are low; when F3-F2 is less than or equal to 0 N / m, the drop pass rate of the battery cell is low, the electrode tear rate is high, the battery cell is easily damaged by force, affecting the service life of the battery cell.

[0145] 5. Referring to Examples 15-18, when F7 is greater than or equal to 50 N / m, the drop pass rate and cycle number of the battery cell are high, and the electrode tear rate and weld open rate are low; when F7 is less than 50 N / m, the drop pass rate of the battery cell decreases, the weld open rate increases, the battery cell is easily damaged by force, and the service life of the battery cell is affected.

[0146] An embodiment of the present application further provides an electrical device, comprising a battery cell 10 according to any of the above solutions, and the battery cell 10 is used to provide electrical energy to the electrical device.

[0147] The electrical equipment may be any of the aforementioned devices or equipment using the battery cell 10 .

[0148] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application may be combined with each other.

[0149] The above are only preferred embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A battery cell, characterized in that: It comprises a shell and an electrode assembly, wherein the electrode assembly is accommodated in the shell, and the shell comprises a first end wall and a second end wall which are arranged opposite to each other along the thickness direction of the electrode assembly; The electrode assembly comprises a first positive electrode sheet, a first negative electrode sheet and a first separator, wherein the first negative electrode sheet is bonded to the first end wall via a first bonding layer, the first positive electrode sheet is located on a side of the first negative electrode sheet facing away from the first end wall, and the first separator is disposed between the first positive electrode sheet and the first negative electrode sheet; Among them, the adhesion force of the first adhesive layer is F1, satisfying F1≥10N / m; the adhesion force between the first negative electrode plate and the first separator is F2, and the adhesion force between the first positive electrode plate and the first separator is F3, satisfying F2<F3.

2. The battery cell according to claim 1, characterized in that: F3-F2≥5N / m.

3. The battery cell according to claim 1, characterized in that: 10N / m≤F2≤95N / m, 15N / m≤F3≤100N / m.

4. The battery cell according to claim 1, characterized in that: The first negative electrode plate comprises a negative electrode current collector and a negative electrode active material layer. The negative electrode active material layer is arranged on a side of the negative electrode current collector facing the first positive electrode plate. A groove is arranged on a side of the negative electrode active material layer facing the first separator.

5. The battery cell according to claim 4, characterized in that: The projection area of ​​the groove in the thickness direction of the first negative electrode sheet is S1, and the projection area of ​​the negative electrode active material layer in the thickness direction of the first negative electrode sheet is S2, satisfying 5%≤S1 / S2≤35%.

6. The battery cell according to claim 4, characterized in that: The groove extends along the first direction, the width of the groove along the second direction is W1, the width of the negative electrode active material layer along the second direction is W2, and 5%≤W1 / W2≤35% is satisfied; The thickness direction of the electrode assembly, the first direction, and the second direction are perpendicular to each other.

7. The battery cell according to claim 4, characterized in that: The first positive electrode plate comprises a positive electrode current collector, a first positive electrode active material layer and a second positive electrode active material layer, wherein the first positive electrode active material layer is arranged on a side of the positive electrode current collector facing the first negative electrode plate, and the second positive electrode active material layer is arranged on a side of the positive electrode current collector facing away from the first negative electrode plate; The first positive electrode active material layer is arranged in a plane on a side facing the first separator.

8. The battery cell according to claim 1, characterized in that: The first negative electrode plate includes a negative electrode current collector and a negative electrode active material layer. The negative electrode active material layer is arranged on the side of the negative electrode current collector facing the first positive electrode plate. The negative electrode active material layer includes a first adhesive. The content of the first adhesive in the negative electrode active material layer is 0.3% to 0.8%.

9. The battery cell according to claim 1, characterized in that: The first positive electrode plate includes a positive electrode collector, a first positive electrode active material layer and a second positive electrode active material layer, the first positive electrode active material layer is arranged on the side of the positive electrode collector facing the first negative electrode plate, and the second positive electrode active material layer is arranged on the side of the positive electrode collector facing away from the first negative electrode plate; the first positive electrode active material layer includes a second adhesive, and the content of the second adhesive in the first positive electrode active material layer is 0.8% to 2%.

10. The battery cell according to claim 1, characterized in that: The first diaphragm includes a base layer, a second adhesive layer and a third adhesive layer, the second adhesive layer is arranged on the side of the base layer facing the first negative electrode sheet, the third adhesive layer is arranged on the side of the base layer facing the first positive electrode sheet, the second adhesive layer includes a third adhesive, the content of the third adhesive in the second adhesive layer is a, the third adhesive layer includes a fourth adhesive, the content of the fourth adhesive in the third adhesive layer is b, satisfying a<b.

11. The battery cell according to claim 10, characterized in that: 45%≤a≤85%。 12. The battery cell according to claim 1, characterized in that: The first diaphragm includes a base layer, a second bonding layer and a third bonding layer, the second bonding layer is arranged on the side of the base layer facing the first negative electrode plate, the third bonding layer is arranged on the side of the base layer facing the first positive electrode plate, the second bonding layer includes a first ceramic material, the content of the first ceramic material in the second bonding layer is c, the third bonding layer includes a second ceramic material, the content of the second ceramic material in the third bonding layer is d, satisfying c>d.

13. The battery cell according to claim 11, characterized in that: 10%≤c≤50%。 14. The battery cell according to claim 1, characterized in that: The electrode assembly further includes a second positive electrode sheet, a second negative electrode sheet, and a second separator, wherein the second negative electrode sheet is bonded to the second end wall via a fourth bonding layer, the second positive electrode sheet is located on a side of the second negative electrode sheet facing away from the second end wall, and the second separator is disposed between the second positive electrode sheet and the second negative electrode sheet; The bonding force of the fourth bonding layer is F4, satisfying F4≥10N / m; the bonding force between the second negative electrode plate and the second separator is F5, and the bonding force between the second positive electrode plate and the second separator is F6, satisfying F5<F6.

15. The battery cell according to claim 1, characterized in that: The housing further comprises a side wall, the side wall being arranged around the first end wall, the side wall connecting the first end wall and the second end wall; The electrode assembly includes a plurality of side surfaces connected end to end, a fifth adhesive layer is disposed between at least one of the side surfaces and the side wall, and the electrode assembly is bonded to the side wall via the fifth adhesive layer.

16. The battery cell according to claim 15, characterized in that: The adhesive force of the fifth adhesive layer is F7, satisfying F7≥50N / m.

17. The battery cell according to claim 15, characterized in that: The ratio of the length of each of the fifth adhesive layers to the length of the side surface where the fifth adhesive layer is located is between 40% and 80%.

18. The battery cell according to claim 1, characterized in that: The shell is a hard shell.

19. The battery cell according to claim 1, characterized in that: The electrode assembly is a laminated structure.

20. An electrical equipment, characterized in that: The invention comprises a battery cell as described in any one of claims 1 to 19, wherein the battery cell is used to provide electrical energy.

Citation Information

Cited By

  • Battery cell and electrical device

    WO2026032070A1

  • Secondary battery and electric device

    WO2026117932A1

  • Battery cell and electric device

    WO2026184312A1

  • Secondary battery and electric device

    WO2026194546A1