Ink set, image recording method, and image recorded matter
By using an ink group containing amide structure polymerizable compound and indium metal particles in high-speed printing, combined with inkjet recording and active energy ray irradiation technology, the problem of difficult to obtain heavy image in high-speed printing is solved, and the metallic luster of the image is achieved Improved sex and brightness.
Patent Information
- Application Number
- CN202380032814.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-08
- Filing Date
- 2023-03-31
- Publication Date
- 2024-11-19
AI Technical Summary
When high-speed printing is performed using active energy ray curing ink containing polymerizable compounds, it is difficult to obtain images with a visually heavy feeling.
Using an ink group containing a polymerizable compound having an amide structure and metal particles containing indium, the first ink is imparted to the substrate by an inkjet recording method and an active energy ray is irradiated, and then the second ink is imparted to the first ink film and Active energy rays are irradiated to form images with a heavy feeling.
Even under high-speed printing conditions, images with visual heavyness can be recorded, achieving improved metallic luster and brightness.
Smart Images

Figure BDA0005072846580000131 
Figure BDA0005072846580000331 
Figure BDA0005072846580000341
Abstract
Description
Technical Field
[0001] The present invention relates to an ink set, an image recording method and an image recorded article. Background Art
[0002] In recent years, studies have been conducted on methods of recording images using active energy ray-curable inks containing polymerizable compounds.
[0003] For example, Japanese Patent Application Laid-Open No. 2013-230637 describes a method for producing a recorded object, which includes: a first ink imparting step of imparting a first ink containing a first polymerizable compound that is polymerized by ultraviolet irradiation to a surface of a substrate at least of which is composed of a non-liquid-absorbing material by an inkjet method; a first curing step of polymerizing / curing the first polymerizable compound; a second ink imparting step of imparting a second ink containing a second polymerizable compound that is polymerized by ultraviolet irradiation and a metal powder to a cured product of the first polymerizable compound by an inkjet method; and a second curing step of polymerizing / curing the second polymerizable compound. Summary of the invention
[0004] Technical issues to be solved by the invention
[0005] However, when high-speed printing is performed using an active energy ray-curable ink containing a polymerizable compound, it is sometimes necessary to obtain an image that visually has a heavy feel.
[0006] The present invention has been made in view of such circumstances, and according to one embodiment of the present invention, an ink set and an image recording method are provided that can record an image that looks visually heavy even when high-speed printing is performed.
[0007] According to another embodiment of the present invention, there is provided an image record having an image having a visually heavy feeling.
[0008] Means for solving technical problems
[0009] The present invention includes the following aspects.
[0010] <1> An ink set comprising: a first ink which is an active energy ray-curable inkjet ink containing a polymerizable compound; and a second ink which is an active energy ray-curable inkjet ink containing metal particles containing indium and a polymerizable compound, wherein the surface tension of the first ink is 30 mN / m or more.
[0011] <2> The ink set according to <1>, wherein
[0012] The polymerizable compound contained in the first ink includes a polymerizable compound having an amide structure.
[0013] <3> The ink set according to <2>, wherein
[0014] The content of the polymerizable compound having an amide structure is 5% by mass to 50% by mass based on the total amount of the first ink.
[0015] <4> The ink set according to any one of <1> to <3>, wherein
[0016] The polymerizable compound contained in the first ink includes a polyfunctional polymerizable compound.
[0017] <5> The ink set according to <4>, wherein
[0018] The ratio of the polyfunctional polymerizable compound to the polymerizable compound is 1% by mass to 50% by mass.
[0019] <6> The ink set according to any one of <1> to <5>, wherein
[0020] The polymerizable compound contained in the first ink contains a monofunctional polymerizable compound including at least one structure selected from the group consisting of a cyclic ether structure and an alicyclic structure.
[0021] <7> The ink set according to any one of <1> to <6>, wherein
[0022] The polymerizable compound contained in the first ink includes a polymerizable compound having an amide structure and a monofunctional polymerizable compound including at least one structure selected from the group consisting of a cyclic ether structure and an alicyclic structure.
[0023] <8> An image recording method using the ink set described in any one of <1> to <7>, the image recording method comprising: a step of applying a first ink to a substrate using an inkjet recording method; a step of irradiating the first ink applied to the substrate with active energy rays A to form a first ink film; a step of applying a second ink to the first ink film using an inkjet recording method; and a step of recording an image by irradiating the second ink applied to the first ink film with active energy rays B.
[0024] <9> The image recording method according to <8>, wherein:
[0025] The step of recording an image includes: a step of pre-curing the second ink by irradiating an active energy ray B1 having an irradiation energy lower than the active energy ray B; and a step of irradiating the active energy ray B to the ink film formed by the pre-curing of the second ink.
[0026] <10> An image recorded material comprising a substrate and an image arranged on the substrate, the image comprising: a first ink layer formed on a surface of the substrate; and a second ink layer formed on a surface of the first ink layer, wherein metal particles containing indium are present only in a region up to 70% of the thickness of the second ink layer from the surface of the second ink layer toward the interior of the second ink layer.
[0027] Effects of the Invention
[0028] According to one embodiment of the present invention, there is provided an ink set and an image recording method capable of recording an image that visually gives a heavy feeling even when high-speed printing is performed.
[0029] According to another embodiment of the present invention, there is provided an image record having an image having a visually heavy feeling. DETAILED DESCRIPTION
[0030] Hereinafter, the ink set, image recording method, and image recorded article of the present invention will be described in detail.
[0031] In the present specification, a numerical range expressed using "to" means a range including the numerical values described before and after "to" as the minimum value and the maximum value, respectively.
[0032] In the numerical ranges recorded in stages in this specification, the upper limit or lower limit recorded in a certain numerical range can be replaced by the upper limit or lower limit of the numerical range recorded in other stages. In addition, in the numerical ranges recorded in this specification, the upper limit or lower limit recorded in a certain numerical range can also be replaced by the value shown in the embodiments.
[0033] In the present specification, when a plurality of substances corresponding to each component are present in a composition, the amount of each component in the composition refers to the total amount of the plurality of substances present in the composition unless otherwise specified.
[0034] In the present specification, a combination of two or more preferred aspects is a more preferred aspect.
[0035] In this specification, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process can be achieved.
[0036] In this specification, "image" refers to the entire film, and "image recording" refers to the formation of an image (ie, film). Furthermore, the concept of "image" in this specification also includes a solid image.
[0037] In this specification, “(meth)acrylate” is a concept including both acrylate and methacrylate, “(meth)acryloyl” is a concept including both acryloyl and methacryloyl, and “(meth)acrylic acid” is a concept including both acrylic acid and methacrylic acid.
[0038] [Ink set]
[0039] The ink set of the present invention comprises: a first ink containing a polymerizable compound; and a second ink containing metal particles containing indium and a polymerizable compound, wherein the surface tension of the first ink is 30 mN / m or more.
[0040] According to the ink set of the present invention, even when high-speed printing is performed, an image with visually rich feeling can be obtained.
[0041] Hereinafter, each component contained in the first ink and the second ink in the ink set according to one embodiment of the present invention will be described.
[0042] The ink set of the present invention comprises: a first ink which is an active energy ray-curable inkjet ink; and a second ink which is an active energy ray-curable inkjet ink. That is, the first ink and the second ink are cured by irradiation with active energy rays. Examples of active energy rays include gamma rays, beta rays, electron beams, ultraviolet rays, and visible rays. Among them, the active energy rays are preferably ultraviolet rays. The first ink and the second ink are preferably ultraviolet curable inks.
[0043] The first ink and the second ink are inkjet inks, that is, the first ink and the second ink are inks to be ejected by an inkjet recording method.
[0044] <First ink>
[0045] (Polymerizable compound)
[0046] The first ink included in the ink set of the present invention contains at least one polymerizable compound.
[0047] The polymerizable compound is a compound having a polymerizable group. The polymerizable group is preferably a radical polymerizable group or a cation polymerizable group, and more preferably a radical polymerizable group.
[0048] The polymerizable compound may have only one type of polymerizable group, or may have two or more types of polymerizable groups.
[0049] As the polymerizable compound, a radical polymerizable compound is preferred.
[0050] The radical polymerizable group is preferably an ethylenically unsaturated group, more preferably at least one selected from the group consisting of a (meth)acryloyl group, an allyl group, a styryl group, and a vinyl group, and further preferably a (meth)acryloyl group.
[0051] Examples of the cationically polymerizable group include an epoxy group and an oxetane group.
[0052] The polymerizable compound may be a polymerizable monomer, a polymerizable polymer, or a combination of a polymerizable monomer and a polymerizable polymer.
[0053] Here, a polymerizable monomer refers to a polymerizable compound having a molecular weight of less than 1000, and a polymerizable polymer refers to a polymerizable compound having a weight average molecular weight (Mw) of not less than 1000. The concept of "polymerizable polymer" in the present invention also includes so-called oligomers.
[0054] The weight average molecular weight (Mw) of the polymerizable compound is preferably 30,000 or less, more preferably 20,000 or less, and further preferably 10,000 or less.
[0055] Examples of the lower limit of the Mw of the polymerizable compound include 50, 60, and 70.
[0056] In the present invention, the weight average molecular weight (Mw) refers to a value measured by gel permeation chromatography (GPC).
[0057] In the measurement based on GPC, HLC (registered trademark)-8020GPC (TOSOH CORPORATION) was used as a measuring device, three TSKgel (registered trademark) Super Multipore HZ-H (4.6 mmID×15 cm, TOSOH CORPORATION) were used as columns, and THF (tetrahydrofuran) was used as an eluent. In addition, as measurement conditions, the sample concentration was set to 0.45% by mass, the flow rate was set to 0.35 ml / min, the sample injection volume was set to 10 μL, and the measurement temperature was set to 40° C., and the measurement was performed using an RI detector.
[0058] The calibration curve was prepared based on eight samples of "Standard Samples TSK Standard, Polystyrene" of TOSOH CORPORATION: "F-40", "F-20", "F-4", "F-1", "A-5000", "A-2500", "A-1000", and "n-propylbenzene".
[0059] The polymerizable compound may be a monofunctional polymerizable compound or a polyfunctional polymerizable compound.
[0060] Here, a monofunctional polymerizable compound refers to a compound containing only one polymerizable group in one molecule, and a polyfunctional polymerizable compound refers to a compound containing two or more polymerizable groups in one molecule.
[0061] Examples of the monofunctional polymerizable compound include monofunctional (meth)acrylates, monofunctional (meth)acrylamides, monofunctional aromatic vinyl compounds, monofunctional vinyl ethers, and monofunctional N-vinyl compounds.
[0062] Examples of the monofunctional (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, tert-octyl (meth)acrylate, isoamyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, octadecyl (meth)acrylate, isooctadecyl (meth)acrylate, cyclohexyl (meth)acrylate, 4-n-butylcyclohexyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, and 1,2-dimethylformamide (meth)acrylate. Bornyl ester, isobornyl (meth)acrylate, 2-ethylhexyl diethylene glycol (meth)acrylate, butoxyethyl (meth)acrylate, 2-chloroethyl (meth)acrylate, 4-bromobutyl (meth)acrylate, cyanoethyl (meth)acrylate, benzyl (meth)acrylate, butoxymethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 2-(2-methoxyethoxy)ethyl (meth)acrylate, 2-(2-butoxyethoxy)ethyl (meth)acrylate, ethyl carbitol (meth)acrylate, 4-butylphenyl (meth)acrylate, phenyl (meth)acrylate, 2,4,5-Tetramethylphenyl (meth)acrylate, 4-chlorophenyl (meth)acrylate, 2-phenoxymethyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, glycidyl (meth)acrylate, glycidyloxybutyl (meth)acrylate, glycidyloxyethyl (meth)acrylate, glycidyloxypropyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate , 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, cyclic trimethylolpropane formal (meth)acrylate, phenyl glycidyl ether (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, diethylaminopropyl (meth)acrylate, trimethoxysilylpropyl (meth)acrylate, trimethylsilylpropyl (meth)acrylate, polyethylene oxide monomethyl ether (meth)acrylate, polyethylene oxide alkyl (meth)acrylate, polyethylene oxide monoalkyl ether (meth)acrylate, dipropylene glycol (meth)acrylate, polypropylene oxide monoalkyl ether (meth)acrylate, 2-methacryloyloxyethyl succinate, 2-methacryloyloxyhexahydrophthalate, 2-methacryloyloxyethyl-2-hydroxypropyl phthalate, butoxydiethylene glycol (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, ethylene oxide (EO) modified phenol (meth)acrylate, EO modified cresol (meth)acrylate, ,
[0063] Examples of the monofunctional (meth)acrylamide include (meth)acrylamide, N-methyl (meth)acrylamide, N-ethyl (meth)acrylamide, N-propyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-n-butyl (meth)acrylamide, N-tert-butyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, N-isobutoxymethyl (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, N-phenyl (meth)acrylamide, N-benzyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, hydroxyethyl (meth)acrylamide, hydroxymethyl (meth)acrylamide, and (meth)acryloyl morpholine.
[0064] Examples of the monofunctional aromatic vinyl compound include styrene, dimethylstyrene, trimethylstyrene, isopropylstyrene, chloromethylstyrene, methoxystyrene, acetoxystyrene, chlorostyrene, dichlorostyrene, bromostyrene, methyl vinylbenzoate, 3-methylstyrene, 4-methylstyrene, 3-ethylstyrene, 4-ethylstyrene, 3-propylstyrene, 4-propylstyrene, 3-butylstyrene, 4-butylstyrene, 3-hexylstyrene, 4-hexylstyrene, 3-octylstyrene, 4-octylstyrene, 3-(2-ethylhexyl)styrene, 4-(2-ethylhexyl)styrene, allylstyrene, isopropenylstyrene, butenylstyrene, octenylstyrene, 4-tert-butoxycarbonylstyrene and 4-tert-butoxystyrene.
[0065] Examples of the monofunctional vinyl ether include methyl vinyl ether, ethyl vinyl ether, propyl vinyl ether, n-butyl vinyl ether, tert-butyl vinyl ether, 2-ethylhexyl vinyl ether, n-nonyl vinyl ether, dodecyl vinyl ether, cyclohexyl vinyl ether, cyclohexyl methyl vinyl ether, 4-methylcyclohexyl methyl vinyl ether, benzyl vinyl ether, dicyclopentenyl vinyl ether, 2-dicyclopentenyloxyethyl vinyl ether, methoxyethyl vinyl ether, ethoxyethyl vinyl ether, butoxyethyl vinyl ether, methoxyethoxyethyl vinyl ether, ethoxyethoxyethyl vinyl ether, methoxypolyethylene glycol vinyl ether, tetrahydrofurfuryl vinyl ether, 2-hydroxyethyl vinyl ether, 2-hydroxypropyl vinyl ether, 4-hydroxybutyl vinyl ether, 4-hydroxymethylcyclohexyl methyl vinyl ether, diethylene glycol monovinyl ether, polyethylene glycol vinyl ether, chloroethyl vinyl ether, chlorobutyl vinyl ether, chloroethoxyethyl vinyl ether, phenylethyl vinyl ether, and phenoxypolyethylene glycol vinyl ether.
[0066] Examples of the monofunctional N-vinyl compound include N-vinyl caprolactam and N-vinyl pyrrolidone.
[0067] The polyfunctional polymerizable compound is a polymerizable compound having two or more functional groups.
[0068] Examples of the bifunctional polymerizable compound include bifunctional (meth)acrylates, bifunctional vinyl ethers, bifunctional (meth)acrylamides, and bifunctional polymerizable compounds containing a vinyl ether group and a (meth)acryloyl group.
[0069] Examples of the bifunctional (meth)acrylate include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, butanediol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, hexanediol di(meth)acrylate, heptanediol di(meth)acrylate, EO Modified neopentyl glycol di(meth)acrylate, PO modified neopentyl glycol di(meth)acrylate, EO modified hexanediol di(meth)acrylate, PO modified hexanediol di(meth)acrylate, octanediol di(meth)acrylate, nonanediol di(meth)acrylate, decanediol di(meth)acrylate, dodecanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, glycerol di(meth)acrylate, pentaerythritol di(meth)acrylate, ethylene glycol diglycidyl ether di(meth)acrylate, diethylene glycol diglycidyl ether di(meth)acrylate, and tricyclodecane dimethanol di(meth)acrylate.
[0070] Examples of the bifunctional vinyl ether include 1,4-butanediol divinyl ether, ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, polyethylene glycol divinyl ether, propylene glycol divinyl ether, butanediol divinyl ether, hexanediol divinyl ether, 1,4-cyclohexanedimethanol divinyl ether, bisphenol A alkylene oxide divinyl ether, and bisphenol F alkylene oxide divinyl ether.
[0071] Examples of the bifunctional (meth)acrylamide include N,N′-methylenebis(meth)acrylamide and N,N′-ethylenebis(meth)acrylamide.
[0072] Examples of the bifunctional polymerizable compound containing a vinyl ether group and a (meth)acryloyl group include 2-(2-vinyloxyethoxy)ethyl (meth)acrylate.
[0073] Examples of the trifunctional or higher-functional polymerizable compound include trifunctional or higher-functional (meth)acrylates and trifunctional or higher-functional vinyl ethers.
[0074] Examples of the trifunctional or higher-functional (meth)acrylate include trimethylolethane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, EO-modified trimethylolpropane tri(meth)acrylate, PO-modified trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tri(meth)acryloyloxyethoxytrimethylolpropane, glycerol polyglycidyl ether poly(meth)acrylate, and tris(2-acryloyloxyethyl)isocyanurate.
[0075] Examples of the trifunctional or higher-functional vinyl ether include trimethylolethane trivinyl ether, trimethylolpropane trivinyl ether, ditrimethylolpropane tetravinyl ether, glycerol trivinyl ether, pentaerythritol tetravinyl ether, dipentaerythritol pentavinyl ether, dipentaerythritol hexavinyl ether, EO-modified trimethylolpropane trivinyl ether, PO-modified trimethylolpropane trivinyl ether, EO-modified ditrimethylolpropane tetravinyl ether, PO-modified ditrimethylolpropane tetravinyl ether, EO-modified pentaerythritol tetravinyl ether, PO-modified pentaerythritol tetravinyl ether, EO-modified dipentaerythritol hexavinyl ether, and PO-modified dipentaerythritol hexavinyl ether.
[0076] As the polyfunctional polymerizable compound, urethane (meth)acrylate may also be mentioned.
[0077] The urethane (meth)acrylate is preferably a compound containing two or three (meth)acryloyl groups and at least one urethane bond.
[0078] Examples of the urethane (meth)acrylate include urethane (meth)acrylates which are reaction products of a bifunctional isocyanate compound and a hydroxyl group-containing (meth)acrylate (and, if necessary, other active hydrogen group-containing compounds).
[0079] Examples of the bifunctional isocyanate compound include aliphatic diisocyanates such as methylene diisocyanate, dimethylene diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, dipropyl ether diisocyanate, 2,2-dimethylpentane diisocyanate, 3-methoxyhexane diisocyanate, octamethylene diisocyanate, 2,2,4-trimethylpentane diisocyanate, nonamethylene diisocyanate, decamethylene diisocyanate, 3-butoxyhexane diisocyanate, 1,4-butanediol dipropyl ether diisocyanate, and thiodihexyl diisocyanate; and m-phenylene glycol diisocyanate. diisocyanate, p-phenylene diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, dimethylphenylene diisocyanate, ethylphenylene diisocyanate, isopropylphenylene diisocyanate, tolidine diisocyanate, 1,4-naphthalene diisocyanate, 1,5-naphthalene diisocyanate, 2,6-naphthalene diisocyanate, 2,7-naphthalene diisocyanate, m-xylylene diisocyanate, p-xylylene diisocyanate, tetramethylxylylene diisocyanate and other aromatic diisocyanates; and hydrogenated xylylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane 4,4'-diisocyanate and other alicyclic diisocyanates.
[0080] Examples of the hydroxyl group-containing (meth)acrylate include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, phenyl glycidyl ether (meth)acrylate, pentaerythritol (meth)acrylate, and dipentaerythritol penta (meth)acrylate.
[0081] Commercially available products of urethane (meth) acrylates include CN996 (difunctional urethane acrylate, weight average molecular weight (Mw) = 2850) from Sartomer Company, Inc., UA-122P (difunctional urethane acrylate, Mw = 1100) from SHIN-NAKAMURA CHEMICAL Co., Ltd., Ziguang (registered trademark) UV-6630B (difunctional urethane acrylate, Mw = 3000), Ziguang (registered trademark) UV-3310B (difunctional urethane acrylate, Mw = 5000), and Ziguang (registered trademark) UV-7630B (hexafunctional urethane acrylate, Mw = 2200) from Nippon Synthetic Chemical Industry Co., Ltd.
[0082] Examples of the polyfunctional polymerizable compound include silicone compounds having an ethylenically unsaturated group.
[0083] As the silicone compound having an ethylenically unsaturated group, silicone polyether acrylate is preferred, polyfunctional silicone polyether acrylate is more preferred, and penta- to hexa-functional silicone polyether acrylate is further preferred.
[0084] Examples of the above-mentioned bifunctional polymerizable compounds and trifunctional or higher-functional polymerizable compounds include epoxy (meth)acrylates.
[0085] Here, epoxy (meth)acrylate refers to a reaction product formed by reacting a carboxyl group in (meth)acrylic acid with two or three epoxy groups in an epoxy compound containing two or three epoxy groups. That is, epoxy (meth)acrylate does not contain an epoxy group in its structure.
[0086] Examples of epoxy (meth)acrylate include reaction products of (meth)acrylic acid and epoxy resin.
[0087] Examples of the epoxy resin include bisphenol A type epoxy resin and cresol novolac type epoxy resin.
[0088] The content of the polymerizable compound is preferably 50% by mass to 95% by mass, and more preferably 60% by mass to 90% by mass, based on the total amount of the ink.
[0089] Among them, the polymerizable compound contained in the first ink preferably contains a polymerizable compound having an amide structure. Hereinafter, the polymerizable compound having an amide structure will be described as "polymerizable compound A".
[0090] In the present invention, the amide structure refers to a structure represented by "-C(=O)-N<". The atoms bonded to the terminal carbon atom and the nitrogen atom are not particularly limited, and examples thereof include hydrogen atoms and carbon atoms.
[0091] If the first ink contains the polymerizable compound A, when the second ink is applied after the first ink, a part of the polymerizable compound A transfers to the second ink. The transfer of the polymerizable compound A increases the energy of the second ink film and promotes the metal particles contained in the second ink to be pushed to the air-liquid interface, thereby further improving the metallic gloss of the image. In addition, the movement of the metal particles contained in the second ink to the air-liquid interface becomes faster, and even in the case of high-speed printing, the brightness of the image is reduced, so that a visually heavy image can be obtained.
[0092] Examples of the polymerizable compound A include the above-mentioned monofunctional (meth)acrylamide, bifunctional (meth)acrylamide, 3-(meth)acryloyl-2-oxazolidinone, N-vinylpyrrolidone, and N-vinylcaprolactam.
[0093] From the viewpoint of increasing the migration speed of the metal particles contained in the second ink to the gas-liquid interface, the content of the polymerizable compound A is preferably 5% to 50% by mass, more preferably 10% to 50% by mass, and further preferably 15% to 50% by mass, relative to the total amount of the first ink.
[0094] As the polymerizable compound, the first ink preferably contains a multifunctional polymerizable compound, and more preferably contains a monofunctional polymerizable compound and a multifunctional polymerizable compound. By making the first ink contain a multifunctional polymerizable compound, a first ink film with excellent curability can be formed. If the curability of the first ink film is high, the surface of the first ink film is smooth. Therefore, when the second ink is applied to the first ink film, the surface of the second ink film can also be smooth, so that an image with excellent metallic gloss can be obtained.
[0095] From the viewpoint of improving the metallic gloss of an image, the proportion of the polyfunctional polymerizable compound in the polymerizable compound is preferably 1% by mass to 50% by mass, and more preferably 10% by mass to 40% by mass.
[0096] Furthermore, the first ink preferably contains a monofunctional polymerizable compound including at least one structure selected from the group consisting of a cyclic ether structure and an alicyclic structure as a polymerizable compound. Hereinafter, the monofunctional polymerizable compound including at least one structure selected from the group consisting of a cyclic ether structure and an alicyclic structure will be described as "polymerizable compound B".
[0097] The polymerizable compound having a ring structure tends to have a high glass transition temperature and a good balance between elasticity and viscosity of the ink film. Therefore, if the first ink contains the polymerizable compound B, the adhesion to the substrate is improved.
[0098] In the polymerizable compound B, examples of the cyclic ether structure include a furan ring structure, a pyran ring structure, an oxirane ring structure, an oxetane ring structure, a dioxane ring structure, a dioxolane ring structure, and a morpholine ring structure.
[0099] In the polymerizable compound B, the number of carbon atoms constituting the ring of the alicyclic structure is not particularly limited, but is preferably 5 to 10. Examples of the alicyclic structure include a cyclohexane ring structure, a dicyclopentyl ring structure, a dicyclopentenyl ring structure, a norbornane ring structure, an isobornane ring structure, a norbornene ring structure, an isobornene ring structure, and an adamantane ring structure.
[0100] Examples of the polymerizable compound B include the following compounds. Acryloylmorpholine also corresponds to the polymerizable compound A described above.
[0101] [Table 1]
[0102]
[0103] Furthermore, the polymerizable compound B preferably contains a cyclic ether structure. If a cyclic ether structure is included, the odor tends to be reduced.
[0104] The content of the polymerizable compound B is preferably 45% by mass or more, more preferably 60% by mass to 80% by mass, and further preferably 65% by mass to 80% by mass, based on the total amount of the first ink, from the viewpoint of adhesion to the substrate.
[0105] The polymerizable compound contained in the first ink preferably contains a polymerizable compound A and a polymerizable compound B.
[0106] In the first ink, the mass ratio of the content of the polymerizable compound B to the content of the polymerizable compound A is preferably 1-10, more preferably 1-5, and even more preferably 1-4.
[0107] In the first ink, the total content of all polymerizable compounds contained in the first ink is preferably 70% by mass to 90% by mass, and more preferably 80% by mass to 90% by mass, relative to the total amount of the first ink.
[0108] (Photopolymerization Initiator)
[0109] The first ink preferably contains at least one photopolymerization initiator.
[0110] The polymerization initiator is preferably a photoradical polymerization initiator that generates radicals by irradiation with light.
[0111] Examples of the photoradical polymerization initiator include (a) alkylphenone compounds, (b) acylphosphine oxide compounds, (c) aromatic onium salt compounds, (d) organic peroxides, (e) thio compounds (for example, thioxanthone compounds such as isopropylthioxanthone), (f) hexaarylbiimidazole compounds, (g) ketone oxime ester compounds, (h) borate compounds, (i) azinium compounds, (j) metallocene compounds, (k) active ester compounds, (l) compounds having a carbon-halogen bond, and (m) alkylamine compounds.
[0112] Among them, the photopolymerization initiator preferably contains an acylphosphine oxide compound.
[0113] Examples of the acylphosphine oxide compound include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,6-dimethylbenzoyl)phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-2-methoxyphenylphosphine oxide, bis(2,6-dimethylbenzoyl)-2-methoxyphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,4-dimethoxyphenylphosphine oxide, bis(2,6-dimethylbenzoyl)-2,4-dimethoxyphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,4-dipentyloxyphenylphosphine oxide, bis(2,6-dimethylbenzoyl)-2,4-dipentyloxyphenylphosphine oxide, and bis(2,6-dimethylbenzoyl)-2,4-dimethoxyphenylphosphine oxide. benzoyl)-2,4-dipentyloxyphenylphosphine oxide, 2,4,6-trimethylbenzoylethoxyphenylphosphine oxide, 2,6-dimethylbenzoylethoxyphenylphosphine oxide, 2,4,6-trimethylbenzoylmethoxyphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2,6-dimethylbenzoylmethoxyphenylphosphine oxide, 2,4,6-trimethylbenzoyl(4-pentyloxyphenyl)phenylphosphine oxide, and 2,6-dimethylbenzoyl(4-pentyloxyphenyl)phenylphosphine oxide.
[0114] Among them, the acylphosphine oxide compound is preferably bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide or 2,4,6-trimethylbenzoyldiphenylphosphine oxide.
[0115] The photopolymerization initiator may be a low-molecular-weight photopolymerization initiator having a molecular weight of less than 500, or may be a high-molecular-weight photopolymerization initiator having a molecular weight of 500 or more.
[0116] The molecular weight of the photopolymerization initiator is preferably 500 to 3,000, more preferably 700 to 2,500, and even more preferably 900 to 2,100.
[0117] Regarding the photopolymerization initiator, reference can be made to known documents such as JP-A-2017-105902 (paragraph 0038, etc.) and JP-T-2017-522364 (paragraphs 0017 to 0053).
[0118] Examples of commercially available radical polymerization initiators include:
[0119] Omnirad TPO H, Omnirad 819, Omnirad 369, Omnirad 907, Omnirad 2959, Omnipol 910, Omnipol TX, Omnipol 9210 (all manufactured by IGM Resins BV); and Speedcure 7005, Speedcure 7010, Speedcure 7010L, Speedcure 7040, Speedcure TPO (manufactured by Lambson).
[0120] The content of the photopolymerization initiator is preferably 1% by mass to 20% by mass, and more preferably 5% by mass to 15% by mass, based on the total amount of the first ink.
[0121] On the other hand, when the first ink is an ink that is cured by electron beams as active energy rays, the content of the photopolymerization initiator relative to the total amount of the first ink may be less than 1% by mass.
[0122] Here, the content of the photopolymerization initiator relative to the total amount of the first ink being less than 1 mass % means that the first ink does not contain a photopolymerization initiator, or even if it contains a photopolymerization initiator, the content of the photopolymerization initiator relative to the total amount of the first ink is less than 1 mass %.
[0123] (Surfactant)
[0124] The first ink may contain at least one surfactant.
[0125] As surfactants, surfactants described in Japanese Patent Application Laid-Open No. 62-173463 and Japanese Patent Application Laid-Open No. 62-183457 can be cited. Also, as surfactants, for example, anionic surfactants such as dialkyl sulfosuccinates, alkylnaphthalene sulfonates, and fatty acid salts; nonionic surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene alkyl allyl ethers, acetylene glycols, and polyoxyethylene / polyoxypropylene block copolymers; and cationic surfactants such as alkylamine salts and quaternary ammonium salts can be cited. Also, the surfactant can be a fluorine-based surfactant or a silicone-based surfactant.
[0126] From the viewpoint of setting the surface tension of the ink to 30 mN / m or more, the first ink preferably contains no surfactant or contains a surfactant content of less than 0.01% by mass.
[0127] (Inhibitor)
[0128] The first ink preferably contains at least one polymerization inhibitor.
[0129] Examples of the polymerization inhibitor include p-methoxyphenol, quinones (e.g., hydroquinone, benzoquinone, methoxybenzoquinone, etc.), phenothiazines, catechols, alkylphenols (e.g., butylhydroxytoluene (BHT)), alkylbisphenols, zinc dimethyldithiocarbamate, copper dimethyldithiocarbamate, copper dibutyldithiocarbamate, copper salicylate, thiodipropionate esters, mercaptobenzimidazole, phosphites, 2,2,6,6-tetramethylpiperidin-1-oxyl (TEMPO), 2,2,6,6-tetramethyl-4-hydroxypiperidin-1-oxyl (TEMPOL), and tris(N-nitroso-N-phenylhydroxylamine)aluminum salt (also known as cupferroin Al).
[0130] Among them, the polymerization inhibitor is preferably at least one selected from p-methoxyphenol, catechols, quinones, alkylphenols, TEMPO, TEMPOL and tris(N-nitroso-N-phenylhydroxylamine)aluminum salt, and more preferably at least one selected from p-methoxyphenol, hydroquinone, benzoquinone, BHT, TEMPO, TEMPOL and tris(N-nitroso-N-phenylhydroxylamine)aluminum salt.
[0131] When the first ink contains a polymerization inhibitor, the content of the polymerization inhibitor is preferably 0.01 to 5.0% by mass, more preferably 0.05 to 4.0% by mass, and even more preferably 0.1 to 3.0% by mass, based on the total amount of the first ink.
[0132] (Other ingredients)
[0133] The first ink may contain other components in addition to the above-mentioned components as necessary.
[0134] Examples of other components include colorants (eg, pigments, dyes), resins, dispersants, waxes, antioxidants, anti-fading agents, conductive salts, basic compounds, etc. The first ink preferably does not contain metal particles.
[0135] (physical properties)
[0136] The surface tension of the first ink is 30 mN / m or more. If the surface tension of the first ink is 30 mN / m or more, when the second ink is applied after the first ink, even if part of the components contained in the first ink are transferred to the second ink, the surface tension of the second ink can be suppressed from decreasing due to the transfer of the components. If the surface tension of the second ink is high, the metal particles are easily gathered at the air-liquid interface, and the speed at which the metal particles are concentrated on the surface of the second ink film is fast, so that even in the case of high-speed printing, a visually heavy image can be obtained.
[0137] From the viewpoint of image quality, the surface tension of the first ink is preferably 40 mN / m or less. That is, the surface tension of the first ink is preferably 30 mN / m to 40 mN / m, and more preferably 32 mN / m to 38 mN / m.
[0138] The surface tension refers to a value measured at 25°C.
[0139] The surface tension is a value measured using a surface tensiometer, and can be measured using, for example, a product name “Automatic Surface Tensiometer CBVP-Z (manufactured by Kyowa Interface Science Co., Ltd.)”.
[0140] The viscosity of the first ink is preferably 5 mPa·s to 50 mPa·s, more preferably 10 mPa·s to 30 mPa·s, and even more preferably 10 mPa·s to 25 mPa·s.
[0141] The viscosity refers to a value measured at 25°C.
[0142] The viscosity is a value measured using a viscometer, and can be measured using, for example, VISCOMETER RE-85L (manufactured by TokiSangyo Co., Ltd.).
[0143] <Second ink>
[0144] The second ink included in the ink set of the present invention contains metal particles containing indium and a polymerizable compound.
[0145] (Metal Particles)
[0146] The second ink contains at least one type of metal particles containing indium.
[0147] The shape of the metal particles is not particularly limited, and for example, circular, oval, rectangular, flaky, and irregular shapes can be cited. Among them, the shape of the metal particles is preferably flaky. In the present invention, "flaky" refers to a thin and flat shape, which is a concept including a flat plate and a curved plate.
[0148] Since the metal particles contain indium, the obtained image has excellent metallic gloss. Furthermore, if the metal particles containing indium are concentrated on the surface of the second ink film formed by the second ink, the whiteness of the image is suppressed and the lightness is reduced, thereby visually obtaining a thicker image.
[0149] The metal particles may contain metals other than indium. Examples of the metals other than indium include nickel, aluminum, iron, chromium, silver, gold, platinum, tin, zinc, titanium, and copper.
[0150] Among them, from the viewpoint of further improving metallic gloss, it is preferred that the metal contained in the metal particles is only indium.
[0151] The metal particles may also contain non-metallic elements (for example, oxygen (O), nitrogen (N), carbon (C), etc.).
[0152] The content of the metal is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 80% by mass or more, based on the total amount of the metal particles.
[0153] The average particle size of the metal particles is not particularly limited, but is preferably 0.05 μm to 0.5 μm, and more preferably 0.1 μm to 0.4 μm.
[0154] When the average particle diameter is 0.05 μm or more, the metallic gloss of the image is improved, and when the average particle diameter is 0.5 μm or less, the storage stability and ejection properties of the second ink are improved.
[0155] The average particle size mentioned here refers to the average value of the primary particle sizes of the metal particles (average primary particle size).
[0156] The average particle size of the metal particles is measured using a particle size distribution measuring device. The average particle size of the metal particles is measured three times using a laser diffraction / scattering particle size distribution measuring device, and the 50% volume cumulative diameter (D50) is calculated as the average of the three measured values. As a laser diffraction / scattering particle size distribution measuring device, for example, the product name "LA-960" manufactured by HORIBA, Ltd. can be used. In addition, the average particle size of the metal particles is the average particle size when the shape of the metal particles is assumed to be a sphere.
[0157] The average aspect ratio of the metal particles is not particularly limited, but is preferably 5-100, more preferably 5-50, and even more preferably 5-20.
[0158] When the average aspect ratio is 5 or more, the metallic gloss of the image is improved. When the average aspect ratio is 100 or less, the production suitability of the metal particles is improved.
[0159] In the present invention, the average aspect ratio refers to the ratio of the average equivalent circle diameter to the average thickness.
[0160] The average equivalent circle diameter and average thickness of the metal particles were measured by the following method.
[0161] As a liquid sample, a metal particle dispersion liquid (metal particle concentration: 20 mass %) containing metal particles as a dispersion and propylene glycol monomethyl ether (PGME) as a dispersion medium was prepared.
[0162] The liquid sample was coated on a polyethylene terephthalate (PET) film to obtain a coating film.
[0163] The surface of the coating film is observed by a scanning electron microscope (SEM) (e.g., Nova200 FIB-SEM manufactured by Thermo Fisher Scientific Inc., the same below). 50 metal particles are selected from the obtained SEM image, and the equivalent circle diameter of each metal particle is measured. The arithmetic mean of the equivalent circle diameters of the 50 metal particles is obtained and used as the average equivalent circle diameter of the metal particles.
[0164] The cross section of the coating film was observed by SEM, 50 metal particles were selected from the obtained SEM image, and the thickness of each metal particle was measured. The arithmetic mean of the thickness of the 50 metal particles was calculated and taken as the average thickness of the metal particles.
[0165] The average thickness of the metal particles is not particularly limited, but is preferably 10 nm to 50 nm, more preferably 15 nm to 45 nm, and even more preferably 20 nm to 40 nm from the viewpoint of improving the metallic gloss of the image.
[0166] As the shape of the metal particles when viewed from above, for example, polygonal, elliptical and irregular shapes can be listed. From the viewpoint of improving the metallic glossiness of the image, when viewed from above, the metal particles preferably have an outline formed by combining a straight line and a curve. Furthermore, when viewed from above, the outline of the metal particles is preferably R-shaped.
[0167] In the present invention, the R-shape refers to a shape in which there are no vertices where two sides touch each other. In short, the metal particle preferably has a rounded outline when viewed from above. In addition, the outline of the metal particle when viewed from above may also have a concave portion.
[0168] At least a part of the surface of the metal particles is preferably coated with a polymer, and more preferably coated with at least one polymer selected from the group consisting of cellulose acetate butyrate, cellulose acetate propionate, and cellulose acetate.
[0169] When the surface of the metal particles is coated with the polymer, the metal particles are pushed to the air-liquid interface of the ink together with the polymer due to the surface energy of the polymer. The metal particles gather at the air-liquid interface of the ink and are concentrated on the surface of the ink film after the ink is cured, so an image with excellent metallic gloss can be obtained.
[0170] The metal particles coated with the polymer are preferably release sheets of a metal film. The release sheet of a metal film can be obtained, for example, by the following method.
[0171] At least one polymer selected from the group consisting of cellulose acetate butyrate, cellulose acetate propionate and cellulose acetate is applied to a substrate to form a polymer layer. A metal film containing a metal is formed on the polymer layer. The polymer layer is dissolved to peel off the metal film. Metal particles can be obtained by disintegrating or crushing the metal film.
[0172] The metal film may be peeled off with the polymer layer adsorbed on one side. By disintegrating or crushing the metal film with the polymer layer adsorbed on one side, metal particles coated with the polymer can be obtained.
[0173] As a method for forming a metal film, evaporation, sputtering, etc. can be cited. For example, a metal film containing indium does not form a continuous film during evaporation, but forms an island structure dispersed in an island shape. Therefore, without applying a large force, metal particles can be obtained only by breaking them up. When viewed from above, the peeling piece of the metal film containing indium (that is, the metal particles containing indium) has an R-shaped profile.
[0174] The content of the metal particles is preferably 0.5% by mass to 10% by mass, and more preferably 1.0% by mass to 8.0% by mass, based on the total amount of the second ink.
[0175] (Polymerizable compound)
[0176] The second ink contains at least one polymerizable compound.
[0177] Examples of the polymerizable compound contained in the second ink include the same examples as those of the polymerizable compound contained in the first ink.
[0178] Among them, from the viewpoint of reducing surface curability, the second ink preferably contains the polymerizable compound B. When the surface curability of the second ink film is reduced, the smoothness of the second ink film surface is improved, a visually heavy image is obtained, and metallic gloss is improved.
[0179] The second ink preferably contains a polyfunctional polymerizable compound as the polymerizable compound. When the second ink contains a polyfunctional polymerizable compound, a second ink film having excellent curability can be formed.
[0180] The content of the multifunctional polymerizable compound is preferably 40% by mass or more, more preferably 50% by mass or more, relative to the total amount of the second ink. The upper limit of the content is not particularly limited, and is, for example, 80% by mass.
[0181] The second ink preferably contains a fluorine-containing polymerizable compound, and the fluorine-containing polymerizable compound is a polymerizable compound containing fluorine atoms. The number of fluorine atoms contained in the fluorine-containing polymerizable compound may be only one, or may be two or more.
[0182] In the present invention, the fluorine-containing polymerizable compound refers to a compound having a fluorine atom and a polymerizable group.
[0183] Fluorine-containing polymerizable compounds are easily inhibited from polymerization by oxygen. Therefore, if the second ink contains a fluorine-containing polymerizable compound, the curability of the surface of the second ink film decreases. In the process of curing the second ink film by polymerizing the polymerizable compound contained in the second ink, the surface of the second ink film is cured in a smooth state, and a second ink film having a smooth surface is formed, thereby obtaining an image with excellent metallic gloss.
[0184] From the viewpoint of reactivity, the fluorine-containing polymerizable compound is preferably a (meth)acrylate having a fluorine atom.
[0185] Examples of the fluorine-containing polymerizable compound include trifluoroethyl 2,2,2-(meth)acrylate, tetrafluoropropyl 2,2,3,3-(meth)acrylate, hexafluorobutyl 2,2,3,4,4,4-(meth)acrylate, hexafluoro-2-(meth)acrylate propyl, octafluoropentyl 2,2,3,3,4,4,5,5-(meth)acrylate, 3,3,4,4,5,5,6,6,6-(meth)acrylate nonafluorohexyl 2,2,3,3,4,4,5,5,6,6,7,7-(meth)acrylate dodecafluoroheptyl and 3,3,4,4,5,5,6,6,7,7,8,8,8-(meth)acrylate tridecafluorooctyl.
[0186] The content of the fluorine-containing polymerizable compound is preferably 0.5% by mass to 10% by mass, more preferably 1.0% by mass to 5.0% by mass, based on the total amount of the second ink.
[0187] In the second ink, the total content of all polymerizable compounds contained in the second ink is preferably 70% by mass to 90% by mass, and more preferably 75% by mass to 85% by mass, based on the total amount of the second ink.
[0188] (Photopolymerization Initiator)
[0189] The second ink preferably contains at least one photopolymerization initiator.
[0190] Preferred aspects of the photopolymerization initiator contained in the second ink are the same as preferred aspects of the photopolymerization initiator contained in the first ink.
[0191] (Surfactant)
[0192] The second ink may contain at least one surfactant.
[0193] From the viewpoint of setting the surface tension of the second ink to 30 mN / m or more, the second ink preferably does not contain a surfactant or contains a surfactant in an amount of less than 0.01% by mass.
[0194] (Inhibitor)
[0195] The second ink preferably contains at least one polymerization inhibitor.
[0196] Preferred embodiments of the polymerization inhibitor contained in the second ink are the same as preferred embodiments of the polymerization inhibitor contained in the first ink.
[0197] (Other ingredients)
[0198] The second ink may contain other components in addition to the above-mentioned components as necessary.
[0199] Examples of other components include colorants (eg, pigments, dyes), resins, dispersants, waxes, antioxidants, anti-fading agents, conductive salts, and basic compounds.
[0200] (physical properties)
[0201] The surface tension of the second ink of the present invention is preferably 30 mN / m or more. If the surface tension of the second ink is 30 mN / m or more, the metal particles are easily gathered at the air-liquid interface, and the metal particles are localized on the image surface, thereby improving the metallic gloss of the image.
[0202] From the viewpoint of image quality, the surface tension of the second ink is preferably 40 mN / m or less. That is, the surface tension of the second ink is preferably 30 mN / m to 40 mN / m, and more preferably 32 mN / m to 38 mN / m.
[0203] The viscosity of the second ink is preferably 5 mPa·s to 50 mPa·s, more preferably 10 mPa·s to 30 mPa·s, and even more preferably 10 mPa·s to 25 mPa·s.
[0204] [Image recording method]
[0205] The image recording method of the present invention uses the above-mentioned ink set, and the image recording method includes: a step of applying a first ink to a substrate using an inkjet recording method (hereinafter also referred to as a "first ink applying step"); a step of irradiating the first ink applied to the substrate with active energy rays A to form a first ink film (hereinafter also referred to as a "first ink film forming step"); a step of applying a second ink to the first ink film using an inkjet recording method (hereinafter also referred to as a "second ink applying step"); and a step of irradiating the second ink applied to the first ink film with active energy rays B to record an image (hereinafter also referred to as an "image recording step").
[0206] <First ink application step>
[0207] The first ink applying step includes a step of applying the first ink on the substrate using an inkjet recording method.
[0208] The substrate may be a permeable substrate such as paper or a non-permeable substrate.
[0209] In the image recording method of the present invention, an image is recorded by irradiating with active energy rays. Therefore, even when the substrate is a non-permeable substrate, it is easy to ensure the adhesion between the substrate and the image.
[0210] In the present invention, the impermeable substrate refers to a substrate having a water absorption rate (mass %, 24 hours) of less than 0.2 as measured according to ASTM D570 of the ASTM test method.
[0211] In the present invention, the permeable substrate refers to a substrate having a water absorption rate (mass %, 24 hours) of 0.2 or more as measured according to ASTM D570 of the ASTM test method.
[0212] Examples of the impermeable substrate include glass, quartz, plastic films, and leather.
[0213] Examples of the resin constituting the plastic film include cellulose diacetate, cellulose triacetate, cellulose propionate, cellulose butyrate, cellulose acetate butyrate, cellulose nitrate, acrylic resin, chlorinated polyolefin resin, polyethersulfone resin, polyethylene terephthalate (PET), polyethylene naphthalate, nylon, polyethylene, polystyrene (PS), polypropylene (PP), polycycloolefin resin, polyimide resin, polycarbonate (PC) resin, and polyvinyl acetal.
[0214] The plastic film may be a film containing only one type of these resins, or may be a film containing two or more types.
[0215] Examples of leather include natural leather (also referred to as "genuine leather"), synthetic leather (eg, PVC (polyvinyl chloride) leather, PU (polyurethane) leather), etc. For leather, for example, see paragraphs 0163 to 0165 of Japanese Patent Application Laid-Open No. 2009-058750.
[0216] The thickness of the impermeable substrate is not particularly limited, but is preferably 10 μm to 2000 μm, more preferably 20 μm to 1000 μm, further preferably 30 μm to 500 μm, and particularly preferably 30 μm to 400 μm.
[0217] Examples of the permeable substrate include paper and cloth.
[0218] Examples of paper include uncoated paper (for example, premium paper), coated paper, cardboard, liner paper for corrugated board, cloth, etc. Cardboard may be provided with a coating layer.
[0219] As the permeable substrate, coated paper and coated paperboard are preferred. Since the ink permeates slowly, the metallic gloss of the recorded image tends to be more prominent.
[0220] The inkjet recording method is not particularly limited as long as it can record an image, and a known method can be used. Examples of the inkjet recording method include a charge control method that uses electrostatic induction force to eject ink, a drop-on-demand method (pressure pulse method) that uses vibration pressure of a piezoelectric element, an acoustic inkjet method that converts an electrical signal into an acoustic beam and irradiates the ink to eject the ink using radiation pressure, and a thermal inkjet (Bubble Jet (registered trademark)) method that heats the ink to form bubbles and uses the generated pressure.
[0221] Examples of inkjet heads used in inkjet recording include a shuttle method that uses a short serial head to scan the head in the width direction of the substrate and perform recording, and a line method that uses a line head with recording elements arranged over the entire area of one side of the substrate.
[0222] In the inline method, by scanning the substrate in a direction intersecting the arrangement direction of the recording elements, a pattern can be formed on the entire surface of the substrate, and a transport system such as a carriage for scanning a short head is not required. In addition, in the inline method, there is no need to perform complex scanning control on the movement of the carriage and the substrate, and only the substrate is moved, so the recording speed can be increased compared to the reciprocating method.
[0223] The ejection amount of the ink ejected from the inkjet head is preferably 1 pL (picoliter) to 100 pL, more preferably 3 pL to 80 pL, and even more preferably 3 pL to 50 pL.
[0224] <First ink film forming step>
[0225] The first ink film forming step includes a step of irradiating the first ink applied onto the substrate with active energy rays A to form a first ink film.
[0226] In the first ink film forming step, the first ink applied to the substrate is irradiated with active energy rays A to polymerize the polymerizable compound in the first ink to form the first ink film. The active energy rays A are preferably ultraviolet rays.
[0227] The peak wavelength of ultraviolet rays is, for example, preferably 200 nm to 405 nm, more preferably 250 nm to 400 nm, and further preferably 300 nm to 400 nm.
[0228] As the light source for ultraviolet irradiation, mercury lamps, gas lasers and solid lasers are mainly used, and the most well-known ones are mercury lamps, metal halide lamps and ultraviolet fluorescent lamps. In addition, UV-LED (light emitting diode) and UV-LD (laser diode) have the characteristics of small size, long life, high efficiency and low cost, and are expected to become the light source for ultraviolet irradiation. Among them, the light source for ultraviolet irradiation is preferably a metal halide lamp, a high-pressure mercury lamp, a medium-pressure mercury lamp, a low-pressure mercury lamp or a UV-LED.
[0229] In the first ink film forming step, the content of the photopolymerization initiator in the first ink is less than 1% by mass relative to the total amount of the ink, and the first ink is cured by irradiation with electron beams as active energy rays A. Since the content of the photopolymerization initiator is less than 1% by mass, the elution of the photopolymerization initiator from the image can be further suppressed. Therefore, for example, the method is particularly preferred as a method for producing an image recorded material for food packaging.
[0230] In the first ink film forming step, the first ink film may be preliminarily cured, or the first ink film may be fully cured.
[0231] Here, in short, the full curing means that substantially all of the polymerizable compounds in the ink film are polymerized to substantially completely cure the ink film.
[0232] Specifically, the main curing means that the polymerizable compound in the ink film is polymerized until the curing rate of the ink film (ie, the polymerization rate of the polymerizable compound determined by high performance liquid chromatography) reaches 90% to 100%, thereby curing the ink film.
[0233] In the present invention, irradiation with active energy rays for main curing may be referred to as “curing exposure”, and active energy rays for main curing may be referred to as “curing exposure light”.
[0234] On the other hand, pre-curing is, in short, polymerizing only a part of the polymerizable compound in the ink film.
[0235] Specifically, the pre-curing is to polymerize a part of the polymerizable compound in the ink film to such an extent that the curing rate of the ink film is less than 90%, thereby pre-curing the ink film.
[0236] In the present invention, irradiation with active energy rays for preliminary curing may be referred to as “needle fixed exposure”, and active energy rays for preliminary curing may be referred to as “needle fixed exposure light”.
[0237] In the first ink film forming step, when the first ink is applied to the entire surface of the substrate, it is preferred that the first ink film be fully cured.
[0238] From the viewpoint of further improving the adhesion between the substrate and the image, the illuminance of the active energy ray A as the curing exposure light is preferably 1.0 W / cm 2 More preferably, 2.0 W / cm 2 More preferably, 4.0 W / cm 2 above.
[0239] The upper limit of the illuminance of the active energy ray A as the curing exposure light is not particularly limited, but is, for example, 10 W / cm 2 .
[0240] From the viewpoint of further improving the adhesion between the substrate and the image, the irradiation energy (i.e., exposure amount) of the active energy ray A as the curing exposure light is preferably 500 mJ / cm 2 More preferably, 800 mJ / cm 2 above.
[0241] The upper limit of the exposure amount of the active energy ray A as the curing exposure light is not particularly limited, and is, for example, 2000 mJ / cm 2 .
[0242] <Second ink application step>
[0243] The second ink applying step includes a step of applying the second ink on the first ink film using an inkjet recording method.
[0244] A preferred embodiment of the method of applying the second ink is the same as a preferred embodiment of the method of applying the first ink.
[0245] <Image recording process>
[0246] The image recording step includes irradiating the second ink applied to the first ink film with active energy rays B to record an image.
[0247] In the image recording step, the second ink applied to the first ink film is irradiated with active energy rays B, so that the polymerizable compound in the second ink is polymerized to form a second ink film. Thus, an image is recorded. The active energy rays B are preferably ultraviolet rays.
[0248] The active energy ray B is preferably curing exposure light.
[0249] A preferred embodiment of the active energy ray B as the curing exposure light is the same as a preferred embodiment of the active energy ray A as the curing exposure light.
[0250] The image recording step preferably includes: a step of pre-curing the second ink by irradiating an active energy ray B1 having an irradiation energy lower than that of the active energy ray B; and a step of irradiating the ink film formed by the pre-curing of the second ink with the active energy ray B. If the image recording step includes the pre-curing step, the line quality of the image is improved.
[0251] The curing rate of the pre-cured second ink film is more preferably 80% or less, further preferably 70% or less, and further preferably 50% or less.
[0252] The curing rate of the pre-cured second ink film is preferably 10% or more, more preferably 20% or more, and even more preferably 30% or more.
[0253] The illuminance of the active energy ray B1 as the pin-fixed exposure light is preferably 0.10 W / cm 2 ~0.50W / cm 2 , more preferably 0.20 W / cm 2 ~0.49W / cm 2 , more preferably 0.20W / cm 2 ~0.45W / cm 2 .
[0254] The irradiation energy (i.e., exposure amount) of the active energy ray B1 as the needle fixed exposure light is preferably 50 mJ / cm 2 ~500mJ / cm 2 , more preferably 100 mJ / cm 2 ~300mJ / cm 2 .
[0255] The image recording method of the present invention may include other steps in addition to the above steps. For example, the image recording method of the present invention may further include: a step of applying a third ink, which is an active energy ray-curable inkjet ink containing a colorant and a polymerizable compound, to a second ink film formed by the second ink using an inkjet recording method; and a step of irradiating the third ink applied to the second ink film with active energy rays C to record an image.
[0256] As the colorant contained in the third ink, a generally known colorant can be used, and the irradiation of the active energy ray C can be performed by the same method as the irradiation of the above-mentioned active energy ray A. By applying the third ink (specifically, a colored ink) on the second ink film, a color metallic image can be obtained.
[0257] Furthermore, for example, the image recording method of the present invention may further include: a step of applying a fourth ink, which is an active energy ray-curable inkjet ink containing a polymerizable compound, to a third ink film formed of the third ink using an inkjet recording method; and a step of recording an image by irradiating the fourth ink applied to the third ink film with active energy rays D. The fourth ink is a transparent ink containing no colorant.
[0258] The irradiation with the active energy ray D can be performed by the same method as the irradiation with the active energy ray A. By applying the fourth ink (specifically, transparent ink) on the third ink film, a glossy colored metallic image can be obtained.
[0259] [Visual Records]
[0260] The image recorded material of the present invention includes a substrate and an image arranged on the substrate, the image including: a first ink layer formed on the surface of the substrate; and a second ink layer formed on the surface of the first ink layer, wherein metal particles containing indium are present only in a region up to 70% of the thickness of the second ink layer from the surface of the second ink layer toward the inside of the second ink layer.
[0261] Preferred embodiments of the substrate in the image recorded article of the present invention are as described in the above-mentioned image recording method section.
[0262] The image disposed on the substrate is preferably an image recorded on the substrate using the above-mentioned image recording method. Specifically, the above-mentioned first ink can be applied to the substrate, and the first ink applied to the substrate can be irradiated with active energy rays, thereby forming a first ink layer. Furthermore, the above-mentioned second ink can be applied to the first ink layer, and the second ink applied to the first ink layer can be irradiated with active energy rays, thereby forming a second ink layer. Therefore, it is preferred that the first ink layer contains a polymer of the polymerizable compound contained in the above-mentioned first ink. Furthermore, it is preferred that the second ink layer contains a polymer of the polymerizable compound contained in the above-mentioned second ink.
[0263] In the image recorded material of the present invention, the second ink layer contains metal particles containing indium, and the metal particles containing indium are present only in a region up to 70% of the thickness of the second ink layer from the surface of the second ink layer (i.e., the surface of the image) toward the inside of the second ink layer. In other words, the metal particles containing indium are not present in a region up to 30% of the thickness of the second ink layer from the interface between the first ink layer and the second ink layer toward the inside of the second ink layer.
[0264] In the image recorded material of the present invention, the metal particles containing indium are concentrated near the surface of the image, so that a sense of thickness can be visually obtained.
[0265] Preferred embodiments of the metal particles containing indium are as described in the above-mentioned image recording method section.
[0266] Example
[0267] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to the following Examples unless it departs from the gist of the present invention.
[0268] <Preparation of Metal Particle Dispersion>
[0269] (1) Indium particle dispersion
[0270] A 5.0 mass % solution of cellulose acetate butyrate dissolved in ethyl acetate was applied on a polyethylene terephthalate (PET) film having a film thickness of 50 μm using a gravure coater, and the coating solution was dried to form a polymer layer.
[0271] A metal film including indium is formed on the polymer layer by vacuum evaporation to obtain a laminate including a PET film, a polymer layer and a metal film. The laminate is immersed in propylene glycol monomethyl ether (PGME) to dissolve the polymer layer. An ultrasonic disperser is used to perform micronization and dispersion treatment to obtain an indium particle dispersion containing indium particles whose surface is at least partially coated with a polymer.
[0272] The obtained dispersion liquid is filtered through a SUS mesh filter having a pore size of 5 μm, and the solvent is removed or added by an evaporator or the like as necessary, thereby obtaining an indium particle dispersion liquid having a predetermined concentration.
[0273] (2) Aluminum particle dispersion
[0274] An aluminum particle dispersion was obtained by the same method as that for the indium particle dispersion except that indium was replaced by aluminum.
[0275] <Preparation of the first ink>
[0276] The first ink was prepared by mixing the components such that the contents (mass %) of the polymerizable compound, the photopolymerization initiator, the polymerization inhibitor, and the surfactant became the values shown in Tables 2 to 4.
[0277] <Preparation of the second ink>
[0278] -Preparation of the second ink M1-
[0279] The following components were mixed into the following composition to prepare the second ink M1.
[0280] ·Indium particle dispersion...6 mass%
[0281] ·DPGDA……50.2% by mass
[0282] PEGDA400……9.3% by mass
[0283] CTFA: 20% by mass
[0284] TFEA……2.5% by mass
[0285] ·Omni.819……4% by mass
[0286] ·TPO……6% by mass
[0287] ·UV22……1.5% by mass
[0288] ·MEHQ……0.5% by mass
[0289] -Preparation of the second ink M2-
[0290] The following components were mixed into the following composition to prepare the second ink M2.
[0291] ·Indium particle dispersion...6 mass%
[0292] ・ISTA……30% by mass
[0293] ·3MPDDA……41% by mass
[0294] ·TCDDMDA……11% by mass
[0295] ·Omni.819……4% by mass
[0296] ·TPO……6% by mass
[0297] ·UV22……1.5% by mass
[0298] ·MEHQ……0.5% by mass
[0299] -Preparation of the second ink M3-
[0300] The second ink M3 was prepared in the same manner as the second ink M1 except that the indium particle dispersion in the second ink M1 was changed to an aluminum particle dispersion.
[0301] The details of each component contained in the first ink and the second ink are as follows.
[0302] (Polymerizable compound A (polymerizable compound having an amide structure))
[0303] ACMO: Acryloylmorpholine
[0304] AO: 3-Acryloyl-2-oxazolidinone
[0305] NVP: N-vinyl pyrrolidone
[0306] NVC: N-vinyl caprolactam
[0307] DMAA: N,N-dimethylacrylamide
[0308] ·HEAA: Hydroxyethyl acrylamide
[0309] BMAA: N-Butoxymethylacrylamide
[0310] EBAA: N,N'-vinylidenebisacrylamide
[0311] PAA: N-phenylacrylamide
[0312] ·PrAA: N-propylacrylamide
[0313] (Polymerizable compound B (monofunctional polymerizable compound including at least one structure selected from the group consisting of a cyclic ether structure and an alicyclic structure))
[0314] CTFA: Cyclic trimethylolpropane formal acrylate (product name "VISCOAT#200", manufactured by OSAKA ORGANIC CHEMICAL INDUSTRY LTD.)
[0315] (Other polymerizable compounds)
[0316] ·4-HBA: 4-Hydroxybutyl acrylate (product name "4-HBA", manufactured by OSAKA ORGANIC CHEMICAL INDUSTRY LTD.)
[0317] NPGPODA: Propylene oxide-modified neopentyl glycol diacrylate (product name "SR9003NS", manufactured by Sartomer)
[0318] DPGDA: dipropylene glycol diacrylate (product name "SR508", manufactured by Sartomer)
[0319] PEGDA400: Polyethylene glycol (400) diacrylate (product name "SR344", manufactured by Sartomer)
[0320] TFEA: 2,2,2-trifluoroethyl acrylate (product name "VISCOAT 3F", manufactured by OSAKA ORGANIC CHEMICAL INDUSTRY LTD.)
[0321] ISTA: Octadecyl acrylate (product name "ISTA", manufactured by OSAKA ORGANIC CHEMICAL INDUSTRY LTD.)
[0322] 3MPDDA: 3-methyl-1,5-pentanediol diacrylate (product name "SR341", manufactured by Sartomer)
[0323] TCDDMDA: tricyclodecane dimethanol diacrylate (product name "SR833S", manufactured by Sartomer)
[0324] (Photopolymerization Initiator)
[0325] Omni.819: Bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (product name "Omnirad 819", manufactured by IGM Resins BV)
[0326] ·TPO: 2,4,6-trimethylbenzoyldiphenylphosphine oxide (product name "Speedcure TPO", manufactured by Lambson)
[0327] (Inhibitor)
[0328] UV12: tris(N-nitroso-N-phenylhydroxylamine)aluminum salt (product name "FLORSTAB UV-12", manufactured by Kromachem)
[0329] UV22: A mixture of 2,6-bis(1,1-dimethylethyl)-4-(phenylmethylene)-2,5-cyclohexadien-1-one and propoxylated glycerol triacrylate (product name "IRGASTAB UV-22", manufactured by BASF)
[0330] ·MEHQ: 4-methoxyphenol (manufactured by Tokyo Chemical Industry Co., Ltd.)
[0331] (Surfactant)
[0332] UV3500: Polyether-modified polydimethylsiloxane having an acryloyl group (product name "BYK-UV3500", manufactured by BYK)
[0333] <Image recording method 1>
[0334] A single-pass inkjet ejection device (Samba head manufactured by Fujifilm Dimatix) was used to introduce the first ink into the first head and the second ink into the second head. A VIEWFUL PET (thickness 188 μm) was prepared as a substrate. The first ink was applied to the substrate in a solid image shape (solid image shape) of 1200 dpi×1200 dpi and 100% dot rate, and curing exposure light was irradiated as active energy ray A to form a first ink film (first ink application step, first ink film formation step).
[0335] Then, the second ink was applied onto the first ink film, and 10 seconds later, curing exposure light was irradiated as active energy rays B to obtain an image recorded object (second ink applying step, image recording step).
[0336] The curing exposure light was ultraviolet light with a peak wavelength of 385 nm. The irradiation energy of the curing exposure light was set to 1000 mJ / cm 2 .
[0337] In addition, in Comparative Example 1, the first ink was not used.
[0338] <Image recording method 2>
[0339] The first ink was introduced into the white throttle valve and the second ink was introduced into the transparent throttle valve of a multi-pass (i.e., shuttle scanning) inkjet printer (product name "Acuity LED 1600R", manufactured by FUJIFILM Corporation). VIEWFUL PET (thickness 188 μm) was prepared as a substrate.
[0340] The first ink was applied to the substrate in the form of a solid image with a dot rate of 100% and a hollow character image pattern with 2, 4, 6, 8, and 10 dots (first ink applying step).
[0341] The ink application conditions were set to 1200 dpi×1200 dpi (dots per inch), 48 passes, and bidirectional printing.
[0342] The first ink applied to the substrate is irradiated with curing exposure light as active energy rays A by setting the lamp operation of the inkjet printer, thereby forming a first ink film (first ink film forming step).
[0343] The curing exposure light was ultraviolet light with a peak wavelength of 385 nm. The irradiation energy of the curing exposure light was set to 1000 mJ / cm 2 .
[0344] The second ink was applied to the first ink film in a solid image state (Solid image state) with a dot rate of 100% and a hollow character image pattern of 2, 4, 6, 8, and 10 points (second ink application process). When the first ink was applied in a solid image state, the second ink was applied in a solid image state. Furthermore, when the first ink was applied in a hollow character image pattern, the second ink was applied in the same hollow character image pattern.
[0345] The ink application conditions were set to 1200 dpi×1200 dpi (dots per inch), 48 passes, and bidirectional printing.
[0346] By setting the light operation of the inkjet printer, the second ink applied to the first ink film is sequentially irradiated with the needle-fixed exposure light (exposure light for pre-curing) as the active energy ray B1 and the curing exposure light (exposure light for formal curing) as the active energy ray B, thereby obtaining an image record (image recording process).
[0347] The time from the second ink landing on the first ink film to the pin fixed exposure light being irradiated is 0.1 seconds.
[0348] The time from when the second ink landed on the first ink film to when the curing exposure light was irradiated was 2.0 seconds.
[0349] Here, the fixing exposure light is ultraviolet light having a peak wavelength of 385 nm, and the curing exposure light is ultraviolet light having a peak wavelength of 385 nm.
[0350] The irradiation energy of the fixed exposure light was set to 200 mJ / cm 2 The curing exposure light irradiation energy is set to 1000mJ / cm 2 .
[0351] In addition, in Comparative Example 1, the first ink was not used.
[0352] The obtained image records were used to evaluate brightness, metallic gloss, and image quality. The evaluation method was as follows.
[0353] (Brightness)
[0354] The L in the image recorded material produced by the image recording method 1 was measured using a fluorescence spectrodensitometer (product name "FD-7", manufactured by Konica Minolta, Inc.). * In addition, L * The lower the value of , the thicker the image will be visually. The evaluation criteria are as follows.
[0355] A: L * Less than 25.
[0356] B:L * 25 or more and less than 30
[0357] C:L * It is 30 or more and less than 35.
[0358] D:L * 35 and above.
[0359] (Metallic luster)
[0360] The 20° glossiness of the solid image in the image recorded by the image recording method 2 was measured using a gloss meter (product name "micro-gloss micro triangle gloss meter", manufactured by BYK-Gardner). The higher the 20° glossiness, the better the metallic glossiness. The evaluation criteria are as follows.
[0361] AA: 20° glossiness is 600 or more.
[0362] A: 20° glossiness is 400 or more and less than 600.
[0363] B: 20° glossiness is 200 or more and less than 400.
[0364] C: 20° glossiness is 100 or more and less than 200.
[0365] D: 20° glossiness is less than 100.
[0366] (Image quality)
[0367] The hollow character images of the image recorded product produced by the image recording method 2 were visually observed from a position 20 cm away from the image recorded product, and the image quality was evaluated based on whether or not the hollow character images were visually recognizable. The evaluation criteria are as follows.
[0368] A: Can visually recognize hollow text images of 2 points or more.
[0369] B: Able to visually recognize hollow text images of 4 points or more.
[0370] C: Able to visually recognize hollow text images of 8 points or more.
[0371] D: Only the hollow text image of 10 points can be visually identified.
[0372] The evaluation results are shown in Tables 2 to 4. In Tables 2 to 4, "polymerizable compound A" refers to a polymerizable compound having an amide structure. "Polymerizable compound B" refers to a monofunctional polymerizable compound including at least one structure selected from the group including a cyclic ether structure and an alicyclic structure. "Other polymerizable compounds" refer to polymerizable compounds that do not belong to any of polymerizable compound A and polymerizable compound B. "Number of functional groups" refers to the number of polymerizable groups contained in the polymerizable compound. "The proportion of polyfunctional polymerizable compounds" refers to the proportion (mass %) of polyfunctional polymerizable compounds in all polymerizable compounds. "Metal species" refers to the type of metal contained in the metal particles.
[0373] [Table 2]
[0374]
[0375] [Table 3]
[0376]
[0377] [Table 4]
[0378]
[0379] As shown in Tables 2 to 4, the ink set of Examples 1 to 19 comprises: a first ink containing a polymerizable compound; and a second ink containing metal particles containing indium and a polymerizable compound. The surface tension of the first ink is greater than 30 mN / m, so when high-speed printing is performed, it is possible to record images with excellent metallic gloss and a visually thick feel.
[0380] In Comparative Example 1, since the first ink was not used, the brightness of the image surface was high, and a visually thick image could not be obtained. This is considered to be because the speed at which the metal particles localized at the air-liquid interface was slow after the second ink was applied.
[0381] In Comparative Example 2, since the surface tension of the first ink was less than 30 mN / m, the brightness of the image surface was high, and a visually heavy image could not be obtained. In addition, the metallic gloss of the image was not obtained. This is considered to be because the metal particles were not localized at the gas-liquid interface after the second ink was applied.
[0382] In Comparative Example 3, the metal particles contained in the second ink did not contain indium, so the brightness of the image surface was high, and a visually heavy image was not obtained. In addition, the metallic gloss of the image was not obtained.
[0383] In addition, the disclosure of Japanese Patent Application No. 2022-087675 filed on May 30, 2022 is incorporated into this specification by reference in its entirety. Furthermore, all documents, patent applications, and technical standards described in this specification are incorporated into this specification by reference to the same extent as if each document, patent application, and technical standard incorporated by reference was specifically and separately described.
Claims
1. An ink set comprising: The first ink is an active energy ray-curable inkjet ink containing a polymerizable compound; and The second ink is an active energy ray-curable inkjet ink containing metal particles containing indium and a polymerizable compound. The surface tension of the first ink is 30 mN / m or more.
2. The ink set according to claim 1, wherein: The polymerizable compound contained in the first ink includes a polymerizable compound having an amide structure.
3. The ink set according to claim 2, wherein: The content of the polymerizable compound having an amide structure is 5% by mass to 50% by mass based on the total amount of the first ink.
4. The ink set according to claim 1, wherein: The polymerizable compound contained in the first ink includes a polyfunctional polymerizable compound.
5. The ink set according to claim 4, wherein: The ratio of the polyfunctional polymerizable compound in the polymerizable compound is 1% by mass to 50% by mass.
6. The ink set according to claim 1, wherein: The polymerizable compound contained in the first ink includes a monofunctional polymerizable compound including at least one structure selected from the group consisting of a cyclic ether structure and an alicyclic structure.
7. The ink set according to claim 1, wherein: The polymerizable compound contained in the first ink includes a polymerizable compound having an amide structure and a monofunctional polymerizable compound including at least one structure selected from the group consisting of a cyclic ether structure and an alicyclic structure.
8. An image recording method using the ink set according to any one of claims 1 to 7, The image recording method comprises: A step of applying the first ink to a substrate using an inkjet recording method; a step of irradiating the first ink applied onto the substrate with active energy rays A to form a first ink film; a step of applying the second ink to the first ink film by inkjet recording; and A step of irradiating the second ink applied to the first ink film with active energy rays B to record an image.
9. The image recording method according to claim 8, wherein: The process of recording the image includes: a step of pre-curing the second ink by irradiating with an active energy ray B1 having less energy than the active energy ray B; and A step of irradiating the ink film formed by the preliminary curing of the second ink with the active energy ray B.
10. An image recorded article comprising a substrate and an image disposed on the substrate, The images include: a first ink layer formed on the surface of the substrate; and a second ink layer formed on the surface of the first ink layer, The metal particles containing indium exist only in a region up to 70% of the thickness of the second ink layer from the surface of the second ink layer toward the inside of the second ink layer.