Supported silver catalyst as well as preparation method and application thereof
Through step-by-step impregnation and calcination, a supported silver catalyst with high selectivity and stability was prepared, which solved the problem of insufficient catalyst selectivity and ethylene oxide yield in the prior art, and achieved high activity and low cost catalytic effect.
Patent Information
- Application Number
- CN202411085093.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
AI Technical Summary
In the process of ethylene oxidation to ethylene oxide, the selectivity and ethylene oxide yield of the existing silver catalysts are insufficient, and the service life is short, so it is necessary to improve the spatio-temporal yield and stability of the catalyst.
The silver particles, additives and co-adjuvant are attached to the support by step-by-step impregnation method, and the supported silver catalyst with high selectivity and stability is prepared by step-by-step calcination activation. The specific steps include the support in the rhenium-containing salt liquid. Immerse, dry and calcined, followed by re-impregnation and calcination in silver salts, amine-based organic compounds and cesium salts.
A silver catalyst with high selectivity and high activity was achieved, with an ethylene oxide yield of 2.62 mol%, a silver content of precious metals, a small industrial investment cost, and excellent performance and stability.
Smart Images

Figure CN118988309A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of silver catalysts, and in particular to a supported silver catalyst and a preparation method and application thereof. Background Art
[0002] Ethylene oxide (EO) is an important petrochemical intermediate, widely used in the synthesis of ethylene glycol and other polyols. Industrial production mainly adopts the direct reaction of ethylene and oxygen, and most of its production equipment is equipped with ethylene oxide hydration to produce ethylene glycol (EG). The main uses of ethylene glycol are synthetic polyester fibers, bottle resins, films, antifreeze and coolants. In recent years, my country's polyester industry has developed rapidly, and the demand for ethylene glycol has increased rapidly. my country's ethylene oxide / ethylene glycol production capacity and output have increased year by year, and the demand for silver catalysts for ethylene oxide production has therefore expanded.
[0003] The research and development focus of ethylene oxidation to ethylene oxide production technology is catalysts. Silver catalysts are generally based on α-alumina or modified α-alumina as carriers, loaded with the main active substance silver, and a certain amount of additives and co-additives are added to improve the performance of the catalyst. In the actual application of the catalyst, the three performance indicators of activity, selectivity and stability are mainly examined.
[0004] Improving the carrier or adding effective additives during the preparation of the silver catalyst will help improve the selectivity and activity of the catalyst. Patent CN111683750A proposes a component of a silver impregnation solution, which mainly includes silver ions, a polar organic additive containing 2-4 carbon atoms and 2-4 functional groups selected from hydroxyl, carboxylic acid and amine groups. U.S. Patent 4766105 describes an ethylene oxide catalyst comprising silver, alkali metals, rhenium and co-auxiliaries, and the co-auxiliaries are mainly sulfur, molybdenum, tungsten, chromium and mixtures thereof. U.S. Patent US2014 / 0179516A1 discloses a catalyst for preparing ethylene oxide from ethylene, which is prepared by loading silver, cesium and rhenium on a carrier, and the selectivity is improved. US2013 / 0296587A1 describes a tungsten-free catalyst for epoxidation of olefins, which is loaded with silver, molybdenum and tin on the carrier to improve activity and selectivity. The above patented technologies all improve the performance of the catalyst by improving the impregnation liquid method, but the selectivity of the catalyst and the yield of ethylene oxide are insufficient. It is necessary to increase the catalyst space-time yield and extend the service life of the catalyst. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a supported silver catalyst and a preparation method and application thereof.
[0006] In a first aspect, the present invention provides a method for preparing a supported silver catalyst, the preparation method comprising the following steps:
[0007] The carrier is impregnated in a first impregnation solution containing a rhenium salt, and then centrifuged, dried, and first calcined for activation to obtain a first carrier;
[0008] The first carrier is immersed in a second impregnation solution containing a silver salt, an amine organic compound and a cesium salt, and then allowed to stand and taken out to obtain a silver catalyst precursor;
[0009] Under an inert gas atmosphere, the silver catalyst precursor is subjected to a second calcination activation to obtain the supported silver catalyst.
[0010] Furthermore, in terms of weight percentage, the concentration of the rhenium salt in the first impregnation solution is 0.05-0.3 g / mL; the rhenium salt includes ammonium perrhenate.
[0011] Furthermore, the step of immersing the carrier in a first impregnation solution containing rhenium salt includes: placing the carrier in a rotary evaporator, vacuuming the carrier at 0.1-0.2 MPa for 1-4 hours, injecting the first impregnation solution containing rhenium salt, and immersing the carrier for 1-3 hours.
[0012] Furthermore, the working condition parameters of the first calcination activation include: temperature of 350-550° C., time of 15-45 minutes; the working condition parameters of the second calcination activation include: temperature of 300-500° C., time of 3-20 minutes.
[0013] Furthermore, in terms of weight percentage, the concentration of silver salt in the second impregnation solution is 0.25-0.6 g / mL, and the silver salt includes silver oxalate; in terms of weight percentage, the concentration of cesium salt in the second impregnation solution is 0.05-0.4 g / mL, and the cesium salt includes cesium carbonate; in terms of weight percentage, the concentration of amine organic compound in the second impregnation solution is 0.45-0.85 g / mL, and the amine organic compound includes ethylenediamine.
[0014] Furthermore, the step of impregnating the first carrier in a second impregnation solution containing silver salt, amine organic compound and cesium salt includes: placing the carrier in a rotary evaporator, vacuuming it under the condition of 0.1-0.2Mpa for 1-4 hours, injecting the first impregnation solution containing rhenium salt, and impregnating it for 1-3 hours.
[0015] In a second aspect, the present invention provides a supported silver catalyst, wherein the supported silver catalyst is prepared by the method for preparing the supported silver catalyst described in any one of the first aspects.
[0016] In a third aspect, the present invention provides use of the supported silver catalyst described in any one of the second aspects in the production of ethylene oxide by oxidation of ethylene.
[0017] The above technical solution provided by the embodiment of the present invention has at least the following advantages compared with the prior art:
[0018] The embodiment of the present invention provides a method for preparing a supported silver catalyst. The present invention prepares a highly selective ethylene oxide silver catalyst, which uses a step-by-step impregnation method to attach silver particles, additives and co-auxiliaries to a carrier, and is characterized by excellent performance and good stability. The catalyst is activated after the step-by-step impregnation to promote the uniform distribution of nano-scale silver particles, additives and co-auxiliaries. The catalyst has a simple preparation process, stable performance, high catalytic activity and selectivity, low precious metal silver content, and low industrial input cost. Specifically:
[0019] 1. During the test, when the amount of raw materials added to the catalyst did not reach the industrial application limit, the yield of ethylene oxide could reach 2.62 mol%, indicating that the catalyst had a high space-time yield and excellent selectivity.
[0020] 2. Compared with existing catalysts, the use of precious metal silver has reached the industry-leading level, with the silver content accounting for only 16wt.% of the catalyst. In industrial production, the raw material cost is low, the economic investment is less, and it has more market competitive advantages. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0023] Figure 1 A schematic flow chart of a method for preparing a supported silver catalyst provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0026] In a first aspect, the present invention provides a method for preparing a supported silver catalyst, such as Figure 1 As shown, the preparation method comprises the following steps:
[0027] The carrier is impregnated in a first impregnation solution containing a rhenium salt, and then centrifuged, dried, and first calcined for activation to obtain a first carrier;
[0028] The first carrier is immersed in a second impregnation solution containing a silver salt, an amine organic compound and a cesium salt, and then allowed to stand and taken out to obtain a silver catalyst precursor;
[0029] Under an inert gas atmosphere, the silver catalyst precursor is subjected to a second calcination activation to obtain the supported silver catalyst.
[0030] The embodiment of the present invention provides a method for preparing a supported silver catalyst. The present invention prepares a highly selective ethylene oxide silver catalyst, wherein silver particles, an auxiliary agent and a co-auxiliary agent are attached to a carrier by a step-by-step impregnation method, and the catalyst is characterized by excellent performance and good stability. The catalyst is activated after the step-by-step impregnation to promote uniform distribution of nano-scale silver particles, auxiliary agents and co-auxiliary agents. The catalyst has a simple preparation process, stable performance, high catalytic activity and selectivity, low precious metal silver content, and low industrial input cost.
[0031] The preparation of the catalyst uses an α-alumina carrier. First, the carrier is placed in a rhenium solution for impregnation. After the impregnation is completed, a centrifugal device is used for solid-liquid separation, and then high-temperature roasting is performed in an inert gas (argon or nitrogen) to obtain a sample after the first impregnation. A secondary impregnation solution is prepared, which mainly includes an amine organic compound, silver, an auxiliary agent cesium and other alkali metal and alkaline earth metal co-auxiliaries. The sample after the first impregnation is placed in the secondary impregnation solution for impregnation, drained after completion, and then high-temperature roasting is performed in an inert gas (argon or nitrogen) to obtain the supported silver catalyst.
[0032] During the preparation process, the time and speed of centrifugation should be set to ensure that the outer surface of the carrier is covered with a layer of impregnation liquid and no water droplets are formed. The calcination temperature of the sample after the first impregnation is 350-550°C and the calcination time is 15-45 minutes. The calcination temperature of the sample after the second impregnation is 300-500°C and the calcination time is 3-20 minutes. A silver catalyst impregnated once was prepared as a control to illustrate the effect of step-by-step impregnation of rhenium compounds on the activity and selectivity of the catalyst.
[0033] In some specific embodiments, the carrier can be directly a commercially available product that meets the specification parameters shown in Table 1.
[0034] Table 1
[0035] Water pore volume, mL / g >0.5 <![CDATA[Specific surface area, m 2 / g]]> 1-3 Bulk ratio, g / mL 0.4-0.9 Average strength, N / grain >80 Main crystal phase <![CDATA[α-Al2O3]]> <![CDATA[Al2O3]]> >99% Wear rate <1% Loss on burning <8%
[0036] In some specific embodiments, the concentration of the rhenium salt in the first impregnation solution is 0.05-0.3 g / mL in weight percentage; the rhenium salt includes ammonium perrhenate.
[0037] In some specific embodiments, the step of impregnating the carrier in a first impregnation solution containing a rhenium salt includes: placing the carrier in a rotary evaporator, vacuuming the carrier at 0.1 to 0.2 MPa for 1 to 2 hours, injecting the first impregnation solution containing a rhenium salt, and impregnating the carrier for 1.5 to 2.5 hours.
[0038] In some specific embodiments, the working condition parameters of the first calcination activation include: temperature of 350-550° C., time of 15-45 minutes; the working condition parameters of the second calcination activation include: temperature of 300-500° C., time of 3-20 minutes.
[0039] In some specific embodiments, the concentration of the silver salt in the second impregnation solution is 0.25-0.6 g / mL by weight, and the silver salt includes silver oxalate; the concentration of the cesium salt in the second impregnation solution is 0.05-0.4 g / mL by weight, and the cesium salt includes cesium carbonate; the concentration of the amine organic compound in the second impregnation solution is 0.45-0.85 g / mL by weight, and the amine organic compound includes ethylenediamine.
[0040] In some specific embodiments, the step of impregnating the first carrier in a second impregnation solution containing a silver salt, an amine organic compound and a cesium salt includes: placing the carrier in a rotary evaporator, vacuuming it at 0.1 to 0.2 MPa for 1 to 2 hours, injecting the first impregnation solution containing a rhenium salt, and impregnating it for 1.5 to 2.5 hours.
[0041] In a second aspect, the present invention provides a supported silver catalyst, wherein the supported silver catalyst is prepared by the method for preparing the supported silver catalyst described in any one of the first aspects.
[0042] In a third aspect, the present invention provides use of the supported silver catalyst described in any one of the second aspects in the production of ethylene oxide by oxidation of ethylene.
[0043] It should be noted that the various components involved in the supported silver catalyst and its preparation method and application provided in the embodiments of the present invention, unless otherwise specified or specified, can all be commercially available products; at the same time, the steps and parameters involved in the preparation method, unless otherwise specified or specified, can all be carried out according to existing processes or using existing equipment.
[0044] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0045] Example 1
[0046] This example provides a supported silver catalyst, the preparation method of which comprises the following steps:
[0047] Weigh 0.44g of ammonium perrhenate and dissolve it in 100mL of deionized water to obtain a primary impregnation solution. Place 20g of the carrier in a rotary evaporator, vacuum it for 1 hour under 0.1Mpa, inject the primary impregnation solution, and after 2 hours of impregnation, take out the carrier and centrifuge it, and then place it in an oven at 60°C for 4 hours. Activate the dried carrier by roasting at 400°C for 10 minutes to obtain a primary impregnation sample. Mix 14g of silver oxalate with 25g of deionized water, dissolve 7.2g of ethylenediamine in 20g of deionized water in a cold water bath, and then slowly add the silver oxalate mixture to the ethylenediamine solution to obtain a colorless clear solution. Add 0.12g of cesium sulfate to the above clear solution to obtain a secondary impregnation solution. Vacuum the primary impregnation sample at 0.1MPa for 1 hour, then inject the secondary impregnation solution into the reaction bottle, let it stand for more than 2 hours, remove the impregnated carrier, drain it, and obtain a silver catalyst precursor. The silver catalyst precursor was placed in an activation furnace at 21 m 3 / h flow rate nitrogen was activated for 5 minutes at a temperature of 390°C to obtain a silver catalyst, which was recorded as ReCs-390.
[0048] Example 2
[0049] This example provides a supported silver catalyst, the preparation method of which comprises the following steps:
[0050] Weigh 0.44g of ammonium perrhenate and dissolve it in 100mL of deionized water to obtain a primary impregnation solution. Place 20g of the carrier in a rotary evaporator, vacuum it for 1 hour under 0.1Mpa, inject the primary impregnation solution, and after 2 hours of impregnation, take out the carrier and centrifuge it, and then place it in an oven at 60°C for 4 hours. Activate the dried carrier by roasting at 400°C for 10 minutes to obtain a primary impregnation sample. Mix 14g of silver oxalate with 25g of deionized water, dissolve 7.2g of ethylenediamine in 20g of deionized water in a cold water bath, and then slowly add the silver oxalate mixture to the ethylenediamine solution to obtain a colorless clear solution. Add 0.12g of cesium sulfate to the above clear solution to obtain a secondary impregnation solution. Vacuum the primary impregnation sample at 0.1MPa for 1 hour, then inject the secondary impregnation solution into the reaction bottle, let it stand for more than 2 hours, remove the impregnated carrier, drain it, and obtain a silver catalyst precursor. The silver catalyst precursor was placed in an activation furnace at 27 m 3 The catalyst was activated under nitrogen gas at a flow rate of / h for 3 minutes at a temperature of 500°C to obtain a silver catalyst, which was recorded as ReCs-500.
[0051] Example 3
[0052] This example provides a supported silver catalyst, the preparation method of which comprises the following steps:
[0053] Weigh 0.44g of ammonium perrhenate and dissolve it in 100mL of deionized water to obtain a primary impregnation solution. Place 20g of the carrier in a rotary evaporator, vacuum it for 1 hour under 0.1Mpa, inject the primary impregnation solution, and after 2 hours of impregnation, take out the carrier and centrifuge it, and then place it in an oven at 60°C for 4 hours. Activate the dried carrier by roasting at 400°C for 10 minutes to obtain a primary impregnation sample. Mix 14g of silver oxalate with 25g of deionized water, dissolve 7.2g of ethylenediamine in 20g of deionized water in a cold water bath, and then slowly add the silver oxalate mixture to the ethylenediamine solution to obtain a colorless clear solution. Add 0.12g of cesium sulfate to the above clear solution to obtain a secondary impregnation solution. Vacuum the primary impregnation sample at 0.1MPa for 1 hour, then inject the secondary impregnation solution into the reaction bottle, let it stand for more than 2 hours, remove the impregnated carrier, drain it, and obtain a silver catalyst precursor. The silver catalyst precursor was placed in an activation furnace at 18 m 3 The catalyst was activated under nitrogen gas at a flow rate of / h for 15 minutes at a temperature of 270°C to obtain a silver catalyst, which was recorded as ReCs-270.
[0054] Comparative Example 1
[0055] Mix 14g of silver oxalate with 25g of deionized water, dissolve 7.2g of ethylenediamine in 20g of deionized water in a cold water bath, and then slowly add the silver oxalate mixture to the ethylenediamine solution to obtain a colorless clear solution. Add 0.44g of ammonium perrhenate and 0.12g of cesium sulfate to the above clear solution to obtain an impregnation solution. Take 20g of the carrier and vacuum treat it at 0.1MPa for 1 hour, then inject the impregnation solution into the reaction bottle, let it stand for more than 2 hours, remove the impregnated carrier, drain it, and obtain a silver catalyst precursor. Put the silver catalyst precursor into an activation furnace and activate it at 21m 3 The catalyst was activated under nitrogen gas at a flow rate of / h for 5 minutes at a temperature of 390°C to obtain a silver catalyst, which was recorded as ReCs-390-1.
[0056] Comparative Example 2
[0057] Mix 14g of silver oxalate with 25g of deionized water, dissolve 7.2g of ethylenediamine in 20g of deionized water in a cold water bath, and then slowly add the silver oxalate mixture to the ethylenediamine solution to obtain a colorless clear solution. Add 0.44g of ammonium perrhenate and 0.12g of cesium sulfate to the above clear solution to obtain an impregnation solution. Take 20g of the carrier and vacuum treat it at 0.1MPa for 1 hour, then inject the impregnation solution into the reaction bottle, let it stand for more than 2 hours, remove the impregnated carrier, drain it, and obtain a silver catalyst precursor. Put the silver catalyst precursor into an activation furnace and activate it at 27m 3 / h flow rate nitrogen was activated for 3 minutes at a temperature of 500°C to obtain a silver catalyst, which was recorded as ReCs-500-1.
[0058] Comparative Example 3
[0059] Mix 14g of silver oxalate with 25g of deionized water, dissolve 7.2g of ethylenediamine in 20g of deionized water in a cold water bath, and then slowly add the silver oxalate mixture to the ethylenediamine solution to obtain a colorless clear solution. Add 0.44g of ammonium perrhenate and 0.12g of cesium sulfate to the above clear solution to obtain an impregnation solution. Take 20g of the carrier and vacuum treat it at 0.1MPa for 1 hour, then inject the impregnation solution into the reaction bottle, let it stand for more than 2 hours, remove the impregnated carrier, drain it, and obtain a silver catalyst precursor. Put the silver catalyst precursor into an activation furnace and activate it at 18m 3 The catalyst was activated under nitrogen gas at a flow rate of / h for 15 minutes at a temperature of 270°C to obtain a silver catalyst, which was recorded as ReCs-270-1.
[0060] Comparative Example 4
[0061] Mix 14g of silver oxalate with 25g of deionized water, dissolve 7.2g of ethylenediamine in 20g of deionized water in a cold water bath, and then slowly add the silver oxalate mixture to the ethylenediamine solution to obtain a colorless clear solution. Add 0.12g of cesium sulfate to the above clear solution to obtain an impregnation solution. Take 20g of the carrier and vacuum treat it under 0.1MPa for 1 hour, then inject the impregnation solution into the reaction bottle, let it stand for more than 2 hours, remove the impregnated carrier, drain it, and obtain a silver catalyst precursor. Put the silver catalyst precursor into an activation furnace and activate it at 21m 3 / h flow rate nitrogen was activated for 5 minutes at a temperature of 390°C to obtain a silver catalyst, which was recorded as Cs-390-1.
[0062] Comparative Example 5
[0063] Mix 14g of silver oxalate with 25g of deionized water, dissolve 7.2g of ethylenediamine in 20g of deionized water in a cold water bath, and then slowly add the silver oxalate mixture to the ethylenediamine solution to obtain a colorless clear solution. Add 0.12g of cesium sulfate to the above clear solution to obtain an impregnation solution. Take 20g of the carrier and vacuum treat it at 0.1MPa for 1 hour, then inject the impregnation solution into the reaction bottle, let it stand for more than 2 hours, remove the impregnated carrier, drain it, and obtain a silver catalyst precursor. Put the silver catalyst precursor into an activation furnace and activate it at 27m 3 / h flow rate nitrogen was activated for 3 minutes at a temperature of 500°C to obtain a silver catalyst, which was recorded as Cs-500-1.
[0064] Comparative Example 6
[0065] Mix 14g of silver oxalate with 25g of deionized water, dissolve 7.2g of ethylenediamine in 20g of deionized water in a cold water bath, and then slowly add the silver oxalate mixture to the ethylenediamine solution to obtain a colorless clear solution. Add 0.12g of cesium sulfate to the above clear solution to obtain an impregnation solution. Take 20g of the carrier and vacuum treat it under 0.1MPa for 1 hour, then inject the impregnation solution into the reaction bottle, let it stand for more than 2 hours, remove the impregnated carrier, drain it, and obtain a silver catalyst precursor. Put the silver catalyst precursor into an activation furnace and heat it at 18m 3 The catalyst was activated under nitrogen gas at a flow rate of / h for 15 minutes at a temperature of 270°C to obtain a silver catalyst, which was recorded as Cs-270-1.
[0066] Test Case
[0067] In this example, the catalytic performance of the catalysts obtained in the above examples and comparative examples was investigated, and the selectivity and activity of various silver catalysts prepared in the present invention were evaluated using a fixed bed reactor. The silver catalyst was crushed and sieved to take out 0.3 g of catalyst particles with a size of 40-60 mesh, which were loaded into the reactor and compacted and placed in a constant temperature section. The pressure of the catalyst evaluation was 2.0 MPa and the volume space velocity was 5000 h -1 , reaction temperature 225°C. The reaction inlet gas composition includes 35 mol% ethylene, 7 mol% oxygen, less than 0.8 mol% carbon dioxide, 0.5-10 ppm ethyl chloride / ethylene dichloride, and nitrogen as the balance gas.
[0068] After the measurement results were corrected for volume shrinkage, the selectivity (S) was calculated according to the following formula:
[0069] S=ΔEO / (ΔEO+0.5*ΔCO2)*100%
[0070] Where ΔEO is the concentration difference of ethylene oxide in the reactor inlet and outlet gases, and ΔCO2 is the concentration difference of carbon dioxide in the reactor inlet and outlet gases.
[0071] The test results are shown in Table 2. In Table 2, if the ethylene oxide yield does not meet the conditions, the selectivity and ethylene single-pass conversion are not calculated and are represented by "-".
[0072] Table 2
[0073]
[0074] Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0075] In the description of the specification of the present invention, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or plural, respectively.
[0076] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for preparing a supported silver catalyst, It is characterized in that The preparation method comprises the following steps: The carrier is impregnated in a first impregnation solution containing a rhenium salt, and then centrifuged, dried, and first calcined for activation to obtain a first carrier; The first carrier is immersed in a second impregnation solution containing a silver salt, an amine organic compound and a cesium salt, and then allowed to stand and taken out to obtain a silver catalyst precursor; Under an inert gas atmosphere, the silver catalyst precursor is subjected to a second calcination activation to obtain the supported silver catalyst.
2. The method for preparing a supported silver catalyst according to claim 1, It is characterized in that In terms of weight percentage, the concentration of the rhenium salt in the first impregnation solution is 0.05-0.3 g / mL; the rhenium salt includes ammonium perrhenate.
3. The method for preparing a supported silver catalyst according to claim 1, It is characterized in that The step of immersing the carrier in a first impregnation liquid containing rhenium salt comprises: placing the carrier in a rotary evaporator, vacuuming the carrier under a condition of 0.1 to 0.2 MPa for 1 to 4 hours, injecting the first impregnation liquid containing rhenium salt, and immersing the carrier for 1 to 3 hours.
4. The method for preparing a supported silver catalyst according to claim 1, It is characterized in that The working condition parameters of the first calcination activation include: temperature of 350-550° C. and time of 15-45 minutes; the working condition parameters of the second calcination activation include: temperature of 300-500° C. and time of 3-20 minutes.
5. The method for preparing a supported silver catalyst according to claim 1, It is characterized in that In terms of weight percentage, the concentration of the silver salt in the second impregnation solution is 0.15-0.45 g / mL, and the silver salt includes silver oxalate; in terms of weight percentage, the concentration of the cesium salt in the second impregnation solution is 0.05-0.4 g / mL, and the cesium salt includes cesium carbonate; in terms of weight percentage, the concentration of the amine organic compound in the second impregnation solution is 0.45-0.85 g / mL, and the amine organic compound includes ethylenediamine.
6. The method for preparing a supported silver catalyst according to claim 1, It is characterized in that The step of impregnating the first carrier in a second impregnation solution containing silver salt, amine organic compound and cesium salt comprises: placing the carrier in a rotary evaporator, vacuuming the carrier under the condition of 0.1-0.2 MPa for 1-4 hours, injecting the first impregnation solution containing rhenium salt, and impregnating the carrier for 1-3 hours.
7. A supported silver catalyst, It is characterized in that The supported silver catalyst is prepared by the preparation method described in any one of claims 1 to 7.
8. Use of the supported silver catalyst according to claim 7 in preparing ethylene oxide by oxidation of ethylene.
Citation Information
Patent Citations
Calcination in an inert gas in the presence of a small concentration of an oxidizing component
CN101171080A
Carrier of silver catalyst for producing ethylene oxide, preparation method thereof, silver catalyst prepared by using same and application thereof in producing ethylene oxide
CN101850243A
Silver catalyst carrier for ethylene oxide production, preparation method, silver catalyst prepared by silver catalyst carrier, and application thereof
CN102397795A
Preparation method for silver catalyst, and silver catalyst and application thereof
CN105327712A
Method for preparing silver catalyst, silver catalyst and application thereof of silver catalyst
CN105817224A