Zinc air battery bifunctional catalyst and preparation method thereof
By loading manganese-cobalt-nickel trimetal alloy with nitrogen-doped iron-based carbon nanotubes with nitrogen-doped iron-based carbon nanotubes, an efficient dual-function catalyst for zinc-air battery was prepared, which solved the problem of insufficient performance of zinc-air battery catalysts and achieved the Low-cost, high-performance electrocatalytic effect.
Patent Information
- Application Number
- CN202411062577.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-22
AI Technical Summary
The slow kinetics of oxygen reaction and redox reactions of zinc air batteries lead to insufficient power density and cycle stability. The existing catalysts are costly and unstable, making it difficult to apply on a large scale.
A manganese-cobalt-nickel trimetal alloy co-doped with nitrogen and sulfur is supported on the surface of nitrogen-doped iron-based carbon nanotubes, and a dual-function catalyst is prepared through hydrothermal reaction and radio frequency plasma technology to improve catalytic activity and stability.
The electrocatalytic performance of oxygen reduction reaction and redox reaction is significantly improved, the charge transfer efficiency is enhanced, the reaction energy barrier is reduced, the cycle stability and charge and discharge performance are improved, and the low-cost and high-performance zinc-air battery catalyst is realized.
Smart Images

Figure CN119008984A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of zinc-air battery catalysts, and in particular relates to a zinc-air battery bifunctional catalyst in which a nitrogen-sulfur co-doped metal alloy is loaded on the surface of a nitrogen-doped iron-based carbon nanotube and a preparation method thereof. Background Art
[0002] Traditional energy is becoming increasingly scarce worldwide due to overexploitation and overuse, and the development and utilization efficiency of new energy sources are becoming increasingly important in the context of the trend of carbon peak and carbon neutrality. Wind energy, solar energy and tidal energy have received widespread attention due to their clean and renewable advantages, but these resources are often restricted in use due to the influence of geographical environment and other factors. Therefore, it is crucial to find a low-cost and green clean energy and storage technology.
[0003] Among various energy storage devices, secondary batteries represented by lithium ions have been widely used as energy storage devices in life. In addition, there are other energy storage devices, such as fuel cells, which are the greenest and cleanest, because the final products of the fuel cells during use are mainly water and other harmless substances, and no harmful substances are produced. However, the cost of traditional fuel cells is relatively high, and hydrocarbon fuels cannot be effectively used, resulting in some bottlenecks in price and technology of fuel cells. Rechargeable metal-air batteries are considered to be one of the most promising power sources for converting and storing chemical energy due to their superior energy density. Rechargeable zinc-air batteries (ZAB, also known as zinc-air batteries) have been widely studied due to their high safety, abundant reserves of metal zinc, and high theoretical specific energy. However, the multi-step electron transfer reaction kinetics of oxygen in the charging and discharging process are slow, resulting in low round-trip energy efficiency, coupled with limited cycle life, which restricts the development of rechargeable ZAB.
[0004] The power density and cycle stability of zinc-air batteries are limited by the oxygen reactions at their air cathodes, including ORR and OER. The ORR reaction rate directly determines the power density of zinc-air batteries, while the OER reaction rate directly affects the cycle stability of the battery. Since the kinetics of these two reactions are extremely slow, there is a large overpotential during the actual operation of the battery, which makes the performance of actual zinc-air batteries lower than the theoretical performance. Therefore, the development of practical electrocatalysts with enhanced electrochemical performance remains a challenge. Platinum-based electrocatalysts are the most effective ORR catalysts to date. For OER, electrocatalysts based on iridium and ruthenium oxides are considered to be the most effective catalysts. However, these materials are expensive, have poor stability, and have inert intermediates that are not easily reacted, which limits their large-scale application. Therefore, it is of great significance to develop electrocatalysts with high activity, high stability, and low cost.
[0005] Compared with precious metals, transition metals are relatively cheap and abundant on earth. Moreover, transition metals have multiple valence states and can form a variety of compounds with different crystal structures. Transition metal catalysts such as oxides (including perovskites and spinels), sulfides and nitrides have shown good catalytic activity. Among them, transition metal chalcogenides show their unique advantages, such as their modulated electronic structure and high catalytic activity for OER and ORR. However, its low conductivity, agglomeration and dissolution after several battery cycles make it unfeasible.
[0006] In contrast, carbon-based catalysts have many advantages such as high conductivity, adjustable porous structure, good chemical stability and low price, and have been widely studied in the field of energy electrochemistry. For carbon materials, the number of active sites is limited, and the catalytic ability of a single site is insufficient. Therefore, precise element doping and defect construction of carbon materials provide more possibilities for the design of advanced oxygen electrocatalysts. Among them, nitrogen-doped carbon nanotubes are an excellent conductive substrate. Their nano-three-dimensional structure is conducive to the conduction of electrons. At the same time, their extremely high specific surface area can provide abundant active sites for the reaction; and the metal compounds loaded on their surface can achieve uniform loading while maintaining the nanoscale structure. In addition, due to the close radii of carbon atoms and nitrogen atoms, nitrogen doping can alleviate lattice distortion, thereby improving the stability and performance of the material, and it can also increase electron affinity, promote oxygen adsorption and decomposition of intermediate peroxides, thereby improving catalytic activity and battery performance.
[0007] Therefore, coupling transition metal chalcogenides with nitrogen-doped carbon nanotubes is an effective alternative to overcome the problems associated with Zn-air battery catalysts. Summary of the invention
[0008] A technical problem to be solved by the present invention is to provide a zinc-air battery bifunctional catalyst in which a nitrogen- and sulfur-co-doped metal alloy is loaded on the surface of nitrogen-doped iron-based carbon nanotubes, which has high specific surface area, multiple active sites, excellent performance, low cost and long-term stability, and a preparation method thereof.
[0009] The technical solution adopted by the zinc-air battery bifunctional catalyst to solve the above technical problems is: a zinc-air battery bifunctional catalyst, whose structural unit uses nitrogen-doped iron-based carbon nanotubes as a conductive network, and nitrogen and sulfur co-doped manganese, cobalt and nickel tri-metal alloys are loaded on the conductive network.
[0010] Another technical problem to be solved by the present preparation method is to provide a preparation method of the above-mentioned zinc-air battery bifunctional catalyst, which specifically comprises the following steps:
[0011] (a) preparation of nitrogen-doped iron-based carbon nanotubes;
[0012] (ii) loading manganese, cobalt, nickel trimetallic hydroxide nanoneedles by hydrothermal reaction to obtain manganese, cobalt, nickel trimetallic hydroxide@nitrogen-doped iron-based carbon nanotubes;
[0013] (iii) In an inert atmosphere, plasma-assisted sulfurization of manganese-cobalt-nickel trihydroxide@nitrogen-doped iron-based carbon nanotubes was performed using radio frequency plasma technology.
[0014] Compared with the prior art, the advantages of the present invention are: the zinc-air battery bifunctional catalyst has excellent ORR and OER electrocatalytic performance, and the introduction of nitrogen and sulfur elements in the preparation method can improve the charge transfer efficiency, reduce the reaction energy barrier, improve the electrocatalytic activity and selectivity, enhance the ORR and OER reaction performance, and improve the cycle stability and charge-discharge performance; the specific reasons are as follows:
[0015] (1) Nitrogen-doped iron-based carbon nanotubes have excellent electrical conductivity. The electronegativity of nitrogen is much greater than that of carbon, which makes the electrically neutral carbon material doped with nitrogen positively charged and easy to deposit metal nanoparticles. At the same time, nitrogen-doped carbon materials can promote the adsorption of oxygen and the decomposition of intermediate peroxides. Nitrogen-containing functional groups can increase the electron affinity with the matrix and promote the ability of metals to donate electrons, thereby improving the activity of the catalyst; nitrogen-doped iron-based carbon nanotubes have rich void structures and rich iron-based active sites, which can make them exhibit excellent electrocatalytic oxygen reduction performance; nitrogen-doped iron-based carbon nanotubes have a high specific surface area and a stable three-dimensional structure, which can make electrochemically active substances more easily attached to the surface of carbon nanotubes, improving their catalytic performance;
[0016] (2) The manganese, cobalt, and nickel needle-shaped hydroxides loaded on the surface of nitrogen-doped iron-based carbon nanotubes can further improve the catalytic efficiency. This is because the nitrogen-doped iron-based carbon nanotubes have a large specific surface area and strong adsorption capacity, which can provide more catalytic sites, thereby improving the catalytic efficiency; the hydroxide can maintain a stable structure under high temperature and strong acid and alkali environment, and will not decompose or dissolve, so it has good thermal stability and chemical stability. Loading it on nitrogen-doped iron-based carbon nanotubes can further improve the stability and durability of the material;
[0017] (3) The doping of sulfur elements can lead to the construction of topological microstructures and modulated electronic structures, thereby improving the catalytic activity and durability of the bifunctional catalyst; in the plasma-enhanced chemical vapor deposition equipment, the introduction of nitrogen plasma can enhance the stability and conductivity of the material, making it have excellent bifunctional activity that can be applied to zinc-air batteries.
[0018] Preferably, the preparation process of step (1) comprises:
[0019] (1) Cut a piece of 3*4cm 2The raw carbon cloth was placed in ethanol and deionized water, respectively, and ultrasonicated for 10 min;
[0020] (2) Weigh 5 g of Fe(SO4)2·7H2O, dissolve it in 100 mL of deionized water, stir it evenly, put the ultrasonicated carbon cloth into it, soak it in a 60°C environment for 12 h, then take out the iron-attached carbon cloth and put it in an oven to dry for 12 h;
[0021] (3) Place the dried iron-attached carbon cloth on a porcelain boat, place it in a tube furnace, introduce argon and ammonia gas, and heat at 5℃ min -1 After the temperature was raised to 500°C at a heating rate of 100 °C, the temperature was kept for 30 min for nitriding. After cooling, the porcelain boat was taken out. 1.2 g of melamine was weighed and placed under the iron-attached carbon cloth in the porcelain boat. The porcelain boat was placed in a tubular furnace and argon was introduced at 10 °C min -1 The temperature was raised to 850°C at a heating rate for further annealing. After keeping the temperature for 120 minutes, the reaction was completed. After cooling, the nitrogen-doped iron-based carbon nanotubes were taken out and recorded as NCNTs@CC.
[0022] Preferably, the preparation process of step (ii) comprises: dissolving manganese transition metal salt, cobalt transition metal salt, nickel transition metal salt, urea and ammonium fluoride in deionized water, stirring and dissolving them, pouring them into a polytetrafluoroethylene liner, placing nitrogen-doped iron-based carbon nanotubes, and then placing the polytetrafluoroethylene liner in a high-pressure reactor, reacting at 80-200° C. for 6-24 hours, and after the reaction is completed, taking out after cooling, rinsing with deionized water and ethanol, and placing in an oven to dry for 6-24 hours to obtain manganese cobalt nickel trimetallic hydroxide @ nitrogen-doped iron-based carbon nanotubes, recorded as MnCoNiLDH / NCNTs@CC.
[0023] Preferably, the manganese transition metal salt is one or more of MnCO3, MnCl2·4H2O, MnCl2, and Mn(NO3)2·4H2O; the cobalt transition metal salt is one or more of Co(NO3)2·6H2O, CoCl2·6H2O, Co(CH3COO)2·4H2O, CoSO4·6H2O, and CoCl2; the nickel transition metal salt is NiC 10 H 14 One or more of O4, NiCl2·6H2O, Ni(NO3)2·6H2O, NiC4H6O4·4H2O, and NiCO3.
[0024] Wherein, the molar ratio of the manganese transition metal salt: the cobalt transition metal salt: the nickel transition metal salt is 0.25:1:0.5.
[0025] Preferably, the preparation process of step (iii) includes: placing the manganese, cobalt, nickel trimetallic hydroxide @ nitrogen-doped iron-based carbon nanotubes and thiourea obtained in step (ii) into a porcelain boat, placing the porcelain boat into a plasma enhanced chemical vapor deposition device, introducing nitrogen gas, and performing plasma-assisted sulfurization. The pressure in the tube is 20 Pa, the discharge power is 100 W, and the discharge time is 10 min. The obtained zinc-air battery bifunctional catalyst is recorded as p-(Mn)-CoNi2S4@Co2N / NCNTs@CC. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The microstructure of p-(Mn)-CoNi2S4@Co2N / NCNTs@CC prepared as a verification example under a scanning electron microscope (SEM) (scale bar 2 μm);
[0027] Figure 2 Linear sweep voltammetry (LSV) of oxygen reduction reaction (ORR) of verification examples and comparative examples 1, 2, 3, 4 and commercial Pt / C catalysts;
[0028] Figure 3 Linear sweep voltammetry test diagram (LSV) of oxygen evolution reaction (OER) of verification example and comparative examples 1, 2, 3, 4 and commercial RuO2 catalyst. DETAILED DESCRIPTION
[0029] The preferred embodiment is a zinc-air battery bifunctional catalyst, wherein the structural unit uses nitrogen-doped iron-based carbon nanotubes as a conductive network, and nitrogen and sulfur co-doped manganese, cobalt and nickel tri-metal alloys are loaded on the conductive network.
[0030] The preparation method specifically comprises the following steps:
[0031] (a) preparation of nitrogen-doped iron-based carbon nanotubes;
[0032] (ii) loading manganese, cobalt, nickel trimetallic hydroxide nanoneedles by hydrothermal reaction to obtain manganese, cobalt, nickel trimetallic hydroxide@nitrogen-doped iron-based carbon nanotubes;
[0033] (iii) In an inert atmosphere, plasma-assisted sulfurization of manganese-cobalt-nickel trihydroxide@nitrogen-doped iron-based carbon nanotubes was performed using radio frequency plasma technology.
[0034] Among them, the preparation process of step (ii) includes: dissolving manganese transition metal salt, cobalt transition metal salt, nickel transition metal salt, urea and ammonium fluoride in deionized water, stirring them thoroughly to dissolve them, pouring them into a polytetrafluoroethylene liner, placing nitrogen-doped iron-based carbon nanotubes, and then placing the polytetrafluoroethylene liner in a high-pressure reactor, reacting at 80-200° C. for 6-24 hours, and after the reaction is completed, taking it out after cooling, rinsing it with deionized water and ethanol, and placing it in an oven to dry for 6-24 hours to obtain manganese cobalt nickel trimetallic hydroxide @ nitrogen-doped iron-based carbon nanotubes, recorded as MnCoNiLDH / NCNTs@CC.
[0035] The manganese transition metal salt is one or more of MnCO3, MnCl2·4H2O, MnCl2, and Mn(NO3)2·4H2O; the cobalt transition metal salt is one or more of Co(NO3)2·6H2O, CoCl2·6H2O, Co(CH3COO)2·4H2O, CoSO4·6H2O, and CoCl2; the nickel transition metal salt is NiC 10 H 14 O4, NiCl2·6H2O, Ni(NO3)2·6H2O, NiC4H6O4·4H2O, NiCO3. The molar ratio of the manganese transition metal salt: the cobalt transition metal salt: the nickel transition metal salt is 0.25:1:0.5.
[0036] The preparation process of step (iii) includes: placing the manganese, cobalt, nickel trimetallic hydroxide @ nitrogen-doped iron-based carbon nanotubes and thiourea obtained in step (ii) into a porcelain boat, placing the porcelain boat into a plasma enhanced chemical vapor deposition device, introducing nitrogen gas, and performing plasma-assisted sulfurization. The pressure in the tube is 20 Pa, the discharge power is 100 W, and the discharge time is 10 min. The obtained zinc-air battery bifunctional catalyst is recorded as p-(Mn)-CoNi2S4@Co2N / NCNTs@CC.
[0037] The following embodiments of the present invention are described in conjunction with verification examples, comparative examples and accompanying drawings, including various details of the embodiments of the present invention to facilitate understanding, which should be considered as merely exemplary. Therefore, it should be appreciated by those of ordinary skill in the art that various changes and modifications may be made to the embodiments described herein without departing from the scope and spirit of the present invention. Similarly, for clarity and conciseness, the description of well-known functions and structures is omitted in the following description.
[0038] Verification example:
[0039] The preparation method of the zinc-air battery bifunctional catalyst (p-(Mn)-CoNi2S4@Co2N / NCNTs@CC) co-doped with nitrogen and sulfur and supported on the surface of nitrogen-doped iron-based carbon nanotubes specifically comprises the following steps:
[0040] (I) Synthesis of nitrogen-doped iron-based carbon nanotubes:
[0041] Cut a piece of 3*4cm 2 The raw carbon cloth was placed in ethanol and deionized water in turn, and ultrasonicated for 10 minutes respectively. Weigh 5g Fe(SO4)2·7H2O, dissolve it in 100mL deionized water, stir evenly, put the ultrasonicated raw carbon cloth into the stirred solution, soak it in 60℃ environment for 12h, then take out the iron-attached carbon cloth and put it in an oven to dry for 12h. The dried iron-attached carbon cloth was placed on a porcelain boat, placed in a tube furnace, and argon ammonia gas was introduced at 5℃min -1 After heating to 500℃ at a heating rate of 100℃, keep the temperature for 30min for nitridation, wait for it to cool, and take out the porcelain boat. Weigh 1.2g of melamine and put it in the bottom of the porcelain boat. Place the nitrided iron-attached carbon cloth on top of the melamine, put it in a tube furnace, pass argon gas, and heat at 10℃min. -1 The temperature was raised to 850°C at a heating rate for further annealing. After keeping the temperature for 120 minutes, the reaction was completed. After cooling, the nitrogen-doped iron-based carbon nanotubes were taken out and recorded as NCNTs@CC.
[0042] (II) Synthesis of manganese, cobalt, nickel trimetallic hydroxide:
[0043] Weigh 0.25mM MnCl2·4H2O, 1mM CoCl2·6H2O, 0.5mM NiCl2·6H2O, 10mM CO(NH2)2 and 1mM NH4F, mix with 30mL deionized water, stir evenly to dissolve, pour into a polytetrafluoroethylene liner, put in the nitrogen-doped iron-based carbon nanotubes prepared in step (i), and then put the polytetrafluoroethylene liner into a high-pressure reactor, react at 120°C for 11h. After the reaction is completed, take out after cooling, rinse with deionized water and ethanol, and put in an oven to dry for 12h to obtain manganese cobalt nickel trimetallic hydroxide @ nitrogen-doped iron-based carbon nanotubes, recorded as MnCoNiLDH / NCNTs@CC.
[0044] (III) Plasma-assisted sulfurization to synthesize nitrogen and sulfur co-doped manganese, cobalt and nickel trimetallic alloys:
[0045] The manganese, cobalt, nickel trimetallic hydroxide @ nitrogen-doped iron-based carbon nanotubes and thiourea obtained in step (ii) are placed in a porcelain boat, and the porcelain boat is placed in a plasma enhanced chemical vapor deposition equipment, and nitrogen is introduced to perform plasma-assisted sulfurization. The pressure in the tube is 20 Pa, the discharge power is 100 W, and the discharge time is 10 min. The obtained zinc-air battery bifunctional catalyst sample is recorded as p-(Mn)-CoNi2S4@Co2N / NCNTs@CC.
[0046] The morphology of the p-(Mn)-CoNi2S4@Co2N / NCNTs@CC sample obtained in the verification example was analyzed by scanning electron microscopy (SEM). Figure 1 As shown, the p-(Mn)-CoNi2S4@Co2N / NCNTs@CC sample is a uniform nanoneedle with a relatively rough surface and a stable structure.
[0047] Bifunctional catalytic performance evaluation:
[0048] The electrocatalytic performance of the prepared zinc-air battery bifunctional catalyst samples was carried out in a three-electrode device using an electrochemical workstation (CHI760E).
[0049] Preparation of working electrodes for ORR and OER performance tests: Before using the rotating disk electrode (RDE), the glassy carbon electrode (GCE, d = 4.0 mm) was polished to a mirror surface with a polishing cloth containing Al2O3 powder, then rinsed repeatedly with deionized water, ultrasonically dried for a few seconds, and dried at room temperature for later use. The prepared carbon cloth was punched with a circular hole with a diameter of 4 mm, and 5wt.% Nafion was used as a binder to firmly adhere the zinc-air battery bifunctional catalyst sample to the electrode, and the test was performed after it was dried. As a control experiment, a commercial 20wt.% Pt / C catalyst was selected in the ORR test and coated on the carbon cloth for testing. A commercial RuO2 catalyst was selected for the OER test. The preparation method was the same as the above sample. 5mg of RuO2 powder was prepared into a slurry and evenly coated on the carbon cloth. The carbon cloth was then punched and bonded to the electrode for testing. Electrochemical performance test: A standard three-electrode electrochemical test system was used during the test, wherein the counter electrode was a stone mill rod electrode, the reference electrode was a saturated calomel electrode (SCE) and the working electrode prepared above, and the test solution was a 1M KOH solution (pH = 13). All potentials were calculated by the Nernst equation with reference to the reversible hydrogen electrode (RHE): E(RHE) = E(Hg / Hg2Cl2) + 0.2415 + 0.059pH. Before the linear sweep voltammetry (LSV) test, the working electrode was charged at 10mVs -1 The samples were activated by cyclic voltammetry (CV) for 50 cycles at a scan rate of 1.3 Å. All electrochemical tests were performed at room temperature.
[0050] The ORR LSV curves of p-(Mn)-CoNi2S4@Co2N / NCNTs@CC sample and commercial 20wt.%Pt / C catalyst in 1M KOH solution saturated with O2 at a rotation speed of 1600rpm were tested by rotating disk electrode (RDE). Figure 2The p-(Mn)-CoNi2S4@Co2N / NCNTs@CC sample exhibits high ORR electrocatalytic activity with a half-wave potential of 0.85 V vs. RHE and a high limiting current density of 23.82 mA cm -2 , which is higher than that of commercial Pt / C catalyst (22 mA cm -2 ), indicating that the p-(Mn)-CoNi2S4@Co2N / NCNTs@CC sample has faster reaction kinetics in the ORR electrocatalytic process.
[0051] The OER catalytic activity was also tested under exactly the same conditions as the ORR test, and the commercial RuO2 catalyst was tested under the same conditions as a comparative reference. Figure 3 The LSV curve of the OER catalytic performance of the p-(Mn)-CoNi2S4@Co2N / NCNTs@CC sample shows that the p-(Mn)-CoNi2S4@Co2N / NCNTs@CC sample has a current density of 50 mA cm -2 When the OER overpotential is only 293 mV, the current density is 100 mA cm -2 The OER overpotential is 314 mV. Under the same test conditions, it is much better than the commercial RuO2 catalyst, indicating that the p-(Mn)-CoNi2S4@Co2N / NCNTs@CC sample has excellent OER electrocatalytic activity.
[0052] Comparative Example 1:
[0053] The preparation method of the catalyst (p-CoNi2S4@Co2N / NCNTs@CC) co-doped with nitrogen and sulfur and supported on the surface of nitrogen-doped iron-based carbon nanotubes specifically comprises the following steps:
[0054] (I) Synthesis of nitrogen-doped iron-based carbon nanotubes:
[0055] Cut a piece of 3*4cm 2 The raw carbon cloth was placed in ethanol and deionized water in turn, and ultrasonicated for 10 minutes respectively. Weigh 5g Fe(SO4)2·7H2O, dissolve it in 100mL deionized water, stir evenly, put the ultrasonicated raw carbon cloth into the stirred solution, soak it in 60℃ environment for 12h, then take out the iron-attached carbon cloth and put it in an oven to dry for 12h. The dried iron-attached carbon cloth was placed on a porcelain boat, placed in a tube furnace, and argon ammonia gas was introduced at 5℃min -1After heating to 500℃ at a heating rate of 100℃, keep the temperature for 30min for nitridation, wait for it to cool, and take out the porcelain boat. Weigh 1.2g of melamine and put it in the bottom of the porcelain boat. Place the nitrided iron-attached carbon cloth on top of the melamine, put it in a tube furnace, pass argon gas, and heat at 10℃min. -1 The temperature was raised to 850°C at a heating rate for further annealing. After keeping the temperature for 120 minutes, the reaction was completed. After cooling, the nitrogen-doped iron-based carbon nanotubes were taken out and recorded as NCNTs@CC.
[0056] (II) Synthesis of cobalt-nickel double hydroxide:
[0057] Weigh 1mM CoCl2·6H2O, 0.5mM NiCl2·6H2O, 10mM CO(NH2)2 and 1mM NH4F, mix with 30mL deionized water, stir evenly to dissolve, pour into a polytetrafluoroethylene liner, put in nitrogen-doped iron-based carbon nanotubes, and then put the polytetrafluoroethylene liner into a high-pressure reactor, react at 120°C for 11h, and after the reaction is completed, take it out after cooling to obtain cobalt nickel double metal hydroxide @ nitrogen-doped iron-based carbon nanotubes, recorded as CoNiLDH / NCNTs@CC. Where M is the volume molar concentration, that is, mol / L, 1mM is 1×10 -3 mol / L.
[0058] (III) Plasma-assisted sulfurization synthesis of nitrogen and sulfur co-doped cobalt-nickel bimetallic alloys:
[0059] The above-mentioned cobalt nickel bimetallic hydroxide @ nitrogen-doped iron-based carbon nanotubes and thiourea are placed in a porcelain boat, and the porcelain boat is placed in a plasma enhanced chemical vapor deposition equipment. Nitrogen is introduced for plasma-assisted sulfurization. The pressure in the tube is 20 Pa, the discharge power is 100 W, and the discharge time is 10 min. The obtained nitrogen and sulfur co-doped cobalt nickel bimetallic alloy is loaded on the surface of nitrogen-doped iron-based carbon nanotubes. The catalyst sample is recorded as p-CoNi2S4@Co2N / NCNTs@CC.
[0060] Bifunctional catalytic performance evaluation:
[0061] The ORR LSV curve of p-CoNi2S4@Co2N / NCNTs@CC sample was tested in 1M KOH solution saturated with O2 at a rotation speed of 1600rpm using a rotating disk electrode (RDE). Figure 2As shown. The p-CoNi2S4@Co2N / NCNTs@CC sample exhibits high ORR electrocatalytic activity with a half-wave potential of 0.8495 V vs. RHE, which is slightly lower than the commercial Pt / C catalyst (0.8575 V vs. RHE) tested under the same conditions. The p-CoNi2S4@Co2N / NCNTs@CC sample exhibits a high limiting current density of 18.08 mA cm -2 .
[0062] The OER catalytic activity was also tested under exactly the same conditions as the ORR test, e.g. Figure 3 Curve p-CoNi2S4@Co2N / NCNTs@CC sample at a current density of 50 mA cm -2 When the OER overpotential is only 314 mV, the current density is 100 mA cm -2 When the OER overpotential is 333 mV, it is much better than the commercial RuO2 catalyst, indicating that the p-CoNi2S4@Co2N / NCNTs@CC sample has excellent OER electrocatalytic activity.
[0063] Comparative Example 2:
[0064] The preparation method of sulfur-doped manganese-cobalt-nickel trimetallic alloy supported on the surface of nitrogen-doped iron-based carbon nanotubes ((Mn)-CoNi2S4 / NCNTs@CC) specifically comprises the following steps:
[0065] (I) Synthesis of nitrogen-doped iron-based carbon nanotubes:
[0066] Cut a piece of 3*4cm 2 The raw carbon cloth was placed in ethanol and deionized water in turn, and ultrasonicated for 10 minutes respectively. Weigh 5g Fe(SO4)2·7H2O, dissolve it in 100mL deionized water, stir evenly, put the ultrasonicated raw carbon cloth into the stirred solution, soak it in 60℃ environment for 12h, then take out the iron-attached carbon cloth and put it in an oven to dry for 12h. The dried iron-attached carbon cloth was placed on a porcelain boat, placed in a tube furnace, and argon ammonia gas was introduced at 5℃min -1 After heating to 500℃ at a heating rate of 100℃, keep the temperature for 30min for nitridation, wait for it to cool, and take out the porcelain boat. Weigh 1.2g of melamine and put it in the bottom of the porcelain boat. Place the nitrided iron-attached carbon cloth on top of the melamine, put it in a tube furnace, pass argon gas, and heat at 10℃min. -1 The temperature was raised to 850°C at a heating rate for further annealing. After keeping the temperature for 120 minutes, the reaction was completed. After cooling, the nitrogen-doped iron-based carbon nanotubes were taken out and recorded as NCNTs@CC.
[0067] (II) Synthesis of manganese, cobalt, nickel trimetallic hydroxide:
[0068] Weigh 0.25mM MnCl2·4H2O, 1mM CoCl2·6H2O, 0.5mM NiCl2·6H2O, 10mM CO(NH2)2 and 1mM NH4F, mix with 30mL deionized water, stir evenly to dissolve, pour into a polytetrafluoroethylene liner, put in the nitrogen-doped iron-based carbon nanotubes prepared in step (i), and then put the polytetrafluoroethylene liner into a high-pressure reactor, react at 120°C for 11h. After the reaction is completed, take out after cooling, rinse with deionized water and ethanol, and put in an oven to dry for 12h to obtain manganese cobalt nickel trimetallic hydroxide @ nitrogen-doped iron-based carbon nanotubes, recorded as MnCoNiLDH / NCNTs@CC.
[0069] (III) Common sulfurization synthesis of sulfur-doped manganese-cobalt-nickel trimetallic alloy:
[0070] The above-mentioned manganese, cobalt, nickel trimetallic hydroxide @ nitrogen-doped iron-based carbon nanotubes and thiourea are placed in a porcelain boat, and the porcelain boat is placed in a plasma enhanced chemical vapor deposition equipment. Nitrogen gas is introduced without plasma discharge. The pressure in the tube is 20 Pa, the reaction temperature is 400°C, and the insulation time is 10 min for sulfurization. The resulting sulfur-doped manganese, cobalt, nickel trimetallic alloy loaded on the surface of nitrogen-doped iron-based carbon nanotubes is recorded as (Mn)-CoNi2S4 / NCNTs@CC.
[0071] Bifunctional catalytic performance evaluation:
[0072] The LSV curve of ORR of (Mn)-CoNi2S4 / NCNTs@CC sample in 1M KOH solution saturated with O2 at a rotation speed of 1600rpm was tested by rotating disk electrode (RDE). Figure 2 The (Mn)-CoNi2S4 / NCNTs@CC sample exhibits good ORR electrocatalytic activity, with a half-wave potential of 0.889 V vs. RHE and a limiting current density of 16.17 mA cm -2 , slightly lower than that of p-(Mn)-CoNi2S4@Co2N / NCNTs@CC catalyst under the same conditions.
[0073] The OER catalytic activity was also tested under exactly the same conditions as the ORR test, e.g. Figure 3 Curve (Mn)-CoNi2S4 / NCNTs@CC sample at a current density of 50 mA cm -2 When the OER overpotential is 333 mV, the current density is 100 mA cm -2 When , the OER overpotential is 366 mV.
[0074] Comparative Example 3:
[0075] The preparation method of the catalyst (p-(Mn)-CoNi2S4@Co2N / CC) co-doped with nitrogen and sulfur and loaded on the surface of carbon fiber comprises the following steps:
[0076] (I) Synthesis of manganese, cobalt and nickel trimetallic hydroxides:
[0077] The raw carbon cloth was placed in ethanol and deionized water in turn, and then dried after ultrasonic treatment for 10 minutes. 0.25mM MnCl2·4H2O, 1mM CoCl2·6H2O, 0.5mM NiCl2·6H2O, 10mM CO(NH2)2 and 1mM NH4F were weighed, mixed with 30mL deionized water, stirred evenly, and the solution was poured into a polytetrafluoroethylene liner, and the carbon cloth was placed, and then placed in a high-pressure reactor, reacted at 120°C for 660 minutes, and the reaction was completed. After cooling, it was taken out to obtain manganese cobalt nickel trimetallic hydroxide @ carbon cloth, recorded as MnCoNiLDH / CC.
[0078] (II) Synthesis of nitrogen and sulfur co-doped manganese, cobalt and nickel trimetallic alloy by plasma-assisted sulfurization
[0079] The above-mentioned manganese, cobalt, nickel trimetallic hydroxide @ carbon cloth and thiourea are placed in a porcelain boat, and the porcelain boat is placed in a plasma enhanced chemical vapor deposition equipment. Nitrogen is introduced for plasma-assisted sulfurization. The pressure in the tube is 20 Pa, the discharge power is 100 W, and the discharge time is 10 min. The obtained nitrogen and sulfur co-doped manganese, cobalt, and nickel trimetallic alloy catalyst sample loaded on the surface of carbon fiber is recorded as p-(Mn)-CoNi2S4@Co2N / CC.
[0080] Bifunctional catalytic performance evaluation:
[0081] The ORR LSV curve of p-(Mn)-CoNi2S4@Co2N / CC sample was tested in 1M KOH solution saturated with O2 at a rotation speed of 1600rpm using a rotating disk electrode (RDE). Figure 2 The half-wave potential of the p-(Mn)-CoNi2S4@Co2N / CC sample is 0.6 V vs. RHE, and its electrocatalytic activity is lower than that of the p-(Mn)-CoNi2S4@Co2N / NCNTs@CC catalyst under the same conditions. The limiting current density of the p-(Mn)-CoNi2S4@Co2N / CC sample is 13.31 mA cm -2 The OER catalytic activity was also tested under exactly the same conditions as the ORR test, e.g. Figure 3 Curve p-(Mn)-CoNi2S4@Co2N / CC sample at a current density of 50 mA cm -2When the OER overpotential is 365 mM, the current density is 100 mA cm -2 When , the OER overpotential is 389 mV.
[0082] Comparative Example 4:
[0083] The preparation method of the catalyst (p-(Mn)-CoO@NiO / NCNTs@CC) in which the nitrogen and oxygen co-doped metal alloy is loaded on the surface of the nitrogen-doped carbon nanotubes specifically comprises the following steps:
[0084] (I) Synthesis of nitrogen-doped iron-based carbon nanotubes:
[0085] Cut a piece of 3*4cm 2 The raw carbon cloth was placed in ethanol and deionized water in turn, and ultrasonicated for 10 minutes respectively. Weigh 5gFe(SO4)2·7H2O, dissolve it in 100mL deionized water, stir evenly, put the ultrasonicated carbon cloth into the stirred solution, soak it in 60℃ environment for 12h, then take out the iron-attached carbon cloth and put it in an oven to dry for 12h. Place the dried iron-attached carbon cloth on a porcelain boat, place it in a tube furnace, pass argon ammonia gas, and heat it at 5℃min -1 After heating to 500℃ at a heating rate of 100℃, keep the temperature for 30min for nitridation, wait for it to cool, and take out the porcelain boat. Weigh 1.2g of melamine and put it in the bottom of the porcelain boat. Place the nitrided iron-attached carbon cloth on top of the melamine, put it in a tube furnace, pass argon gas, and heat at 10℃min. -1 The temperature was raised to 850°C at a heating rate for further annealing. After keeping the temperature for 120 minutes, the reaction was completed. After cooling, the nitrogen-doped iron-based carbon nanotubes were taken out and recorded as NCNTs@CC.
[0086] (II) Synthesis of manganese, cobalt, nickel trimetallic hydroxide:
[0087] Weigh 0.25mM MnCl2·4H2O, 1mM CoCl2·6H2O, 0.5mM NiCl2·6H2O, 10mM CO(NH2)2 and 1mM NH4F, mix with 30mL deionized water, stir evenly to dissolve, pour into a polytetrafluoroethylene liner, put in nitrogen-doped iron-based carbon nanotubes, and then put the polytetrafluoroethylene liner into a high-pressure reactor. React at 120°C for 11h. After the reaction is completed, take it out after cooling, rinse it with deionized water and ethanol, and put it in an oven to dry for 12h to obtain manganese cobalt nickel trimetallic hydroxide@nitrogen-doped iron-based carbon nanotubes, recorded as MnCoNiLDH / NCNTs@CC.
[0088] (III) Synthesis of Nitrogen and Oxygen Co-doped Metal Alloys by Plasma Treatment
[0089] The above-mentioned manganese, cobalt, nickel trimetallic hydroxide @ nitrogen-doped iron-based carbon nanotubes were placed in a porcelain boat, and the porcelain boat was placed in a plasma enhanced chemical vapor deposition equipment. Nitrogen gas was introduced for plasma treatment. The pressure in the tube was 20 Pa, the discharge power was 100 W, and the discharge time was 10 min. The obtained sample was recorded as (p-(Mn)-CoO@NiO / NCNTs@CC).
[0090] Bifunctional catalytic performance evaluation:
[0091] The LSV curve of ORR of (p-(Mn)-CoO@NiO / NCNTs@CC) sample in 1MKOH solution saturated with O2 at a rotation speed of 1600rpm was tested by rotating disk electrode (RDE). Figure 2 The half-wave potential of the (p-(Mn)-CoO@NiO / NCNTs@CC) sample is 0.8675 V vs. RHE, and the limiting current density is 19.24 mA cm -2 The OER catalytic activity was also tested under exactly the same conditions as the ORR test, e.g. Figure 3 Curve (p-(Mn)-CoO@NiO / NCNTs@CC) sample at a current density of 50 mA cm -2 The OER overpotential is 320 mV. The current density is 100 mA cm -2 When , the OER overpotential is 348 mV.
[0092] The above specific implementations do not constitute a limitation on the protection scope of the present invention. It should be understood by those skilled in the art that various modifications, combinations, sub-combinations and substitutions may occur depending on design requirements and other factors. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A zinc-air battery bifunctional catalyst, characterized in that: Its structural unit uses nitrogen-doped iron-based carbon nanotubes as a conductive network, and nitrogen and sulfur co-doped manganese, cobalt and nickel tri-metal alloys are loaded on the conductive network.
2. A method for preparing a zinc-air battery bifunctional catalyst as claimed in claim 1, characterized in that: The specific steps include: (a) preparation of nitrogen-doped iron-based carbon nanotubes; (ii) loading manganese, cobalt, nickel trimetallic hydroxide nanoneedles by hydrothermal reaction to obtain manganese, cobalt, nickel trimetallic hydroxide@nitrogen-doped iron-based carbon nanotubes; (iii) In an inert atmosphere, plasma-assisted sulfurization of manganese-cobalt-nickel trihydroxide@nitrogen-doped iron-based carbon nanotubes was performed using radio frequency plasma technology.
3. The method for preparing a zinc-air battery bifunctional catalyst according to claim 2, characterized in that: The preparation process of step (1) comprises: (1) Cut a piece of 3*4cm 2 The raw carbon cloth was placed in ethanol and deionized water, respectively, and ultrasonicated for 10 min; (2) Weigh 5 g of Fe(SO4)2·7H2O, dissolve it in 100 mL of deionized water, stir it evenly, put the ultrasonicated carbon cloth into it, soak it in a 60°C environment for 12 h, then take out the iron-attached carbon cloth and put it in an oven to dry for 12 h; (3) Place the dried iron-attached carbon cloth on a porcelain boat, place it in a tube furnace, introduce argon and ammonia gas, and heat at 5℃ min -1 After the temperature was raised to 500°C at a heating rate of 100 °C, the temperature was kept for 30 min for nitriding. After cooling, the porcelain boat was taken out. 1.2 g of melamine was weighed and placed under the iron-attached carbon cloth in the porcelain boat. The porcelain boat was placed in a tubular furnace and argon was introduced at 10 °C min -1 The temperature was raised to 850°C at a heating rate for further annealing. After keeping the temperature for 120 minutes, the reaction was completed. After cooling, the nitrogen-doped iron-based carbon nanotubes were taken out and recorded as NCNTs@CC.
4. The method for preparing a zinc-air battery bifunctional catalyst according to claim 2, characterized in that: The preparation process of the step (ii) comprises: dissolving a manganese transition metal salt, a cobalt transition metal salt, a nickel transition metal salt, urea and ammonium fluoride in deionized water, stirring and dissolving them fully, pouring them into a polytetrafluoroethylene liner, placing nitrogen-doped iron-based carbon nanotubes, and then placing the polytetrafluoroethylene liner in a high-pressure reactor, reacting at 80 to 200° C. for 6 to 24 hours. After the reaction is completed, the reaction is taken out after cooling, rinsed with deionized water and ethanol, and placed in an oven for drying for 6 to 24 hours to obtain manganese, cobalt, and nickel trimetallic hydroxide @ nitrogen-doped iron-based carbon nanotubes, recorded as MnCoNiLDH / NCNTs@CC.
5. The method for preparing a zinc-air battery bifunctional catalyst according to claim 4, characterized in that: The manganese transition metal salt is one or more of MnCO3, MnCl2·4H2O, MnCl2, and Mn(NO3)2·4H2O; the cobalt transition metal salt is one or more of Co(NO3)2·6H2O, CoCl2·6H2O, Co(CH3COO)2·4H2O, CoSO4·6H2O, and CoCl2; the nickel transition metal salt is NiC 10 H 14 One or more of O4, NiCl2·6H2O, Ni(NO3)2·6H2O, NiC4H6O4·4H2O, and NiCO3.
6. The method for preparing a zinc-air battery bifunctional catalyst according to claim 5, characterized in that: The molar ratio of the manganese transition metal salt: the cobalt transition metal salt: the nickel transition metal salt is 0.25:1:0.
5.
7. The method for preparing a zinc-air battery bifunctional catalyst according to claim 2, characterized in that: The preparation process of step (iii) includes: placing the manganese, cobalt, nickel trimetallic hydroxide @ nitrogen-doped iron-based carbon nanotubes and thiourea obtained in step (ii) into a porcelain boat, placing the porcelain boat into a plasma enhanced chemical vapor deposition device, introducing nitrogen gas, and performing plasma-assisted sulfurization. The pressure in the tube is 20 Pa, the discharge power is 100 W, and the discharge time is 10 min. The obtained zinc-air battery bifunctional catalyst is recorded as p-(Mn)-CoNi2S4@Co2N / NCNTs@CC.
Citation Information
Cited By
Iron-nickel bimetallic carbon-based nano-enzyme capable of synergistically generating electricity and treating wastewater, electrode and preparation method and application of iron-nickel bimetallic carbon-based nano-enzyme
CN120040001A
In-situ growth carbon nanotube loaded iron-cobalt bifunctional catalyst as well as preparation method and application thereof
CN121331844A
In-situ grown carbon nanotube supported iron-cobalt bifunctional catalyst, preparation method and application thereof
CN121331844B
Preparation method and application of high-entropy layered double hydroxide oxygen evolution catalyst
CN121874831A