Preparation method of efficient three-phase transition metal sulfide electrolyzed water working electrode
By using hydrothermal method to grow three-phase transition metal sulfide composite materials on foam nickel substrates, the single performance and high cost problems of Ni3S2 electrocatalysts in the prior art are solved, and low energy consumption and high efficiency electrolytic water electrodes are achieved, with excellent electrocatalytic activity and stability.
Patent Information
- Application Number
- CN202411299851.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art cannot simultaneously realize the reduction of the overpotential of the electrolytic water process, improve the reactivity of the working electrode, reduce the cost of the working electrode preparation and improve stability, especially when using Ni3S2 as an electrocatalyst, there is a single catalytic performance, high overpotential, and synthesis. The problems of complex steps, high cost and poor stability.
The three-phase transition metal sulfide composite material (MoS2/Ni3S2/FeS2/NF) was grown on a foam nickel substrate by hydrothermal method. By regulating the reaction time and component ratio, efficient three-phase transition metal sulfide electrolytic work was prepared. Electrode, used for electrocatalytic water analytical hydrogen reaction, oxygen evolution reaction and total water dissolution.
The electrode with excellent electrocatalytic performance and stability at low energy consumption and low cost is realized. The MoS2/Ni3S2/FeS2/NF-24h electrode exhibits low hydrogen evolution reaction overpotential and oxygen evolution reaction overpotential in 1M KOH solution. And it maintains extremely high stability under long-term current density, far exceeding that of precious metal electrodes.
Smart Images

Figure CN119082788A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a working electrode for electrolyzing water. Background Art
[0002] Global warming, environmental pollution and energy crisis have triggered a strong demand for renewable / clean energy. Countries around the world have begun to actively advocate energy transformation and research and exploration of new energy. In this context, the development of renewable, clean and efficient new energy is imminent. Hydrogen energy has attracted much attention among various renewable energy sources due to its environmental friendliness, zero emissions and high energy. The production of hydrogen by electrolysis of water is the safest, most effective and promising energy supply solution to solve the current energy crisis. The electrocatalytic water splitting reaction consists of two half reactions: hydrogen evolution reaction on the cathode and oxygen evolution reaction on the anode. The reaction kinetics of hydrogen evolution reaction is relatively slow under alkaline conditions of industrial water electrolysis. The oxygen evolution reaction is a four-electron reaction process, which is also relatively slow in kinetics and requires a higher overpotential to drive the reaction to occur and proceed, resulting in a significant increase in the total energy required for the electrolysis of water, which is regarded as the bottleneck of electrocatalytic water splitting. Although precious metal catalysts such as Pt, Ru and Ir exhibit high water splitting efficiency, their scarcity and high cost pose a major obstacle to the improvement of commercial water electrolysis electrodes. Therefore, the development of new electrocatalytic working electrodes that are abundant, low-cost, efficient and stable is of great strategic significance in the fields of hydrogen evolution reaction, oxygen evolution reaction and overall water splitting technology.
[0003] In recent years, people have designed and prepared a variety of new transition metal-based electrochemical water splitting electrodes, such as sulfides, borides, phosphides, amorphous metal alloys, etc., which are loaded on conductive substrates to form working electrodes. In particular, transition metal sulfides have attracted widespread research interest due to their unique structural characteristics, rich active sites, changeable components and electronic configurations. Among them, Ni3S2 is a metal sulfide existing in natural ores. Its overall structure has a continuous Ni-Ni bond network and thus has good conductivity. Ni3S2 is widely considered as an oxygen evolution reaction electrocatalyst, but its hydrogen evolution reaction performance is not ideal. Therefore, Ni3S2 as a single system cannot exhibit bifunctional activity. Currently, many studies focus on the exposure of active sites of Ni3S2, among which element doping and defect induction strategies are relatively common means. However, most of the reported electrodes prepared by Ni3S2-related water electrolysis catalysts have problems such as only having a single catalytic performance, high overpotential, complex synthesis steps, high cost and poor stability. Therefore, how to reduce the overpotential of the complete water splitting process, improve the reaction activity of the working electrode, reduce the preparation cost of the working electrode and improve the stability has become a difficult problem in industrial water electrolysis. Summary of the invention
[0004] The present invention aims to solve the problem that the prior art cannot simultaneously achieve reducing the overpotential of the full water splitting process, improving the reaction activity of the working electrode, reducing the preparation cost of the working electrode and improving the stability, and further provide a method for preparing an efficient three-phase transition metal sulfide water electrolysis working electrode.
[0005] A method for preparing an efficient three-phase transition metal sulfide water electrolysis working electrode is carried out according to the following steps:
[0006] The FeMo6 precursor, thiourea and Ni(NO3)2 are dissolved in water to obtain a mixed solution, the mixed solution is poured into a reactor, the nickel foam is immersed in the mixed solution, and then reacted at a temperature of 180°C to 200°C for 20h to 32h, cooled to room temperature, the nickel foam is taken out and washed and dried to obtain an efficient three-phase transition metal sulfide water electrolysis working electrode;
[0007] The mass ratio of the FeMo6 precursor to thiourea is 1:(0.145-0.187); the mass ratio of the FeMo6 precursor to Ni(NO3)2 is 1:(0.092-0.316).
[0008] The beneficial effects of the present invention are:
[0009] The present invention utilizes a hydrothermal method to reasonably control the reaction time, and grows a three-phase transition metal sulfide composite material (abbreviated as MoS2 / Ni3S2 / FeS2 / NF) on a nickel foam substrate as a working electrode for water electrolysis, which is used for electrocatalytic water decomposition hydrogen reaction, oxygen evolution reaction and complete water splitting. The MoS2 / Ni3S2 / FeS2 / NF-24h electrode exhibits excellent electrocatalytic performance in 1M KOH solution. As a working electrode, MoS2 / Ni3S2 / FeS2 / NF-24h has a high electrocatalytic performance at 10 mA cm -2 When the overpotential of hydrogen evolution reaction is 39mV, at 100mAcm -2 When the current density is 100mAcm -2 When the hydrogen evolution reaction and oxygen evolution reaction were carried out for 100 h, the stability changed only slightly. -2 When MoS2 / Ni3S2 / FeS2 / NF-24h∥MoS2 / Ni3S2 / FeS2 / NF-24h is used, the overall water splitting potential of MoS2 / Ni3S2 / FeS2 / NF-24h is only 1.49V, which is much higher than that of precious metal electrodes and has excellent stability. The present invention provides a low-energy, low-cost and simple technical route and research method for the preparation of multiphase transition metal sulfide electrodes and the study of their high-efficiency electrocatalytic hydrogen evolution reaction, oxygen evolution reaction and overall water splitting performance.
[0010] Instruction Manual
[0011] Figure 1 XRD diagrams: (a) MoS2 / Ni3S2 / FeS2 / NF-24h electrode and standard PDF cards of Ni3S2, MoS2, and FeS2; (b) XRD comparison diagram of MoS2 / Ni3S2 / FeS2 / NF electrodes prepared at different reaction times;
[0012] Figure 2 XPS graphs of MoS2 / Ni3S2 / FeS2 / NF-24h electrode, (a) full spectrum, (b) Ni 2p fine spectrum, (c) Mo 3d fine spectrum, (d) Fe 2p fine spectrum, (e) S2p fine spectrum;
[0013] Figure 3 The morphology images of MoS2 / Ni3S2 / FeS2 / NF-24h electrode at different magnifications, (a) scale bar 100μm, (b) scale bar 20μm;
[0014] Figure 4 LSV, Tafel slope and it curve tests of electrocatalytic hydrogen evolution of MoS2 / Ni3S2 / FeS2 / NF electrode and 20% Pt / C / NF electrode, (a) LSV, (b) Tafel slope, (c) it curve;
[0015] Figure 5 LSV, Tafel slope and it curve test of electrocatalytic oxygen evolution reaction of MoS2 / Ni3S2 / FeS2 / NF electrode and RuO2 / NF electrode, (a) LSV, (b) Tafel slope, (c) it curve;
[0016] Figure 6 CV curves of MoS2 / Ni3S2 / FeS2 / NF electrode in the non-Faraday range, (a) MoS2 / Ni3S2 / FeS2 / NF-20h electrode, (b) MoS2 / Ni3S2 / FeS2 / NF-24h electrode, (c) MoS2 / Ni3S2 / FeS2 / NF-28h electrode, (d) MoS2 / Ni3S2 / FeS2 / NF-32h electrode;
[0017] Figure 7 C of MoS2 / Ni3S2 / FeS2 / NF electrode dl Value and Nyquist plot, (a) C dl Value, (b) Nyquist plot;
[0018] Figure 8 MoS2 / Ni3S2 / FeS2 / NF-24h∥MoS2 / Ni3S2 / FeS2 / NF-24h and Pt / C / NF(-) ∥RuO2 / NF (+) Polarization curves and long-term stability it curves of complete water splitting in a two-electrode system, (a) polarization curve (without iR correction), (b) long-term stability it curve. DETAILED DESCRIPTION
[0019] Specific implementation method 1: This implementation method is a method for preparing an efficient three-phase transition metal sulfide water electrolysis working electrode, which is carried out according to the following steps:
[0020] The FeMo6 precursor, thiourea and Ni(NO3)2 are dissolved in water to obtain a mixed solution, the mixed solution is poured into a reactor, the nickel foam is immersed in the mixed solution, and then reacted at a temperature of 180°C to 200°C for 20h to 32h, cooled to room temperature, the nickel foam is taken out and washed and dried to obtain an efficient three-phase transition metal sulfide water electrolysis working electrode;
[0021] The mass ratio of the FeMo6 precursor to thiourea is 1:(0.145-0.187); the mass ratio of the FeMo6 precursor to Ni(NO3)2 is 1:(0.092-0.316).
[0022] The beneficial effects of this embodiment are:
[0023] In this embodiment, a hydrothermal method is used to reasonably control the reaction time, and a three-phase transition metal sulfide composite material (abbreviated as MoS2 / Ni3S2 / FeS2 / NF) is grown on a nickel foam substrate as a working electrode for water electrolysis, which is used for electrocatalytic water decomposition, oxygen evolution reaction and complete water splitting. The MoS2 / Ni3S2 / FeS2 / NF-24h electrode exhibits excellent electrocatalytic performance in 1M KOH solution. As a working electrode, MoS2 / Ni3S2 / FeS2 / NF-24h has a high electrocatalytic performance at 10 mA cm -2 When the overpotential of hydrogen evolution reaction is 39mV, at 100mAcm -2 When the current density is 100mAcm -2 When the hydrogen evolution reaction and oxygen evolution reaction were carried out for 100 h, the stability changed only slightly. -2 When MoS2 / Ni3S2 / FeS2 / NF-24h∥MoS2 / Ni3S2 / FeS2 / NF-24h is used, the overall water splitting potential of MoS2 / Ni3S2 / FeS2 / NF-24h is only 1.49V, which is much higher than that of precious metal electrodes and has excellent stability. This embodiment provides a low-energy, low-cost and simple technical route and research method for the preparation of multiphase transition metal sulfide electrodes and the study of their high-efficiency electrocatalytic hydrogen evolution reaction, oxygen evolution reaction and overall water splitting performance.
[0024] Specific embodiment 2: This embodiment is different from the specific embodiment 1 in that the FeMo6 precursor is prepared according to the following steps:
[0025] ①(NH4)6Mo7O 24 4H2O is dissolved in distilled water to obtain ammonium molybdate solution;
[0026] ② Dissolve Fe(NO3)3·9H2O in distilled water to obtain ferric nitrate solution;
[0027] ③ At a temperature of 80°C to 100°C and under stirring conditions, add the ferric nitrate solution dropwise to the ammonium molybdate solution until the pH is 2.5 to 3, and then continue heating and stirring at a temperature of 80°C to 100°C and under stirring conditions for 1h to 3h to obtain a dark brown solution;
[0028] ④ Filter and separate the dark brown solution to obtain a crude product, recrystallize the crude product, and finally dry it to room temperature to obtain a FeMo6 precursor. The rest is the same as the first embodiment.
[0029] Specific implementation method three: This implementation method is different from the specific implementation method one or two in that: the (NH4)6Mo7O 24 The mass ratio of 4H2O to the volume ratio of distilled water is 1 g: (12-17) mL. The rest is the same as the first or second embodiment.
[0030] Specific embodiment 4: This embodiment differs from Specific embodiments 1 to 3 in that the mass ratio of Fe(NO3)3·9H2O to the volume ratio of distilled water in step ② is 1 g: (13-15) mL. The rest is the same as Specific embodiments 1 to 3.
[0031] Specific embodiment 5: This embodiment is different from specific embodiments 1 to 4 in that the stirring speed in step ③ is 500 rpm to 700 rpm. The rest is the same as specific embodiments 1 to 4.
[0032] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that: in step ③, the ferric nitrate solution is added dropwise to the ammonium molybdate solution at a dropping speed of 2 drops / minute to 5 drops / minute. The rest is the same as specific embodiments 1 to 5.
[0033] Specific embodiment 7: This embodiment is different from Specific embodiments 1 to 6 in that: in step ④, the crude product is recrystallized 1 to 3 times in hot water at a temperature of 60° C. to 100° C. The rest is the same as Specific embodiments 1 to 6.
[0034] Specific implementation eight: This implementation differs from specific implementations one to seven in that the pore size of the foamed nickel is 0.1 mm to 5 mm, and the porosity is 80% to 98%. The rest is the same as specific implementations one to seven.
[0035] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that the mass ratio of the FeMo6 precursor to the volume of water is 1 g: (93-100) mL. The rest is the same as specific embodiments 1 to 8.
[0036] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that the volume ratio of the nickel foam to the mixed solution is 1 cm 3 : (80-85) mL. The rest is the same as the first to ninth embodiments.
[0037] The following examples are used to verify the beneficial effects of the present invention:
[0038] Embodiment 1:
[0039] A method for preparing an efficient three-phase transition metal sulfide water electrolysis working electrode is carried out according to the following steps:
[0040] 0.26g FeMo6 precursor, 0.04g thiourea and 0.03g Ni(NO3)2 were dissolved in 25mL water to obtain a mixed solution, which was poured into a reactor, and 1cm×2cm×1.5mm nickel foam was immersed in the mixed solution, and then reacted at 200℃ for 20h, cooled to room temperature, and the nickel foam was taken out and washed and dried to obtain an efficient three-phase transition metal sulfide water electrolysis working electrode, named MoS2 / Ni3S2 / FeS2 / NF-20h electrode;
[0041] The average pore size of the nickel foam is 0.1 mm, and the porosity is 97%;
[0042] The FeMo6 precursor is specifically prepared according to the following steps:
[0043] ①(NH4)6Mo7O 24 4H2O (5.19 g, 4.2 mmol) was dissolved in 80 mL of distilled water to obtain an ammonium molybdate solution;
[0044] ② Dissolve Fe(NO3)3·9H2O (1.41 g, 3.5 mmol) in 20 mL of distilled water to obtain ferric nitrate solution;
[0045] ③ Under the conditions of temperature of 100°C, stirring speed of 600 rpm and dropping speed of 2 drops / min, add the ferric nitrate solution dropwise to the ammonium molybdate solution until the pH is 2.5-3, then continue heating and stirring for 2 hours at temperature of 100°C and stirring speed of 600 rpm to obtain a dark brown solution;
[0046] ④ The dark brown solution was filtered and separated to obtain a crude product (3.85 g). The crude product was recrystallized twice in hot water at 80°C and finally dried to room temperature to obtain a FeMo6 precursor (3.2 g).
[0047] Example 2: This example is different from Example 1 in that the reaction is carried out at a temperature of 200°C for 24 hours and the product is named MoS2 / Ni3S2 / FeS2 / NF-24h electrode. The rest is the same as Example 1.
[0048] Example 3: This example is different from Example 1 in that the reaction is carried out at a temperature of 200°C for 28 hours and the product is named MoS2 / Ni3S2 / FeS2 / NF-28h electrode. The rest is the same as Example 1.
[0049] Example 4: This example is different from Example 1 in that the reaction is carried out at a temperature of 200°C for 32 hours and the product is named MoS2 / Ni3S2 / FeS2 / NF-32h electrode. The rest is the same as Example 1.
[0050] Comparative experiment: 5 mg of 20% Pt / C or RuO2 powder was dispersed in 1 mL of a solution containing 0.95 mL of anhydrous ethanol and 50 μL of 0.5 wt% nafion. The mixture was then ultrasonicated for 30 minutes to form a uniform slurry. Finally, 0.35 mL of 20% Pt / C or RuO2 slurry was evenly applied to one side of the nickel foam (1 cm × 2 cm × 1.5 mm) over an area of 1 cm. 2 , and dried at room temperature for 24 h to obtain a 20% Pt / C / NF electrode or RuO2 / NF electrode.
[0051] Figure 1 XRD diagrams: (a) MoS2 / Ni3S2 / FeS2 / NF-24h electrode and standard PDF cards of Ni3S2, MoS2, and FeS2; (b) XRD comparison diagram of MoS2 / Ni3S2 / FeS2 / NF electrode prepared at different reaction times. Figure 1As shown in (a), the diffraction peaks at 21.8°, 31.1°, 37.8°, 49.7°, 54.6° and 55.2° correspond to the (101), (110), (003), (113), (104) and (122) crystal planes of Ni3S2 (PDF#44-1418), respectively. The diffraction peaks at 14.4°, 35.9° and 49.9° correspond to the (002), (102) and (105) crystal planes of MoS2 (PDF#73-1508), respectively. The diffraction peaks at 40.8°, 53.4° and 64.3° correspond to the (-1-12), (031) and (-1-23) crystal planes of FeS2 (PDF#71-1680), respectively. The diffraction peaks at 44.6°, 51.8° and 76.4° correspond to the (111), (200) and (220) crystal planes of nickel foam (PDF#04-0850), respectively, indicating that the electrode composition is MoS2, Ni3S2, FeS2 and NF. Figure 1 (b) It can be seen that the XRD characteristic peaks at different reaction times do not change, indicating that the composition of the electrodes is the same.
[0052] Figure 2 XPS graphs of MoS2 / Ni3S2 / FeS2 / NF-24h electrode, (a) full spectrum, (b) Ni 2p fine spectrum, (c) Mo 3d fine spectrum, (d) Fe 2p fine spectrum, (e) S2p fine spectrum. Figure 2 As shown in (a), it can be observed that the MoS2 / Ni3S2 / FeS2 / NF-24h electrode contains Ni 2p, Fe 2p, Mo 3d, and S2p elements. Figure 2 As shown in (b), Ni 2p has two valences, +2 and +3, and the four peaks are: 855.6eV, 873.4eV, 857.7eV and 875.6eV, which correspond to Ni 2+ 2p 3 / 2,Ni 2+ 2p 1 / 2 and Ni 3+ 2p3 / 2、Ni 3+ 2p 1 / 2. Figure 2 As shown in (c), two typical characteristic peaks appear, which are 231.7eV and 234.9eV, respectively, which are attributed to Mo 4+ 3d 5 / 2 and Mo 4+ 3d 3 / 2, which is also the characteristic peak of MoS2. Figure 2 As shown in (d), at 704.3 eV is Fe 0 The characteristic peaks of 710.8eV and 723.2eV are attributed to Fe 2 + 2p 3 / 2 and Fe 2+2p1 / 2, while the characteristic peaks at 716.3eV and 729.2eV belong to Fe 2+ Satellite peaks. Figure 2 As shown in (e), the characteristic peaks at 160.9 eV and 162.1 eV are attributed to S 2- 2p 3 / 2 and S 2- 2p 1 / 2, while the characteristic peaks at 164.1eV and 167.5eV are attributed to S2 2- and SO x characteristic peaks.
[0053] Figure 3 The morphology images of MoS2 / Ni3S2 / FeS2 / NF-24h electrode at different magnifications, (a) scale 100μm, (b) scale 20μm; it can be seen from the figure that many rod-like structures of different sizes, irregularly shaped nanoclusters and nanoparticles are grown on the nickel foam substrate, and the multiphase interface interaction helps to improve the electrocatalytic activity.
[0054] Electrochemical test: The electrochemical test was carried out at room temperature and pressure using Shanghai Chenhua Company's CHI760E electrochemical workstation. A typical three-electrode system was used, with a graphite rod as the counter electrode, Ag / AgCl as the reference electrode, MoS2 / Ni3S2 / FeS2 / NF electrode, 20% Pt / C / NF electrode or RuO2 / NF electrode as the working electrode, and the electrolyte was 1 mol / L KOH solution, pH = 14. Full water splitting test: A two-electrode system was used, with the MoS2 / Ni3S2 / FeS2 / NF-24h electrode as both the positive and negative electrodes, to study its overall water electrolysis performance in a 1.0 mol / L KOH solution (pH = 14), and with a 20% Pt / C / NF (-) ∥RuO2 / NF (+) For comparative experiments.
[0055] Figure 4 LSV, Tafel slope and it curve test of electrocatalytic hydrogen evolution of MoS2 / Ni3S2 / FeS2 / NF electrode and 20% Pt / C / NF electrode, (a) LSV, (b) Tafel slope, (c) it curve. Figure 4 As shown in (a) and 4(b), in 1 mol / L KOH solution, the current density is 10 mA cm -2 When the overpotential of hydrogen evolution reaction of MoS2 / Ni3S2 / FeS2 / NF-20h, 24h, 28h, 32h and 20%Pt / C / NF electrode is 83mV, 39mV, 46mV, 51mV and 21mV, the corresponding Tafel slope is 98mVdec -1 、59mV dec -1、78mV dec -1 、84mV dec -1 and 32mV dec -1 Except for the noble metal 20% Pt / C / NF electrode, the MoS2 / Ni3S2 / FeS2 / NF-24h electrode has the lowest overpotential and Tafel slope for hydrogen evolution reaction, indicating that the MoS2 / Ni3S2 / FeS2 / NF-24h electrode has the best electrocatalytic hydrogen evolution activity. Long-term stability is very important for catalysts. Figure 4 (c) is at a current density of 100 mA cm -2 The IT cycle curve after 100h shows that the current density retention rate after 100h of cycling is as high as 98%, indicating that the hydrogen evolution reaction stability of the MoS2 / Ni3S2 / FeS2 / NF-24h electrode is very good.
[0056] Figure 5 LSV, Tafel slope and it curve test of the electrocatalytic oxygen evolution reaction of MoS2 / Ni3S2 / FeS2 / NF electrode and RuO2 / NF electrode, (a) LSV, (b) Tafel slope, (c) it curve. Figure 5 (a) and 5(b), in 1 mol / L KOH solution, the current density is 100 mA cm -2 When the oxygen evolution reaction overpotential of MoS2 / Ni3S2 / FeS2 / NF-20h, 24h, 28h, 32h and RuO2 / NF electrode is 486mV, 323mV, 346mV, 350mV and 468mV, the corresponding Tafel slope is 87mVdec -1 、47mV dec -1 、54mV dec -1 、55mV dec -1 and 74mV dec -1 The overpotential and Tafel slope of oxygen evolution reaction of MoS2 / Ni3S2 / FeS2 / NF-24h electrode are the lowest, exceeding that of the precious metal RuO2 / NF electrode, indicating that the electrocatalytic oxygen evolution activity of MoS2 / Ni3S2 / FeS2 / NF-24h electrode is the best. Figure 5 (c) is at 100mAcm -2 The IT cycle curve after 100 h at the current density shows that the current density retention rate after 100 h of cycling is as high as 97%, indicating that the electrocatalytic oxygen evolution reaction stability of the MoS2 / Ni3S2 / FeS2 / NF-24h electrode is very excellent.
[0057] Figure 6CV curves of MoS2 / Ni3S2 / FeS2 / NF electrode in the non-Faraday range, (a) MoS2 / Ni3S2 / FeS2 / NF-20h electrode, (b) MoS2 / Ni3S2 / FeS2 / NF-24h electrode, (c) MoS2 / Ni3S2 / FeS2 / NF-28h electrode, (d) MoS2 / Ni3S2 / FeS2 / NF-32h electrode; Figure 7 C of MoS2 / Ni3S2 / FeS2 / NF electrode dl Value and Nyquist plot, (a) C dl Value, (b) Nyquist plot. Figure 7 (a) is the calculation result of the linear fitting slope of the CV curve of MoS2 / Ni3S2 / FeS2 / NF electrode. It can be seen that the C dl The values are 6.1, 11.6, 8.3 and 7.2 mF cm -2 , indicating that the MoS2 / Ni3S2 / FeS2 / NF-24h electrode has the largest electrochemical active area. The electrochemical impedance of the MoS2 / Ni3S2 / FeS2 / NF electrode is shown in Figure 7 (b), it can be seen that MoS2 / Ni3S2 / FeS2 / NF-24h has the smallest charge transfer resistance.
[0058] Figure 8 MoS2 / Ni3S2 / FeS2 / NF-24h∥MoS2 / Ni3S2 / FeS2 / NF-24h and Pt / C / NF (-) ∥RuO2 / NF (+) Polarization curves and long-term stability it curves of the two-electrode system for complete water splitting, (a) polarization curve (without iR correction), (b) long-term stability it curve. As shown in 8(a), at a current density of 10 mA cm -2 When the electrolysis voltage of the MoS2 / Ni3S2 / FeS2 / NF-24h two-electrode system is 1.49V, the noble metal Pt / C / NF (-) ∥RuO2 / NF (+) is 1.61 V. This shows that the water electrolysis performance of MoS2 / Ni3S2 / FeS2 / NF-24h electrode is much better than that of precious metal electrodes. Figure 8 (b) It can be seen that at a current density of 100 mA cm -2 The MoS2 / Ni3S2 / FeS2 / NF-24h two-electrode system has excellent stability under the condition of 1.5 mol·s·kg / min. It can be seen that the MoS2 / Ni3S2 / FeS2 / NF-24h electrode in situ grown on the nickel foam substrate has excellent bifunctional electrocatalytic activity and outstanding stability.
Claims
1. A method for preparing an efficient three-phase transition metal sulfide water electrolysis working electrode, characterized in that It is carried out in the following steps: The FeMo6 precursor, thiourea and Ni(NO3)2 are dissolved in water to obtain a mixed solution, the mixed solution is poured into a reactor, the nickel foam is immersed in the mixed solution, and then reacted at a temperature of 180°C to 200°C for 20h to 32h, cooled to room temperature, the nickel foam is taken out and washed and dried to obtain an efficient three-phase transition metal sulfide water electrolysis working electrode; The mass ratio of the FeMo6 precursor to thiourea is 1:(0.145-0.187); the mass ratio of the FeMo6 precursor to Ni(NO3)2 is 1:(0.092-0.316).
2. The method for preparing an efficient three-phase transition metal sulfide water electrolysis working electrode according to claim 1, characterized in that The FeMo6 precursor is specifically prepared according to the following steps: ①(NH4)6Mo7O 24 4H2O is dissolved in distilled water to obtain ammonium molybdate solution; ② Dissolve Fe(NO3)3·9H2O in distilled water to obtain ferric nitrate solution; ③ At a temperature of 80°C to 100°C and under stirring conditions, add the ferric nitrate solution dropwise to the ammonium molybdate solution until the pH is 2.5 to 3, and then continue heating and stirring at a temperature of 80°C to 100°C and under stirring conditions for 1h to 3h to obtain a dark brown solution; ④ Filter and separate the dark brown solution to obtain a crude product, recrystallize the crude product, and finally dry it to room temperature to obtain a FeMo6 precursor.
3. The method for preparing an efficient three-phase transition metal sulfide water electrolysis working electrode according to claim 2, characterized in that (NH4)6Mo7O described in step ① 24 The mass ratio of 4H2O to the volume of distilled water is 1g:(12~17)mL.
4. The method for preparing an efficient three-phase transition metal sulfide water electrolysis working electrode according to claim 2, characterized in that The mass ratio of Fe(NO3)3·9H2O to distilled water described in step ② is 1g:(13-15)mL.
5. The method for preparing an efficient three-phase transition metal sulfide water electrolysis working electrode according to claim 2, characterized in that The stirring speed in step ③ is 500 rpm to 700 rpm.
6. The method for preparing an efficient three-phase transition metal sulfide water electrolysis working electrode according to claim 2, characterized in that In step ③, the ferric nitrate solution is added dropwise to the ammonium molybdate solution at a dropping speed of 2 drops / minute to 5 drops / minute.
7. The method for preparing an efficient three-phase transition metal sulfide water electrolysis working electrode according to claim 2, characterized in that In step ④, the crude product is recrystallized 1 to 3 times in hot water at a temperature of 60°C to 100°C.
8. The method for preparing an efficient three-phase transition metal sulfide water electrolysis working electrode according to claim 1, characterized in that The pore size of the foamed nickel is 0.1 mm to 5 mm, and the porosity is 80% to 98%.
9. The method for preparing an efficient three-phase transition metal sulfide water electrolysis working electrode according to claim 1, characterized in that The mass ratio of the FeMo6 precursor to the volume of water is 1g:(93-100)mL.
10. The method for preparing an efficient three-phase transition metal sulfide water electrolysis working electrode according to claim 1, characterized in that The volume ratio of the nickel foam to the mixed solution is 1 cm 3 :(80~85)mL.