Rare earth aluminum phosphites, their preparation methods, uses and compositions

By preparing a compound of rare earth-aluminum phosphite and alkyl phosphonate aluminum, the problem of poor thermal stability of inorganic phosphorus flame retardants was solved, the flame retardant properties and impact strength of the polymer were improved, and the corrosivity was reduced.

CN118992995BActive Publication Date: 2026-11-17BAOTOU RESEARCH INSTITUTE OF RARE EARTHS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411067640.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2026-11-17
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

Existing inorganic phosphorus-based flame retardants, such as aluminum hypophosphite and lanthanum phosphite, suffer from poor thermal stability and high water solubility during use, which makes the polymers prone to decomposition and ignition during processing.

Method used

A rare earth-aluminum phosphite preparation method was adopted, which involves adding aluminum source slurry dropwise to a phosphorous acid solution, followed by the addition of a rare earth compound slurry, and controlling the reaction temperature and time to prepare rare earth-aluminum phosphite. This phosphite is then compounded with aluminum alkylphosphinate for use in polymers.

Benefits of technology

It improves the flame retardant properties of the polymer, maintains high impact strength and low corrosivity, and enhances the safety and stability of the polymer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118992995B_ABST
    Figure CN118992995B_ABST
Patent Text Reader

Abstract

This invention discloses a rare earth-aluminum phosphite, its preparation method, uses, and composition. The preparation method of this invention includes the following steps: (1) adding an aluminum source slurry dropwise to a phosphorous acid solution to obtain an acidic aluminum phosphite slurry; (2) adding a rare earth compound slurry to the acidic aluminum phosphite slurry to obtain the rare earth-aluminum phosphite; wherein the aluminum source in the aluminum source slurry is selected from one or more of aluminum hydroxide, boehmite, gibbsite, and boehmite; and the rare earth compound is selected from one or more of rare earth oxides, rare earth hydroxides, and rare earth carbonates. The rare earth-aluminum phosphite prepared by the method of this invention can effectively improve the flame retardant properties of polymers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a rare earth-aluminum phosphite, its preparation method, uses, and composition. Background Technology

[0002] Inorganic phosphorus-based flame retardants are favored by users due to their advantages such as long-lasting flame retardant effect, good thermal stability, non-volatile nature, and halogen-free content. Aluminum hypophosphite is a representative of inorganic phosphorus-based flame retardants; however, aluminum hypophosphite is prone to decomposition during use and can easily ignite during processing, especially when the raw materials contain fibers.

[0003] CN116812894A discloses a phosphite material with the chemical formula Al. x Zn y (OH) z (HPO3)3·wH2O; where 1.5≤x≤2.5; 0<y≤1; 0<z≤1.5, and w is an integer from 0 to 4. This phosphite contains aluminum and zinc, contains hydroxyl groups and water, and has poor thermal stability.

[0004] CN11483991A discloses a method for preparing lanthanum phosphite. Lanthanum oxide and a catalyst are added to water, and the water temperature is maintained at 30–35°C to obtain a hydration product. The catalyst is selected from formic acid, acetic acid, sulfuric acid, or benzenesulfonic acid. The hydration product is added to a reaction vessel, and phosphorous acid is continuously added dropwise while maintaining the reaction vessel temperature at 40–80°C. After the addition is completed, the reaction is maintained at this temperature for 2–5 hours to obtain a rare earth phosphorous acid product. The rare earth phosphorous acid product is filtered, dried, and pulverized to obtain the finished lanthanum phosphite. The product obtained by this method is lanthanum phosphite, which has poor temperature resistance and high water solubility. Summary of the Invention

[0005] In view of this, one object of the present invention is to provide a method for preparing a rare earth-aluminum phosphite, wherein the rare earth-aluminum phosphite prepared by the method of the present invention can effectively improve the flame retardancy of polymers. Furthermore, when the rare earth-aluminum phosphite prepared by the method of the present invention is added to a polymer, the resulting composition maintains high impact strength and low corrosivity. Another object of the present invention is to provide a rare earth-aluminum phosphite. A further object of the present invention is to provide a use of the rare earth-aluminum phosphite. Yet another object of the present invention is to provide a composition.

[0006] The above objectives are achieved through the following technical solutions.

[0007] On the one hand, the present invention provides a method for preparing rare earth-aluminum phosphite, comprising the following steps:

[0008] (1) Add aluminum source slurry dropwise to phosphorous acid solution to obtain acidic aluminum phosphite slurry;

[0009] (2) Add the rare earth compound slurry to the acidic aluminum phosphite slurry to obtain rare earth-aluminum phosphite;

[0010] The aluminum source in the aluminum source slurry is selected from one or more of aluminum hydroxide, boehmite, gibbsite, and boehmite.

[0011] The rare earth compound is selected from one or more of rare earth oxides, rare earth hydroxides, and rare earth carbonates.

[0012] According to the preparation method of the present invention, preferably, the rare earth compound is selected from one or more of lanthanum oxide, lanthanum hydroxide, and lanthanum carbonate.

[0013] According to the preparation method of the present invention, preferably, in step (1), the reaction temperature is 50-140℃ and the reaction time is 1-8h; in step (2), the reaction temperature is 50-140℃ and the reaction time is 1-8h.

[0014] According to the preparation method of the present invention, preferably, the mass ratio of aluminum source to phosphorous acid is (3.5-6.5):16.88; the molar ratio of rare earth element in rare earth compound to phosphorous acid is (0.2-0.7):2.

[0015] According to the preparation method of the present invention, preferably, step (2) includes the following steps:

[0016] Rare earth compound slurry is added to acidic aluminum phosphite slurry, and then reacted at 50-140℃ for 1-8 hours to obtain reactant; the reactant is filtered and then dried at 100-150℃ to obtain rare earth-aluminum phosphite.

[0017] According to the preparation method of the present invention, preferably, in the aluminum source slurry, the mass ratio of aluminum source to water is (4-6):(6-9); in the phosphorous acid solution, the mass ratio of phosphorous acid to water is 16.88:(20-30); and in the rare earth compound slurry, the mass ratio of rare earth compound to water is 1:(0.7-2).

[0018] On the other hand, the present invention provides a rare earth-aluminum phosphite obtained by the above preparation method.

[0019] In another aspect, the present invention provides the use of the above-mentioned rare earth-aluminum phosphite in improving the flame retardant properties of polymers.

[0020] In another aspect, the present invention provides a composition comprising the above-mentioned rare earth-aluminum phosphite and alkylphosphinate aluminum.

[0021] According to the composition of the present invention, preferably, the composition further comprises a polymer selected from one or more of nylon, polybutylene terephthalate, polyethylene terephthalate, polyurethane, and acrylonitrile-styrene-butadiene copolymer.

[0022] The rare earth-aluminum phosphite prepared by the method of this invention can effectively improve the flame retardancy of polymers. Furthermore, when the rare earth-aluminum phosphite prepared by the method of this invention is added to the polymer, the resulting composition maintains high impact strength and low corrosivity. Attached Figure Description

[0023] Figure 1 and Figure 2 The images are SEM images of the rare earth-aluminum phosphite obtained in Example 1 at different magnifications.

[0024] Figure 3 and Figure 4 The images shown are SEM images of the rare earth-aluminum phosphite obtained in Example 2 at different magnifications.

[0025] Figure 5 and Figure 6 The images shown are SEM images of the rare earth-aluminum phosphite obtained in Example 3 at different magnifications.

[0026] Figure 7 EDS diagram of rare earth-aluminum phosphite obtained in Example 2.

[0027] Figure 8 The XRD patterns are of the rare earth-aluminum phosphites obtained in Examples 1-3. Detailed Implementation

[0028] The present invention will be further described below with reference to specific embodiments, but the scope of protection of the present invention is not limited thereto.

[0029] <Preparation Method of Rare Earth-Aluminum Phosphite>

[0030] The preparation method of the present invention includes the following steps: (1) preparing an acidic aluminum phosphite slurry; and (2) obtaining rare earth-aluminum phosphite. These steps are described in detail below.

[0031] Steps for preparing acidic aluminum phosphite slurry

[0032] Aluminum source slurry is added dropwise to phosphorous acid solution to obtain acidic aluminum phosphite slurry.

[0033] The phosphorous acid solution comprises phosphorous acid and water. The mass ratio of phosphorous acid to water can be 16.88:(20-30); preferably 16.88:(22-28). In some embodiments, the mass ratio of phosphorous acid to water is 16.88:(24-26). Phosphorous acid and water can be mixed to form a phosphorous acid solution.

[0034] The aluminum source in the aluminum source slurry can be selected from one or more of aluminum hydroxide, boehmite, gibbsite, and boehmite. In some embodiments, the aluminum source is aluminum hydroxide. In other embodiments, the aluminum source is boehmite. In still other embodiments, the aluminum source is gibbsite.

[0035] The aluminum source slurry includes an aluminum source and water. The mass ratio of aluminum source to water can be (4-6):(6-9); preferably (4.5-5.5):(6.5-8.5); more preferably (5-5.2):(7-8).

[0036] The aluminum source can be dispersed in water to form an aluminum source slurry.

[0037] The mass ratio of aluminum source to phosphorous acid can be (3.5-6.5):16.88; preferably (4.5-5.5):16.88; more preferably (5.1-5.2):16.88.

[0038] The reaction temperature can be 50–140°C; preferably 70–110°C; more preferably 80–90°C.

[0039] The reaction time can be 1 to 8 hours; preferably 2 to 6 hours; more preferably 2 to 4 hours. The reaction time is calculated from the time the aluminum source slurry is added.

[0040] The phosphorous acid solution can be heated to 50–140°C, preferably 70–110°C, and more preferably 80–90°C, and then aluminum source slurry can be added dropwise to it.

[0041] Steps to obtain rare earth-aluminum phosphite

[0042] Rare earth compound slurry is added to acidic aluminum phosphite slurry to obtain rare earth-aluminum phosphite.

[0043] The rare earth compound may be selected from one or more of rare earth oxides, rare earth hydroxides, and rare earth carbonates. The rare earth element in the rare earth compound may be selected from one or more of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium, and yttrium. Preferably, the rare earth element in the rare earth compound is selected from one or more of lanthanum and cerium. The rare earth compound may be selected from one or more of lanthanum oxide, lanthanum hydroxide, and lanthanum carbonate. According to one embodiment of the present invention, the rare earth compound is lanthanum oxide.

[0044] The rare earth compound slurry comprises rare earth compounds and water. The mass ratio of rare earth compounds to water can be 1:(0.7-2); preferably 1:(1-1.8); more preferably 1:(1.3-1.6).

[0045] Rare earth compounds and water can be stirred at 50–140°C; preferably 70–120°C; more preferably 80–100°C for 1–6 h; and preferably 2–4 h to obtain a rare earth compound slurry.

[0046] Rare earth compound slurries can be pumped into aluminum phosphite slurries. For example, a peristaltic pump can be used to pump the rare earth compound slurry into the aluminum phosphite slurry.

[0047] The molar ratio of rare earth elements to phosphorous acid in rare earth compounds can be (0.2-0.7):2; preferably (0.3-0.6):2; more preferably (0.32-0.4):2.

[0048] The reaction temperature can be 50–140°C; preferably 70–120°C; more preferably 80–100°C.

[0049] The reaction time can be 1 to 8 hours; preferably 2 to 6 hours; more preferably 3 to 5 hours.

[0050] The reaction can be carried out under stirring.

[0051] Specifically, a rare earth compound slurry is added to an acidic aluminum phosphite slurry, and then reacted at 50–140°C for 1–8 hours to obtain a reactant; the reactant is filtered and then dried at 100–150°C to obtain rare earth-aluminum phosphite.

[0052] The drying temperature can be 100–150℃; preferably 110–140℃; more preferably 120–130℃. Drying can be carried out using methods such as oven drying, vacuum drying, flash drying, or ribbon drying.

[0053] Rare Earth Aluminum Phosphites and Their Uses

[0054] The rare earth-aluminum phosphite of the present invention is prepared by the above method. This rare earth-aluminum phosphite can improve the flame retardant properties of polymers.

[0055] Therefore, the present invention also provides the use of the above-mentioned rare earth-aluminum phosphite in improving the flame retardant properties of polymers.

[0056] The polymer can be selected from one or more of nylon, polybutylene terephthalate, polyethylene terephthalate, polyurethane, and acrylonitrile-styrene-butadiene copolymer. Preferably, the polymer is nylon. Nylon can be selected from one or more of PA6, PA66, PA11, and PA12. According to one embodiment of the present invention, the nylon is a mixture of PA6 and PA66. The mass ratio of PA6 to PA66 can be 10:(20-60); preferably 10:(30-50); more preferably 10:(35-45).

[0057] <Composition>

[0058] The composition of this invention comprises the above-mentioned rare earth-aluminum phosphite and alkyl phosphinate aluminum. This invention has found that combining the above-mentioned rare earth-aluminum phosphite with alkyl phosphinate aluminum results in a better flame-retardant effect.

[0059] The alkylphosphinate group in aluminum alkylphosphinate can be represented as shown in formula (I):

[0060]

[0061] R1 and R2 are each independently selected from H, C1-C6 alkyl groups, and at least one of R1 and R2 is not H. Preferably, R1 and R2 are each independently selected from C1-C3 alkyl groups.

[0062] Examples of alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl, neopentyl, n-hexyl, 2-methylpentyl, 3-methylpentyl, 2,3-dimethylbutyl, and 2,2-dimethylbutyl.

[0063] According to one embodiment of the present invention, aluminum alkylphosphinate is aluminum diethylphosphinate.

[0064] The amount of rare earth-aluminum phosphite used can be 1 to 6 parts by weight; preferably 2 to 5 parts by weight; more preferably 3 to 4 parts by weight; and most preferably 3 to 3.2 parts by weight.

[0065] The amount of alkylphosphinic acid aluminum can be 8 to 18 parts by weight; preferably 10 to 16 parts by weight; more preferably 12 to 15 parts by weight; and most preferably 12 to 13 parts by weight.

[0066] The compositions of the present invention may also include polymers. In some embodiments, the compositions may also include one or more of antioxidants, lubricants, color masterbatches, and glass fibers.

[0067] The polymer can be selected from one or more of nylon, polybutylene terephthalate, polyethylene terephthalate, polyurethane, and acrylonitrile-styrene-butadiene copolymer. Preferably, the polymer is nylon. Nylon can be selected from one or more of PA6, PA66, PA11, and PA12. According to one embodiment of the present invention, the nylon is a mixture of PA6 and PA66. The mass ratio of PA6 to PA66 can be 10:(20-60); preferably 10:(30-50); more preferably 10:(35-45).

[0068] The amount of polymer used can be 30 to 70 parts by weight; preferably 40 to 60 parts by weight; more preferably 50 to 55 parts by weight; even more preferably 52 to 53 parts by weight.

[0069] The amount of antioxidant used can be 0.1 to 1.5 parts by weight; preferably 0.3 to 1 part by weight; more preferably 0.5 to 0.8 parts by weight. The antioxidant can be a mixture of antioxidant 1098 and antioxidant 608. The mass ratio of antioxidant 1098 to antioxidant 608 can be 2:(1 to 5); preferably 2:(3 to 4).

[0070] The amount of lubricant used can be 0.1 to 1 part by weight; preferably 0.2 to 0.8 parts by weight; more preferably 0.3 to 0.5 parts by weight. The lubricant can be wax powder. According to one embodiment of the present invention, the lubricant is Honeywell AC540A.

[0071] The amount of color masterbatch can be 0.3 to 3 parts by weight; preferably 0.5 to 2 parts by weight; more preferably 1 to 1.5 parts by weight. Black masterbatch is preferred.

[0072] The amount of glass fiber can be 10 to 50 parts by weight; preferably 20 to 40 parts by weight; more preferably 30 to 35 parts by weight.

[0073] The composition of the present invention can be prepared by the following method: extruding raw materials through a twin-screw extruder to obtain a molded material. Cooling the molded material and then granulating it to obtain the composition.

[0074] The raw materials are described below:

[0075] PA6 grade 2400J was purchased from Hangzhou Juhua Shun New Materials Co., Ltd.

[0076] PA66 grade EPR24 was purchased from Pingdingshan Shenma Engineering Plastics Co., Ltd.

[0077] The glass fiber grade is ECS301UW, purchased from Chongqing International Composite Materials Co., Ltd.

[0078] Aluminum diethylphosphonate was purchased from Qingdao Ouprui New Materials Co., Ltd.

[0079] Aluminum phosphite was purchased from Shenzhen Ruishixing Technology Co., Ltd.

[0080] Lubricant AC540A was purchased from Honeywell.

[0081] The black masterbatch grade is PA3785, purchased from Cabot Corporation in the United States.

[0082] The testing method is described below:

[0083] If the following test methods require processing into specimens, the composition shall be dried and then processed into specimens at 280°C on an injection molding machine, unless otherwise specified.

[0084] UL94: HB rating is evaluated using a horizontal burning test, while V0-V2 ratings are evaluated using a 500W (125mm) vertical burning test.

[0085] Notched impact strength: Tested according to the method specified in ISO 179-1.

[0086] Example 1

[0087] 5.2 kg of aluminum hydroxide and 8.0 kg of water were dispersed to form an aluminum source slurry. 16.88 kg of phosphorous acid was mixed with 25.32 kg of water to obtain a phosphorous acid solution. The phosphorous acid solution was heated to 80 °C, and then the aluminum source slurry was added dropwise to it. After the aluminum source slurry was completely added, the mixture was reacted at 80 °C for 2 hours to obtain an acidic aluminum phosphite slurry.

[0088] 5.61 kg of lanthanum oxide and 8.5 kg of water were stirred at 80 °C for 3 h to obtain a rare earth compound slurry. The rare earth compound slurry was pumped into an acidic aluminum phosphite slurry, and then reacted at 80 °C with stirring for 3 h to obtain the reactant. The reactant was cooled, filtered, and then dried at 120 °C to obtain rare earth-aluminum phosphite.

[0089] Figure 1 and Figure 2 This is a SEM image of the rare earth-aluminum phosphite obtained in this embodiment. Figure 1 and Figure 2 It is understood that the rare earth-aluminum phosphite in this embodiment includes elongated grains and irregular blocky grains; the two types of grains are dispersed or aggregated together.

[0090] According to the TG curve, the thermal weight loss temperature of 1 wt% rare earth-aluminum phosphite in this embodiment is 433.7℃.

[0091] Example 2

[0092] 5.0 kg of boehmite and 7.25 kg of water were dispersed to form an aluminum source slurry. 16.88 kg of phosphorous acid was mixed with 25.62 kg of water to obtain a phosphorous acid solution. The phosphorous acid solution was heated to 95°C, and then the aluminum source slurry was added dropwise to it. After the aluminum source slurry was completely added, the mixture was reacted at 95°C for 2 hours to obtain an acidic aluminum phosphite slurry.

[0093] 5.59 kg of lanthanum oxide and 5.72 kg of water were stirred at 80 °C for 3 h to obtain a rare earth compound slurry. The rare earth compound slurry was pumped into an acidic aluminum phosphite slurry and reacted at 80 °C with stirring for 3 h to obtain the reactant. The reactant was cooled, filtered, and then dried at 120 °C to obtain rare earth-aluminum phosphite.

[0094] Figure 3 and Figure 4 This is a SEM image of the rare earth-aluminum phosphite obtained in this embodiment. Figure 3 and Figure 4 It is understood that the rare earth-aluminum phosphite in this embodiment includes elongated grains and irregular blocky grains; the two types of grains are dispersed or aggregated together.

[0095] According to the TG curve, the thermal weight loss temperature of 1 wt% rare earth-aluminum phosphite in this embodiment is 391.7 °C.

[0096] Figure 7 This is the EDS diagram of rare earth-aluminum phosphite in this embodiment. (From...) Figure 7 It can be seen that the deposits grown on the surface of rare earth diethylphosphite are aluminum-containing compounds, which also contain elements such as phosphorus and oxygen, and can be inferred to be aluminum diethylphosphite.

[0097] Example 3

[0098] 5.3 kg of gibbsite and 7 kg of water were dispersed to form an aluminum source slurry. 16.88 kg of phosphorous acid was mixed with 22.12 kg of water to obtain a phosphorous acid solution. The phosphorous acid solution was heated to 100°C, and then the aluminum source slurry was added dropwise to it. After the aluminum source slurry was completely added, the mixture was reacted at 100°C for 4 hours to obtain an acidic aluminum phosphite slurry.

[0099] 8.40 kg of lanthanum oxide and 8.68 kg of water were stirred at 80 °C for 3 h to obtain a rare earth compound slurry. The rare earth compound slurry was pumped into an acidic aluminum phosphite slurry and reacted at 80 °C with stirring for 5 h to obtain the reactant. The reactant was cooled, filtered, and then dried at 120 °C to obtain rare earth-aluminum phosphite.

[0100] Figure 5 and Figure 6 This is a SEM image of the rare earth-aluminum phosphite obtained in this embodiment. Figure 5and Figure 6 It is understood that the rare earth-aluminum phosphite in this embodiment includes elongated grains and irregular blocky grains; the two types of grains are dispersed or aggregated together.

[0101] According to the TG curve, the thermal weight loss temperature of 1 wt% rare earth-aluminum phosphite in this embodiment is 471.7 °C.

[0102] Figure 8 The images show the XRD patterns of the rare earth-aluminum phosphites obtained in Examples 1-3. Figure 8 It can be seen that the diffraction peak positions and peak heights of the rare earth-aluminum phosphites obtained in Examples 1-3 are basically the same, and the crystal phase structures of the rare earth-aluminum phosphites obtained in each example are the same.

[0103] Examples 4-6, Comparative Examples 1-2

[0104] PA66 and PA6 were placed in a twin-screw extruder (model: KTS35 / 44D); aluminum diethylphosphinate, phosphite, 0.2 parts by weight of antioxidant 1098, 0.3 parts by weight of antioxidant 608, 0.3 parts by weight of AC540A, and 1 part by weight of black masterbatch were mixed and then fed into the twin-screw extruder through the first side feed port at 260°C; 30 parts by weight of glass fiber were added to the twin-screw extruder through the second side feed port; the mixture was extruded through the twin-screw extruder to obtain the molded material. The molded material was cooled in a water bath and then granulated to obtain the composition.

[0105] The types and amounts of some raw materials are shown in Table 1, and the properties of the composition are shown in Table 1.

[0106] Table 1

[0107]

[0108] Note: Each group of UL94 experiments is conducted five times. A*X indicates that X of the five experiments yielded a result of grade A.

[0109] Corrosion test

[0110] PA66 and PA6 were placed in a twin-screw extruder (model: KTS35 / 44D); a brass block with a mass of m1 was installed on the die of the twin-screw extruder; aluminum diethylphosphinate, phosphite, antioxidant 1098, antioxidant 608, AC540A, and black masterbatch were mixed and then added to the twin-screw extruder through the first side feed port at 260°C; glass fiber was added to the twin-screw extruder through the second side feed port; the material was extruded through the twin-screw extruder to obtain the molded material. The molded material was cooled in a water bath and then granulated.

[0111] The total weight of the raw materials (PA66, PA6, aluminum diethylphosphinate, phosphite, antioxidant 1098, antioxidant 608, AC540A, black masterbatch and glass fiber) is 25 kg.

[0112] The mass of the brass block on the die head after granulation is measured and recorded as m2. The loss of the brass block is calculated according to the formula (m1-m2) / m1, and the corrosivity of the composition is judged based on the loss of the brass block.

[0113] The selection and proportion of each raw material are shown in Table 2, and the corrosivity is shown in Table 2.

[0114] Table 2

[0115]

[0116] As shown in Tables 1 and 2, the rare earth-aluminum phosphite compound of the present invention, compared with the aluminum phosphite compound, can achieve better flame retardant effect and maintain high notched impact strength and low corrosivity of nylon.

[0117] This invention is not limited to the above-described embodiments. Any modifications, improvements, or substitutions that can be conceived by those skilled in the art without departing from the essential content of this invention fall within the scope of this invention.

Claims

1. A method for producing a rare earth-aluminum subphosphate, characterized by, Includes the following steps: (1) Add aluminum source slurry dropwise to phosphorous acid solution, and then react at 50-140℃ for 1-8h to obtain acidic aluminum phosphite slurry; (2) Add the rare earth compound slurry to the acidic aluminum phosphite slurry, and then react at 50-140℃ for 1-8 hours to obtain rare earth-aluminum phosphite; The aluminum source in the aluminum source slurry is selected from one or more of aluminum hydroxide, boehmite, gibbsite, and boehmite. The rare earth compound is selected from one or more of rare earth oxides, rare earth hydroxides, and rare earth carbonates.

2. The production method according to claim 1, characterized by, The rare earth compound is selected from one or more of lanthanum oxide, lanthanum hydroxide, and lanthanum carbonate.

3. The preparation method according to claim 1, characterized in that, The mass ratio of aluminum source to phosphorous acid is (3.5~6.5):16.88; the molar ratio of rare earth elements to phosphorous acid in rare earth compounds is (0.2~0.7):

2.

4. The method of claim 1, wherein, Step (2) includes the following steps: Rare earth compound slurry is added to acidic aluminum phosphite slurry, and then reacted at 50-140℃ for 1-8 hours to obtain reactant; the reactant is filtered and then dried at 100-150℃ to obtain rare earth-aluminum phosphite.

5. The preparation method according to claim 1, characterized in that, In the aluminum source slurry, the mass ratio of aluminum source to water is (4-6):(6-9); in the phosphorous acid solution, the mass ratio of phosphorous acid to water is 16.88:(20-30); in the rare earth compound slurry, the mass ratio of rare earth compound to water is 1:(0.7-2).

6. A rare earth-aluminum subphosphate characterized by, The rare earth-aluminum phosphite is obtained by the preparation method according to any one of claims 1 to 5.

7. The use of the rare earth-aluminum phosphite according to claim 6 in improving the flame retardant properties of polymers.

8. A composition characterized in that, The composition comprises the rare earth-aluminum phosphite and alkylphosphinate aluminum as described in claim 6.

9. The composition of claim 8, wherein, The composition further includes a polymer selected from one or more of nylon, polybutylene terephthalate, polyethylene terephthalate, polyurethane, and acrylonitrile-styrene-butadiene copolymer.

Citation Information

Patent Citations

  • Rare earth metal hypophosphite and preparation method and application of rare earth metal hypophosphite

    CN102838098A

  • Flame retardant-stabilizer combination for thermoplastic polymers

    CN103154110A