High-performance natural graphite negative electrode material and preparation method and application thereof
By using hydrated tar and sulfonated graphene coating technology, a high-performance natural graphite anode material with a core-shell structure is formed, which solves the problems of cycle performance and specific capacity of natural graphite in lithium-ion batteries, and realizes the preparation of efficient and low-cost anode materials.
Patent Information
- Application Number
- CN202411042471.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-22
AI Technical Summary
Existing natural graphite anode materials suffer from reduced cycle performance in lithium-ion batteries due to volume expansion during lithium-ion intercalation. Furthermore, conventional amorphous carbon coating methods reduce compaction density and specific capacity, increasing costs.
A composite coating technology using hydrated tar, emulsifier, and sulfonated graphene is employed to form a high-performance natural graphite anode material with a core-shell structure through spray drying and high-temperature carbonization, avoiding complex equipment and toxic solvents, and achieving uniform thin-layer coating.
It improves the cycle performance and initial coulombic efficiency of natural graphite anode materials while maintaining high compaction density and specific capacity, making it suitable for large-scale production.
Smart Images

Figure BDA0004972714050000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of negative electrode materials for lithium ion batteries, and specifically relates to a high-performance natural graphite negative electrode material and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries are widely used in many portable electronic devices such as laptops, mobile phones, and instrument lights due to their high specific capacity, high operating voltage, good safety, and no memory effect. With the popularization of new energy vehicles, their application scope has expanded to electric vehicles and other fields. In recent years, as the requirements for miniaturization, lightweight, multi-function, and long-term driving of electronic products and vehicle-mounted and energy storage equipment continue to increase, the requirements for high energy density, high rate performance, and long cycle life of lithium-ion batteries continue to increase.
[0003] Lithium-ion batteries are widely used in 3C products and power storage and other fields. Commercial lithium-ion batteries mainly use carbon negative electrode materials such as natural graphite, artificial graphite, soft carbon and hard carbon. Among them, natural graphite is widely used as an important negative electrode material because of its high specific capacity, good charge and discharge platform and low cost. However, since the interlayer spacing of the lithium-intercalated compound LixC6 formed during the lithium ion embedding process is larger than the interlayer spacing of natural graphite, the natural graphite will also undergo a volume expansion of about 10% during charging and discharging, causing the graphite layer to peel off, thereby reducing the cycle performance of lithium-ion batteries. In addition, the specific surface area can be reduced by high-temperature amorphous carbon coating. Therefore, it is an important technical means to improve the first charge and discharge efficiency of natural graphite negative electrode materials. However, the conventional method causes a high amorphous carbon content (the coating layer is too thick), which will reduce the compaction density of spherical graphite, resulting in a decrease in the gram capacity of the lithium battery, and will also increase the cost. Therefore, it is necessary to develop a high-performance negative electrode material that takes into account gram capacity, cycle and first coulomb efficiency (first effect). Summary of the invention
[0004] In order to improve the problems existing in the prior art, the present invention provides a high-performance natural graphite negative electrode material and a preparation method and application thereof. The high-performance natural graphite negative electrode material has high compaction density and first coulombic efficiency, and also has excellent cycle performance; the preparation method does not require complex process equipment and toxic organic solvents, meets the requirements of green and low-cost chemistry, and is conducive to the large-scale production of high-performance natural graphite negative electrode materials.
[0005] The object of the present invention is achieved through the following technical solutions:
[0006] A method for preparing a high-performance natural graphite negative electrode material, the preparation method comprising the following steps:
[0007] (1) mixing hydrated tar and an emulsifier to prepare an emulsion;
[0008] (2) under vacuum conditions, mixing natural graphite and the emulsion of step (1), and impregnating under pressure to obtain slurry 1;
[0009] (3) spray drying the slurry 1 obtained in step (2) to obtain powder 1;
[0010] (4) mixing the powder 1 of step (3), the sulfonated graphene and water to obtain a slurry 2;
[0011] (5) spray drying the slurry 2 obtained in step (4) to obtain powder 2;
[0012] (6) mixing the powder 2 of step (5) with the emulsion of step (1) to obtain slurry 3;
[0013] (7) spray drying the slurry 3 obtained in step (6) to obtain powder 3;
[0014] (8) Carbonizing the powder 3 of step (7) to prepare the high-performance natural graphite negative electrode material.
[0015] According to an embodiment of the present invention, in step (1), the hydrated tar is a recovered product of asphalt flue gas, which can be prepared by methods known in the art or purchased through commercial channels.
[0016] According to an embodiment of the present invention, in step (1), the hydrated tar comprises water and tar.
[0017] According to an embodiment of the present invention, in step (1), the mass percentage of water in the hydrated tar is 50-65wt%, for example, 50wt%, 55wt%, 60wt% or 65wt%.
[0018] According to an embodiment of the present invention, in step (1), the mass percentage of tar in the hydrated tar is 35-50wt%, for example, 35wt%, 40wt%, 45wt% or 50wt%.
[0019] According to an embodiment of the present invention, in step (1), the carbon residue value of the hydrated tar after carbonization is ≤5%.
[0020] According to an embodiment of the present invention, in step (1), the emulsifier is selected from non-ionic emulsifiers, such as sucrose fatty acid esters, sorbitan fatty acid, polysorbate, polyoxyethylene fatty acid esters, polyoxyethylene fatty alcohol ethers, or a mixture of several thereof.
[0021] According to an embodiment of the present invention, in step (1), the mass ratio of the emulsifier to the hydrated tar is (2.5-8):100, preferably (2.5-6.5):100, for example, 2.5:100, 3:100, 3.5:100, 4:100, 4.5:100, 5:100, 5.5:100, 6:100 or 6.5:100.
[0022] According to an embodiment of the present invention, in step (1), the mixing is carried out under stirring conditions. The stirring speed is 20-80 r / min, and the stirring time is 40-120 min.
[0023] According to an embodiment of the present invention, in step (2), the mass ratio of the natural graphite to the emulsion is 100:(200-400), for example, 100:200, 100:250, 100:300, 100:350 or 100:400.
[0024] According to an embodiment of the present invention, in step (2), the shape of the natural graphite is at least one of spherical, approximately spherical, oval, and potato-shaped, and the D 50 5~17μm, carbon content ≥99.0%.
[0025] According to an embodiment of the present invention, in step (2), the vacuum degree of the vacuum condition is 0.07 to 0.09 MPa.
[0026] According to an embodiment of the present invention, in step (2), the natural graphite is first placed under vacuum, and then mixed with the emulsion under vacuum. Preferably, the natural graphite is first placed under vacuum for a period of time, such as more than 5 minutes, such as 10-180 minutes, and the air inside the natural graphite is discharged under vacuum.
[0027] According to an embodiment of the present invention, step (2) is performed in a reactor. Preferably, natural graphite is placed in a reactor, and the reactor is evacuated to make it in a vacuum state. The reactor is evacuated for, for example, 10 to 30 minutes. Then, the emulsion is added under vacuum. The emulsion is added by, for example, opening the emulsion suction valve, sucking the emulsion of step (1) into the reactor, and closing the suction valve after the emulsion is added. Preferably, the vacuum is stopped after the emulsion is added.
[0028] According to an embodiment of the present invention, in step (2), the pressure of the pressurized impregnation is 2 MPa to 10 MPa, for example, 2 MPa, 3 MPa, 4 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa or 10 MPa; and the time of the pressurized impregnation is 1 to 5 hours.
[0029] According to an embodiment of the present invention, step (2) further comprises a post-treatment step: after the pressure impregnation is completed, the pressure is reduced to make the pressure inside and outside the reaction system the same, and then the material is discharged and centrifuged.
[0030] According to an embodiment of the present invention, in step (4), the mass ratio of the sulfonated graphene, powder 1 and water is (0.5-1.5):100:(100-300).
[0031] According to an embodiment of the present invention, step (4) specifically comprises: mixing the powder 1 and sulfonated graphene of step (3) with water, stirring the mixture, and centrifuging the mixture to obtain a slurry 2.
[0032] According to an embodiment of the present invention, in step (6), the mass ratio of the emulsion of step (1) to the powder 2 is (100-180):100, for example, 100:100, 120:100, 130:100, 140:100, 150:100, 160:100, 170:100 or 180:100.
[0033] According to an embodiment of the present invention, in step (6), after the mixing is completed, the mixture may be centrifuged.
[0034] According to an embodiment of the present invention, in step (3), (5) or (7), the drying temperature is 100-150° C., for example, 100° C., 110° C., 120° C., 130° C., 140° C. or 150° C. The drying time is 1-6 hours, preferably 2-4 hours, for example, 2 hours, 3 hours, 4 hours, 5 hours or 6 hours.
[0035] According to an embodiment of the present invention, in step (8), the carbonization treatment is performed under an inert atmosphere, such as nitrogen or argon.
[0036] According to an embodiment of the present invention, in step (8), the temperature of the carbonization treatment is 800-1200° C., for example, 800° C., 850° C., 900° C., 950° C., 1000° C., 1050° C., 1100° C., 1150° C. or 1200° C. The time of the carbonization treatment is 1-6 hours, preferably 2-4 hours, for example, 2 hours, 3 hours, 4 hours, 5 hours or 6 hours.
[0037] The present invention also provides a high-performance natural graphite negative electrode material prepared by the method.
[0038] According to an embodiment of the present invention, the high-performance natural graphite negative electrode material has a core-shell structure, wherein the core is natural graphite with amorphous carbon coated on the inner and outer surfaces, the inner shell is sulfonated graphene, and the outer shell is amorphous carbon.
[0039] According to the present invention, the mass fraction of amorphous carbon in the high-performance natural graphite negative electrode material is 1.0-3.5%, for example, 1.5%, 1.8%, 2.0%, 2.6%, 3.0%, 3.2%, 3.5%; the mass fraction of sulfonated graphene is 0.6-2.5%, more preferably 0.6-2%.
[0040] The present invention also provides a use of the high-performance natural graphite negative electrode material, which is used in preparing lithium-ion batteries, preferably in preparing the negative electrode of lithium-ion batteries.
[0041] The present invention also provides a negative electrode for a lithium ion battery, wherein the negative electrode comprises the above-mentioned high-performance natural graphite negative electrode material.
[0042] Beneficial effects of the present invention:
[0043] The method of the present invention comprises the following steps: adding an emulsifier to hydrated tar to uniformly disperse the tar in water to obtain an emulsion; exhausting air inside the natural graphite under vacuum, and then mixing the natural graphite with the emulsion, wherein the tar in the emulsion can penetrate into the curled scaly graphite layers inside the natural graphite under high pressure to form a uniform and thin tar coating layer on the inner surface of the natural graphite, and can also be coated on the outer surface of natural graphite particles; after spray drying (i.e., powder 1), the powder is mixed with sulfonated graphene, and spray dried to coat the sulfonated graphene on the inner and outer surfaces of the natural graphite coated with tar; finally, mixing the natural graphite coated with sulfonated graphene (i.e., powder 2) with the emulsion, wherein during the mixing process, the tar in the emulsion forms a uniform and thin tar coating layer on the surface of the sulfonated graphene; and during the high-temperature carbonization process, the tar coated on the surfaces of the curled scaly graphite layers inside the natural graphite, the outer surface of the natural graphite and the surface of the sulfonated graphene is carbonized to form a uniform and thin amorphous carbon. In the present invention, the uniform and thin amorphous carbon layer coated on the surface of each curled flake graphite layer inside the natural graphite in the core can prevent the organic molecules in the electrolyte from penetrating into the spherical graphite to generate a new SEI film during the charge and discharge process, and prevent the curled graphite layer inside the spherical graphite from peeling off; the sulfonated graphene in the inner shell has good flexibility, which can alleviate the volume expansion of natural graphite during charge and discharge, and improve the cycle performance of natural graphite to 1500 weeks. The outermost amorphous carbon layer can reduce the specific surface area of the sulfonated graphene in the inner shell, and prevent the problem of the first efficiency reduction of the lithium ion battery caused by the sulfonated graphene coating. The amorphous carbon layer in the natural graphite negative electrode material of the present invention is uniform and thin (the amorphous carbon content is low), and will not reduce the compaction density and gram specific capacity of the negative electrode material.
[0044] (2) The preparation method of the present invention does not require complex process equipment and toxic organic solvents, meets the requirements of green, low-cost chemistry, and is conducive to the large-scale production of negative electrode materials. The preparation method can use low-cost asphalt flue gas recovery (i.e., hydrated tar) to prepare negative electrode materials for lithium-ion batteries, realizing the utilization of waste resources. The preparation method uses water as a dispersion medium, has a simple process, does not require post-processing processes such as washing, and does not require complex process equipment, making it easy to achieve large-scale production of graphite negative electrode materials. DETAILED DESCRIPTION
[0045] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0046] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0047] Example 1
[0048] (1) 200 g of hydrated tar (water content of 50% by mass, residual carbon value of 4% after tar carbonization) and 7 g of polysorbate were mixed and stirred (stirring speed of 60 r / min) for 50 min to obtain an emulsion;
[0049] (2) 100 g of natural graphite was placed in a reactor and vacuumed for 50 min. When the vacuum degree of the reactor reached 0.07 MPa, the emulsion suction valve was opened to suck all the emulsion prepared in step (1) into the reactor. After the liquid was added, the suction valve was closed and the vacuum was stopped. At the same time, the mixed liquid was stirred at high speed (30 r / min) for 40 min, pressurized (3 MPa) and immersed for 3 hours. After the pressure inside and outside the reactor was reduced to the same, the material was discharged and centrifuged to obtain slurry 1. The slurry 1 was spray-dried at 120° C. for 2 hours to prepare powder 1;
[0050] (3) 100 g of powder 1 of step (2), 0.8 g of sulfonated graphene and 180 g of aqueous solution were mixed and stirred, and then centrifuged to obtain slurry 2, and the slurry 2 was spray-dried at 130° C. to prepare powder 2;
[0051] (4) 100 g of powder 2 of step (3) and 120 g of the emulsion of step (1) were mixed and stirred, and then centrifuged to obtain slurry 3. The slurry 3 was spray-dried at 130° C. to prepare powder 3; the powder 3 was carbonized at 1200° C. in nitrogen for 2 hours, and cooled to room temperature to obtain a high-performance natural graphite negative electrode material.
[0052] In the high-performance natural graphite negative electrode material, the mass proportion of amorphous carbon is 3.0%, and the mass proportion of sulfonated graphene is 0.8%.
[0053] Example 2
[0054] (1) 200 g of hydrated tar (the mass percentage of water is 60%, and the residual carbon value after tar carbonization is 3.5%) and 8 g of sucrose fatty acid ester are mixed and stirred (stirring speed is 40 r / min) for 40 min to obtain an emulsion;
[0055] (2) 100 g of natural graphite was placed in a reactor and vacuumed for 50 min. When the vacuum degree of the reactor reached 0.07 MPa, the emulsion suction valve was opened to suck all the emulsion prepared in step (1) into the reactor. After the liquid was added, the suction valve was closed and the vacuuming was stopped. At the same time, the mixed liquid was stirred at high speed (30 r / min) for 40 min, pressurized (5 MPa) and immersed for 1 hour. After the pressure inside and outside the reactor was reduced to the same, the material was discharged and centrifuged to obtain slurry 1. The slurry 1 was spray-dried at 120° C. for 2 hours to prepare powder 1;
[0056] (3) 100 g of powder 1 of step (2), 0.6 g of sulfonated graphene and 150 g of aqueous solution were mixed and stirred, and then centrifuged to obtain slurry 2, and the slurry 2 was spray-dried at 120° C. to prepare powder 2;
[0057] (4) 100 g of powder 2 of step (3) and 100 g of the emulsion of step (1) were mixed and stirred, and then centrifuged to obtain slurry 3. The slurry 3 was spray-dried at 120° C. to prepare powder 3; the powder 3 was carbonized at 1200° C. in nitrogen for 2 hours, and cooled to room temperature to obtain a high-performance natural graphite negative electrode material.
[0058] In the high-performance natural graphite negative electrode material, the mass proportion of amorphous carbon is 2.6%, and the mass proportion of sulfonated graphene is 0.6%.
[0059] Example 3
[0060] (2) 250 g of hydrated tar (water content of 60% by mass, 5% residual carbon value after tar carbonization) and 7 g of fatty acid sorbitan were mixed and stirred (stirring speed of 70 r / min) for 30 min to obtain an emulsion;
[0061] (2) 100 g of natural graphite was placed in a reactor and vacuumed for 50 min. When the vacuum degree of the reactor reached 0.07 MPa, the emulsion suction valve was opened to suck all the emulsion prepared in step (1) into the reactor. After the liquid was added, the suction valve was closed and the vacuuming was stopped. At the same time, the mixed liquid was stirred at high speed (30 r / min) for 40 min, pressurized (8 MPa) and immersed for 1 hour. After the pressure inside and outside the reactor was reduced to the same, the material was discharged and centrifuged to obtain slurry 1. The slurry 1 was spray-dried at 120° C. for 2 hours to prepare powder 1;
[0062] (3) 100 g of powder 1 and 1.0 g of sulfonated graphene in step (2) were mixed and stirred with 200 g of aqueous solution, and then centrifuged to obtain slurry 2. The slurry 2 was spray-dried at 130° C. to prepare powder 2;
[0063] (4) 100 g of powder 2 of step (3) and 150 g of the emulsion of step (1) were mixed and stirred, and then centrifuged to obtain slurry 3. The slurry 3 was spray-dried at 130° C. to prepare powder 3; the powder 3 was carbonized at 1200° C. in nitrogen for 2 hours, and cooled to room temperature to obtain a high-performance natural graphite negative electrode material.
[0064] In the high-performance natural graphite negative electrode material, the mass proportion of amorphous carbon is 3.0%, and the mass proportion of sulfonated graphene is 1.1%.
[0065] Example 4
[0066] (1) 200 g of hydrated tar (the mass percentage of water is 53%, and the residual carbon value after tar carbonization is 5%) and 8 g of sucrose fatty acid ester are mixed and stirred (stirring speed is 60 r / min) for 50 min to obtain an emulsion;
[0067] (2) 100 g of natural graphite was placed in a reactor and vacuumed for 50 min. When the vacuum degree of the reactor reached 0.07 MPa, the emulsion suction valve was opened to suck all the emulsion prepared in step (1) into the reactor. After the liquid was added, the suction valve was closed and the vacuuming was stopped. At the same time, the mixed liquid was stirred at high speed (30 r / min) for 40 min, pressurized (10 MPa) and immersed for 2 hours. After the pressure inside and outside the reactor was reduced to the same, the material was discharged and centrifuged to obtain slurry 1. The slurry 1 was spray-dried at 120° C. for 2 hours to prepare powder 1.
[0068] (3) 100 g of powder 1 and 1.3 g of sulfonated graphene in step (2) were mixed with 200 g of aqueous solution, and the mixture was centrifuged to obtain slurry 2. The slurry 2 was spray-dried at 130° C. to obtain powder 2;
[0069] (4) 100 g of powder 2 of step (3) and 160 g of the emulsion of step (1) were mixed and stirred, and then centrifuged to obtain slurry 3. The slurry 3 was spray-dried at 130° C. to prepare powder 3; the powder 3 was high-temperature carbonized in nitrogen at 1200° C. for 2 hours, and cooled to room temperature to obtain a high-performance natural graphite negative electrode material.
[0070] In the high-performance natural graphite negative electrode material, the mass proportion of amorphous carbon is 3.5%, and the mass proportion of sulfonated graphene is 1.5%.
[0071] Comparative Example 1
[0072] (1) 200 g of hydrated tar (the mass percentage of water is 50%, and the residual carbon value after tar carbonization is 3.5%) and 7 g of polysorbate are mixed and stirred (stirring speed is 60 r / min) for 50 min to obtain an emulsion;
[0073] (2) 120 g of natural graphite was placed in a reactor and vacuumed for 50 min. When the vacuum degree of the reactor reached 0.07 MPa, the emulsion suction valve was opened to suck all the emulsion prepared in step (1) into the reactor. After the liquid was added, the suction valve was closed and the vacuuming was stopped. At the same time, the mixed liquid was stirred at high speed (30 r / min) for 40 min, pressurized (3 MPa) and immersed for 3 hours. After the pressure inside and outside the reactor was equalized, the pressure was reduced, the material was discharged and centrifuged to obtain slurry 1, and the slurry 1 was spray-dried at 120° C. for 2 hours to prepare powder 1; the powder 1 was high-temperature carbonized in nitrogen at 1200° C. for 2 hours, and cooled to room temperature to obtain a high-performance natural graphite negative electrode material.
[0074] In the high-performance natural graphite negative electrode material, the mass proportion of amorphous carbon is 3.3%.
[0075] Comparative Example 2
[0076] (1) 200 g of hydrated tar (the mass percentage of water is 50%, and the residual carbon value after tar carbonization is 3.5%) and 7 g of polysorbate are mixed and stirred (stirring speed is 60 r / min) for 50 min to obtain an emulsion;
[0077] (2) 120 g of natural graphite was placed in a reactor and vacuumed for 50 min. When the vacuum degree of the reactor reached 0.07 MPa, the emulsion suction valve was opened to suck all the emulsion prepared in step (1) into the reactor. After the liquid was added, the suction valve was closed and the vacuuming was stopped. At the same time, the mixed liquid was stirred at high speed (30 r / min) for 40 min, pressurized (3 MPa) and immersed for 3 hours. After the pressure inside and outside the reactor was reduced to the same, the material was discharged and centrifuged to obtain slurry 1. The slurry 1 was spray-dried at 120° C. for 2 hours to prepare powder 1;
[0078] (3) 100 g of powder 1 of step (2), 0.8 g of sulfonated graphene and 180 g of aqueous solution were mixed and stirred, and then centrifuged to obtain slurry 2. The slurry 2 was spray-dried at 130° C. to prepare powder 2; the powder 2 was carbonized at 1200° C. in nitrogen for 2 hours, and cooled to room temperature to obtain a high-performance natural graphite negative electrode material.
[0079] In the high-performance natural graphite negative electrode material, the mass proportion of amorphous carbon is 2.9%, and the mass proportion of sulfonated graphene is 0.7%.
[0080] The pole piece compaction density test is in accordance with the national standard GB / T 24533-2019.
[0081] Electrochemical performance test:
[0082] Semi-electric test method: The negative electrode materials prepared in the examples and comparative examples: conductive carbon black (SP): carboxymethyl cellulose (CMC): styrene-butadiene rubber (SBR) = 95:1:1.5:2.5 (mass ratio) were mixed evenly and applied on copper foil. The coated electrode was placed in a vacuum drying oven at 120°C and dried for 12 hours. The simulated battery assembly was carried out in a Braun glove box protected by argon gas. The electrolyte was 1M-LiPF 6 +EC:DEC:DMC (volume ratio of 1:1:1), metal lithium sheet is the counter electrode, and a simulated battery test is carried out in a 5V, 1000mA Xinwei battery test cabinet. The charge and discharge voltage is 0.01-1.5V, and the charge and discharge rate is 0.1C. The 0.1C first charge capacity and 0.1C first coulomb efficiency obtained by the test are listed in Table 1 (Comparative Example 3 in Table 1 is spherical natural graphite).
[0083] Full battery test method: The negative electrode material prepared in the embodiment and the comparative example is used as the negative electrode, lithium cobalt oxide is used as the positive electrode, and 1M-LiPF 6 +EC:DEC:DMC (volume ratio 1:1:1) solution was used as the electrolyte to assemble a full battery, which was charged and discharged at room temperature at a rate of 0.1C with a voltage range of 3.0-4.2V. The cycle performance obtained from the test is listed in Table 1.
[0084] Table 1 Electrochemical performance test results
[0085]
[0086] In Table 1, for Comparative Example 3, after 300 cycles, the 0.1C cycle capacity retention rate is 80.6%, and after 1500 cycles, the 0.1C cycle capacity retention rate is lower than 64.6%.
[0087] The above is an exemplary description of the embodiments of the present invention. However, the protection scope of the present invention is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a high-performance natural graphite negative electrode material, characterized in that: The preparation method comprises the following steps: (1) mixing hydrated tar and an emulsifier to prepare an emulsion; (2) under vacuum conditions, mixing natural graphite and the emulsion of step (1), and impregnating under pressure to obtain slurry 1; (3) spray drying the slurry 1 obtained in step (2) to obtain powder 1; (4) mixing the powder 1 of step (3), the sulfonated graphene and water to obtain a slurry 2; (5) spray drying the slurry 2 obtained in step (4) to obtain powder 2; (6) mixing the powder 2 of step (5) with the emulsion of step (1) to obtain slurry 3; (7) spray drying the slurry 3 obtained in step (6) to obtain powder 3; (8) The powder 3 of step (7) is carbonized to prepare the high-performance natural graphite negative electrode material.
2. The method according to claim 1, characterized in that: In step (1), the mass percentage of water in the hydrated tar is 50-65wt%. Preferably, in step (1), the mass percentage of tar in the hydrated tar is 35-50wt%. Preferably, in step (1), the carbon residue value of the hydrated tar after carbonization is ≤5%. Preferably, in step (1), the emulsifier is selected from non-ionic emulsifiers, such as sucrose fatty acid esters, sorbitan fatty acid, polysorbate, polyoxyethylene fatty acid esters, polyoxyethylene fatty alcohol ethers, or a mixture of several thereof. Preferably, in step (1), the mass ratio of the emulsifier to the hydrated tar is (2.5-8):
100.
3. The method according to claim 1 or 2, characterized in that: In step (2), the mass ratio of the natural graphite to the emulsion is 100:(200-400). Preferably, in step (2), the vacuum degree of the vacuum condition is 0.07-0.09 MPa. Preferably, in step (2), the pressure of the pressurized impregnation is 2 MPa to 10 MPa.
4. The method according to any one of claims 1 to 3, characterized in that: In step (4), the mass ratio of the sulfonated graphene, powder 1 and water is (0.5-1.5):100:(100-300). Preferably, in step (6), the mass ratio of the emulsion in step (1) to the powder 2 is (100-180):
100. Preferably, in step (3), (5) or (7), the temperature of the drying treatment is 100-150° C., and the time of the drying treatment is 1-6 hours.
5. The method according to any one of claims 1 to 4, characterized in that: In step (8), the carbonization treatment is performed under an inert atmosphere, such as nitrogen or argon. Preferably, in step (8), the temperature of the carbonization treatment is 800-1200° C., and the time of the carbonization treatment is 1-6 hours.
6. A high performance natural graphite negative electrode material prepared by the method according to any one of claims 1 to 5.
7. The high performance natural graphite negative electrode material according to claim 6, characterized in that: The high-performance natural graphite negative electrode material has a core-shell structure, wherein the core is natural graphite with amorphous carbon coated on the inner layer surface and the outer layer surface, the inner shell is sulfonated graphene, and the outer shell is amorphous carbon.
8. The high performance natural graphite negative electrode material according to claim 7, characterized in that: The mass fraction of amorphous carbon in the high-performance natural graphite negative electrode material is 1.0-3.5%; the mass fraction of sulfonated graphene is 0.6-2.5%.
9. Use of the high-performance natural graphite negative electrode material according to any one of claims 6 to 8 in the preparation of lithium ion batteries, preferably in the preparation of negative electrodes of lithium ion batteries.
10. A negative electrode for a lithium ion battery, characterized in that: The negative electrode comprises the high-performance natural graphite negative electrode material according to any one of claims 6 to 8.
Citation Information
Patent Citations
Method for preparing carbon cathode material and lithium iron battery using the material
CN101186292A
Preparation method of high-performance silicon carbon anode material
CN107394137A
Carbon nanotube dispersion, slurry for secondary battery electrode, method for producing slurry for secondary battery electrode, secondary battery electrode, and secondary battery
CN111770953A
Cited By
High-performance natural graphite negative electrode material, preparation method therefor, and use thereof
WO2026026206A1