Synthetic method of hafnium dioxide quantum dots

By using hafnium dioxide as a material, using the method of heating and dialysis of the autoclave, hafnium dioxide quantum dots luminescence in the ultraviolet band are prepared, which solves the problem of insufficient luminescence in the prior art and provides stable materials for in the field of luminescence and display.

CN118993142APending Publication Date: 2024-11-22WENZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411062493.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art lacks high stability quantum dots that can emit light in the ultraviolet to blue wavelength (300-450 nm) band, and common semiconductor silicon cannot emit light in this band and has weak response, limiting luminescence, display and imaging. Application in the field.

Method used

By using hafnium dioxide as a material, a synthesis method is designed, including heating the hafnium source and a reducing agent in an autoclave, adjusting the pH value and dialysis treatment, and preparing chemically stable hafnium dioxide quantum dots.

Benefits of technology

The preparation of hafnium dioxide quantum dots luminescent near the ultraviolet band is realized, providing stable material selection for the fields of luminescence, display, photosensitive detection and biological imaging, filling the gaps in the prior art.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993142A_ABST
    Figure CN118993142A_ABST
Patent Text Reader

Abstract

The synthesis method of the hafnium dioxide quantum dots comprises the following steps: 1) preparing an aqueous solution of a hafnium source by taking the hafnium source as a raw material, and adjusting the pH value to 6.5; 2) preparing an aqueous solution of a reducing agent; and 3) mixing the aqueous solution of the hafnium source and the aqueous solution of the reducing agent, then transferring the mixed solution into a high-pressure reaction kettle for heating reaction, and after the reaction is finished, centrifuging to remove large particles and dialyzing to remove unreacted substances to obtain the hafnium dioxide quantum dot solution. According to the synthesis method, the hafnium oxide quantum dots with stable chemical properties can be synthesized, and due to defect-assisted luminescence, the field of the luminescence wavelength is near the ultraviolet band (UVA), so that a choice is provided for preparation of the ultraviolet band luminescence quantum dots with stable chemical properties which are rare at present; the application of the hafnium-based quantum dots in the fields of luminescence, display, optical sensing detection and biological imaging is promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nano material synthesis, and in particular relates to a method for synthesizing hafnium dioxide quantum dots. Background Art

[0002] With the development of display and imaging technology, high luminous efficiency, low energy consumption, and high-quality luminescent materials have become the goal pursued by people. The popular liquid crystal display screens now have some disadvantages: slow response speed, narrow color gamut, narrow light angle, no flexibility and cannot be folded, and relatively fragile. Quantum dots have excellent optical properties, including high color purity, good stability, high fluorescence quantum yield, low energy consumption, and low cost. They have very excellent prospects in the fields of luminescence, display, and imaging. However, there are not many quantum dots that emit light in the ultraviolet to blue wavelength (300-450 nm) band. Common semiconductor silicon cannot emit light in this band and the response is very weak. Therefore, it is very meaningful to develop a quantum dot with stable properties that emits light in the ultraviolet to blue wavelength (300-450nm) band.

[0003] Hafnium dioxide is a material with extremely high stability. The band gap of intrinsic hafnium oxide is large, about 6 eV, and it does not emit light under normal circumstances. It can emit light under the action of defects, and the wavelength is located near the ultraviolet band (UVA) to the blue-violet band. Making hafnium dioxide into a quantum dot structure is very promising for preparing a material with a stable luminescence band from ultraviolet to blue wavelengths, which can pave the way for subsequent luminescence, display, light sensing detection, imaging, and anti-counterfeiting applications. However, the preparation of luminescent hafnium oxide quantum dots has not been reported yet. Summary of the invention

[0004] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for synthesizing hafnium dioxide quantum dots, which is specifically achieved through the following technical solutions: A method for synthesizing hafnium dioxide quantum dots, the method comprising the following steps: 1) Prepare an aqueous solution of hafnium source using hafnium source raw materials and adjust the pH to 6.5; 2) preparing an aqueous solution of a reducing agent; 3) Mixing the aqueous solution of the hafnium source and the aqueous solution of the reducing agent, and then transferring the mixed solution into a high-pressure reactor for heating reaction. After the reaction is completed, centrifugation is performed to remove large particles, and dialysis is performed to remove unreacted substances to obtain a hafnium dioxide quantum dot solution.

[0005] Furthermore, in step 1), the hafnium source is hafnium iodide or hafnium chloride, and the concentration of the aqueous solution of the hafnium source is 10.5-10.7 mmol / L.

[0006] Furthermore, in step 1), the pH value is adjusted by any one of 0.1 mol / L ammonia water, sodium carbonate or sodium bicarbonate.

[0007] Furthermore, in step 2), the reducing agent is any one of cysteine, sodium citrate, potassium citrate, thiourea CH4N2S, glutathione, methionine, and cystine.

[0008] Furthermore, in step 2), the concentration of the aqueous solution of the reducing agent is 0.81-0.84 mol / L.

[0009] Furthermore, in step 3), the volume ratio of the aqueous solution of the hafnium source to the aqueous solution of the reducing agent is 4:1.

[0010] Furthermore, in step 3), the reaction temperature of the high-pressure reactor is 180-220° C., and the reaction time is 18-24 h.

[0011] The synthesis method of the present invention can synthesize hafnium oxide quantum dots with stable chemical properties. Due to defect-assisted luminescence, the luminescent wavelength is in the vicinity of the ultraviolet band (UVA), providing an option for the preparation of chemically stable ultraviolet band luminescent quantum dots, which are still relatively rare, and promoting the application of hafnium-based quantum dots in the fields of luminescence, display, optical sensing detection, and biological imaging. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 Schematic diagram of the device of an embodiment of the present invention; in the figure: hafnium iodide and cysteine ​​solution are mixed and placed into a high-pressure reactor, and then placed in a heating oven for reaction; Figure 2 This is the sample morphology measured by atomic force microscopy (AFM). After drop coating, the hafnium oxide two-dimensional material quantum dots are partially agglomerated; Figure 3 This is the fluorescence spectrum of hafnium dioxide HfO2 quantum dots under 266 nm laser excitation; Figure 4 This is the absorption spectrum of hafnium dioxide HfO2 quantum dots; Figure 5 is the X-ray diffraction spectrum of hafnium dioxide HfO2 quantum dots; Figure 6 Comparison of electron spin resonance spectra of synthesized hafnium dioxide HfO2 quantum dots and purchased hafnium dioxide powder; Figure 7 Comparison of the g-factor of synthesized hafnium dioxide HfO2 quantum dots and purchased hafnium dioxide powder. DETAILED DESCRIPTION

[0013] The present invention is further described below in conjunction with the accompanying drawings in order to better understand the technical solution. Example

[0014] Dissolve 0.146 g of hafnium iodide in 20 mL of water to prepare 20 mL of 7.3 mg / mL hafnium iodide solution, and adjust the pH to 6.5 with 0.1 mol / L ammonia water. Prepare 100 mg / mL cysteine ​​aqueous solution and take 5 mL. Mix the two precursor solutions and ultrasonically treat them for 2 minutes to mix them evenly. Then transfer them to a high-pressure reactor. React at 220°C for 24 hours. After the reaction is completed, slowly cool to room temperature. Remove large particles and unreacted substances through centrifugal redispersion or dialysis to obtain a hafnium dioxide quantum dot solution. The preparation device is shown in the figure. Figure 1 shown.

[0015] The morphology of the hafnium dioxide quantum dot solution prepared in this example is as follows: Figure 2 As shown, it is a sample surface morphology image measured by atomic force microscopy (AFM). The size of the quantum dots is 60-80 nm and they are in a nearly round particle shape, indicating that the hafnium dioxide grown by the embodiment of the present invention is a quantum dot particle.

[0016] like Figure 3 As shown in the figure, it is the fluorescence spectrum obtained by exciting hafnium dioxide quantum dots with a 266 nm laser, indicating that the luminescence is located in the ultraviolet to blue wavelength band. The corresponding band gap is about 3.1 eV. The intrinsic band gap of hafnium dioxide is about 6 eV, and there is usually no fluorescence. The fluorescence in this material should be defect-assisted fluorescence.

[0017] like Figure 4 As shown, it is the absorption spectrum of hafnium dioxide quantum dots, indicating that the absorption is in the wavelength band below violet light.

[0018] like Figure 5 As shown, it is the XRD pattern of hafnium oxide. By comparing with the standard pdf card, it is proved that the synthesized particles are hafnium oxide.

[0019] like Figure 6 As shown, it is a comparison of the electron spin resonance spectra of the hafnium dioxide HfO2 quantum dots synthesized by this method and the purchased hafnium dioxide powder. The hafnium dioxide HfO2 quantum dots synthesized by this method have obvious resonance peaks, indicating the presence of defects.

[0020] like Figure 7 As shown, it is a comparison of the g-factors of the hafnium dioxide HfO2 quantum dots synthesized by the method and the purchased hafnium dioxide powder. The hafnium dioxide HfO2 quantum dots synthesized by the method of the present invention have obvious spectral peaks, which also indicates the existence of defects.

Claims

1. A method for synthesizing hafnium dioxide quantum dots, characterized in that: The synthesis method comprises the following steps: 1) Using a hafnium source as a raw material, prepare an aqueous solution of the hafnium source and adjust the pH to 6.5; 2) Prepare an aqueous solution of a reducing agent; 3) Mixing the aqueous solution of the hafnium source and the aqueous solution of the reducing agent, and then transferring the mixed solution into a high-pressure reactor for heating reaction. After the reaction is completed, centrifugation is performed to remove large particles, and dialysis is performed to remove unreacted substances to obtain a hafnium dioxide quantum dot solution.

2. The method for synthesizing hafnium dioxide quantum dots according to claim 1, wherein In step 1), the hafnium source is hafnium iodide or hafnium chloride, and the concentration of the aqueous solution of the hafnium source is 10.5-10.7 mmol / L.

3. The method for synthesizing hafnium dioxide quantum dots according to claim 1, wherein In step 1), the pH value is adjusted by using any one of 0.1 mol / L ammonia water, sodium carbonate or sodium bicarbonate.

4. The method for synthesizing hafnium dioxide quantum dots according to claim 1, wherein In step 2), the reducing agent is any one of cysteine, sodium citrate, potassium citrate, thiourea CH4N2S, glutathione, methionine, and cystine.

5. The method for synthesizing hafnium dioxide quantum dots according to claim 1, wherein In step 2), the concentration of the reducing agent in the aqueous solution is 0.81-0.84 mol / L.

6. The method for synthesizing hafnium dioxide quantum dots according to claim 1, wherein In step 3), the volume ratio of the aqueous solution of the hafnium source to the aqueous solution of the reducing agent is 4:

1.