High-nickel precursor material with multi-layer structure as well as preparation method and application of high-nickel precursor material
The preparation of multi-layer structure high-nickel precursor materials through co-precipitation method solves the problem of large demand for free lithium ion reactions and oxygen in lithium-ion batteries, improves the cycle stability and electrochemical performance of the battery, and reduces the preparation cost.
Patent Information
- Application Number
- CN202410987436.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-23
AI Technical Summary
During the preparation process of the existing lithium-ion battery ternary cathode materials, free lithium ions react with air to form alkaline substances, which affects performance, and the oxygen demand during calcination is large, resulting in mixed discharge of cations, affecting electrochemical performance, and surface modification treatment. High cost and limited effect.
The co-precipitation method is used to prepare a multi-layer structure of high-nickel precursor material in four stages. Through the first stage, the loose and porous ternary nickel-cobalt-manganese core is generated, the second stage is formed of a niobium doped layer, and the third stage is formed of a dense shell. , In the fourth stage, a metal M cladding layer was formed, combined with slurry treatment, sand grinding and spray pyrolysis, to obtain a material with uniform particle size, high spherical shape and uniform doping.
It improves the discharge capacity, rate performance and cycling performance of lithium-ion batteries, reduces the stress concentration of the material, enhances the electrochemical performance and density, avoids polarization behavior, and improves the transmission efficiency and structural stability of lithium ions.
Smart Images

Figure CN118993167A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a lithium ion battery, and in particular to a high-nickel precursor material with a multilayer structure, and a preparation method and application thereof. Background Art
[0002] At present, lithium-ion batteries, referred to as LIBs, are widely used in various devices. It is expected that the lithium-ion battery market will grow more than five times in the next ten years. In particular, the rapid popularization of medium and large power batteries and energy storage systems (ESS) for electric vehicles (EV, PHEV, HEV, etc.) will drive the growth of the lithium-ion battery market. In recent years, the new energy vehicle market has become the main driving force for the rapid development of the global lithium battery industry. In addition, electrochemical energy storage, as an important part of grid energy storage technology, plays an increasingly important role in peak shaving, new energy grid connection and power system auxiliary services.
[0003] The prior art usually adopts the hydrogen-oxygen coprecipitation method and the calcination method to prepare the ternary positive electrode material. For example, in CN113651371A, a mixed metal ion aqueous solution is pumped into a tank reactor at a controllable rate under nitrogen conditions, and an aqueous solution of alkali and ammonia water is pumped into the tank reactor at the same time, and a coprecipitation reaction occurs. After that, after washing, filtering, and drying, a hydroxide precursor is obtained, and then the hydroxide precursor and LiOH are mixed, and calcined at high temperature in a flowing oxygen atmosphere to obtain the final product. The obtained ternary positive electrode material can be subjected to surface modification treatment. By coating the surface of the ternary material with some metal compounds, lithium salts or conductive carbon materials of moderate thickness, the active material can be isolated from direct contact with the electrolyte, the occurrence of side reactions can be reduced, and the dissolution of transition metal ions can be inhibited. For example, CN110190254A discloses a method for preparing a lithium phosphate-coated lithium-ion battery ternary positive electrode material, the method comprising the following steps:
[0004] (1) dissolving a phosphoric acid source in an organic solvent to form a solution, wherein the mass fraction of the phosphoric acid source in the solution is 0.05-0.8%; (2) adding a lithium ion battery ternary positive electrode material to the solution in step (1), stirring for 5-120 minutes to make it evenly dispersed, and drying until the organic solvent is completely evaporated to obtain a lithium phosphate-coated lithium ion battery ternary positive electrode material.
[0005] However, in the preparation process of ternary cathode materials, excessive lithium salts are generally added to prevent lithium loss during sintering. Therefore, there are always free lithium ions on the surface of the material, which can easily react with H2O and CO2 in the air to generate alkaline substances LiOH and Li2CO3. The formation of residual alkali on the surface seriously hinders the performance of the ternary cathode material itself. In addition, in order to ensure that the Ni in the precursor is 2+ Can be oxidized to Ni 3+, a large amount of oxygen is required during the calcination process, otherwise Ni 2+ and Li + Due to the similar ionic radius, a large amount of cation mixing will occur, thus affecting the electrochemical performance of the positive electrode material.
[0006] Surface modification is an effective means to improve the cycle stability of ternary positive electrode materials. However, the surface coating to improve the interfacial stability of the oxidized positive electrode is limited to the surface of the active material particles, and the coating effect is greatly related to the interfacial compatibility between the coating layer and the active material. At the same time, the conditions of individual modification synthesis processes are relatively harsh and the preparation cost is relatively high.
[0007] In summary, there is a need to develop a high-nickel precursor material with a multilayer structure and a preparation method and application thereof. Summary of the invention
[0008] In view of the problems existing in the prior art, the present invention provides a high-nickel precursor material with a multilayer structure and a preparation method and application thereof. The preparation method adopts a coprecipitation method and is divided into four stages. Through the first stage of coprecipitation, nucleation is completed to generate a loose and porous ternary nickel-cobalt-manganese inner core, through the second stage of coprecipitation, a niobium-doped layer is formed, through the third stage of coprecipitation, a dense ternary nickel-cobalt-manganese outer shell is formed, and through the fourth stage of coprecipitation, a coating layer containing metal M is formed in the outermost layer, thereby obtaining a high-nickel precursor material with uniform particle size distribution, high sphericity, uniform doping, a certain gradient distribution, and a multilayer structure. The prepared positive electrode material can improve the discharge capacity, rate performance and cycle performance of lithium-ion batteries.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] One of the purposes of the present invention is to provide a method for preparing a high nickel precursor material with a multilayer structure, the preparation method comprising the following steps:
[0011] The nickel-cobalt-manganese ternary solution, the precipitant solution and the complexing agent solution are injected into the reaction bottom solution in parallel to carry out the first stage of coprecipitation;
[0012] After reaching the first target particle size, further parallel injection of the niobium salt solution is performed, and four parallel injections are maintained to perform the second stage of co-precipitation;
[0013] After reaching the second target particle size, the injection of the niobium salt solution is stopped, and the three parallel injections are maintained to carry out the third stage of co-precipitation;
[0014] After reaching the third target particle size, the coating agent solution and the dispersant solution are further injected in parallel, and five parallel injections are maintained to carry out the fourth stage of co-precipitation;
[0015] After reaching the final target particle size, solid-liquid separation, washing, drying, slurry treatment, sand milling, and spray pyrolysis are sequentially performed to obtain a high-nickel precursor material with a multilayer structure;
[0016] The coating agent in the coating agent solution is a compound containing metal M, and the metal M includes at least one of aluminum (Al), titanium (Ti), niobium (Nb), zirconium (Zr), tungsten (W), vanadium (V), strontium (Sr) or gallium (Ga).
[0017] The preparation method of the present invention adopts a co-precipitation method and is divided into four stages. Through the first stage of co-precipitation, nucleation is completed to generate a loose and porous ternary nickel-cobalt-manganese inner core. Through the second stage of co-precipitation, a niobium doping layer is formed. Through the third stage of co-precipitation, a dense ternary nickel-cobalt-manganese outer shell is formed. Through the fourth stage of co-precipitation, a coating layer containing metal M is formed in the outermost layer, thereby obtaining a high-nickel precursor material with uniform particle size distribution, high sphericity, uniform doping, a certain gradient distribution, and a multi-layer structure.
[0018] The preparation method of the present invention obtains a high-nickel precursor material with a multilayer structure, and a loose and porous structure is formed at the internal nucleation site, which is beneficial to relieve the stress concentration of the material during the electrochemical reaction and to improve the cycle performance. The surface structure of the outer shell is dense, which is beneficial to improve the tap density of the material, and the gradient distribution structure improves the electrochemical performance of the material.
[0019] The preparation method of the present invention performs niobium doping by coprecipitation in the second stage. During the reaction, niobium oxide is precipitated on the surface of the primary particles to reduce the interface resistance, avoid the occurrence of polarization behavior, and facilitate the rapid transmission of lithium ions. At the same time, the Ni-O structure formed on the surface is also conducive to the stability of the structure and improves the electrochemical cycle performance.
[0020] The preparation method of the present invention adds a surface dispersant in the fourth stage of co-precipitation. Due to the effect of steric hindrance, as the particles are enriched and aggregated, the surface charge increases, and mutual repulsion occurs, thereby promoting deagglomeration, making the particles more evenly dispersed, and preventing agglomeration when the positive electrode slurry is applied, thereby improving the capacity of the battery.
[0021] The preparation method of the present invention performs slurry treatment, sand milling, and spray pyrolysis before sintering. The sand milling treatment makes the co-precipitation doping reaction more uniform. At the same time, the spray pyrolysis method effectively reduces the particle size. The granulation forms more evenly dispersed particle balls, avoiding agglomeration. It is also beneficial to the synthesis of single crystals in the subsequent sintering process, thereby improving the performance of the positive electrode material.
[0022] As a preferred technical solution of the present invention, the molar ratio of the three elements Ni, Co and Mn in the nickel-cobalt-manganese ternary solution is x:y:(1-xy); wherein 0.8<x<1.0, 0<y<0.2.
[0023] Preferably, after the fourth stage co-precipitation and before the solid-liquid separation, the general formula of the niobium-containing precursor in the system is Ni a Co b Mn c Nb d M e (OH)2, wherein 0.6<a<0.9, 0<b<0.2, 0<c<0.1, 0<d<0.1, 0<e<0.1, a+b+c+d+e=1.
[0024] Preferably, the total concentration of metal ions in the nickel-cobalt-manganese ternary solution is 20-120 g / L, for example 20 g / L, 40 g / L, 60 g / L, 80 g / L, 100 g / L or 120 g / L, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0025] Preferably, the precipitant solution is a sodium hydroxide solution or a potassium hydroxide solution.
[0026] Preferably, the concentration of the precipitant solution is 25-35wt%, for example 25wt%, 26wt%, 28wt%, 30wt%, 31wt%, 33wt% or 35wt%, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0027] Preferably, the complexing agent solution is aqueous ammonia.
[0028] Preferably, the concentration of the complexing agent solution is 10-15wt%, such as 10wt%, 11wt%, 12wt%, 13wt%, 14wt% or 15wt%, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0029] Preferably, the reaction base liquid is prepared from pure water, sodium hydroxide solution and ammonia water, specifically comprising: adding pure water, sodium hydroxide solution and ammonia water as the reaction base liquid in a reaction device, starting stirring, heating the reaction base liquid to 40-60° C., adjusting the pH value of the reaction base liquid to 10.0-12.0, the ammonia concentration to 4-6 g / L, introducing N2, and controlling the introduction rate of N2 to 0.2-2 m 3 / h.
[0030] Preferably, in the first stage co-precipitation, the injection flow rate of the complexing agent solution is 500-700 mL / h, for example, 500 mL / h, 550 mL / h, 600 mL / h, 650 mL / h or 700 mL / h, the injection flow rate of the precipitant solution is 1.6-2.0 L / h, for example, 1.6 L / h, 1.7 L / h, 1.8 L / h, 1.9 L / h or 2.0 L / h, and the injection flow rate of the nickel-cobalt-manganese ternary solution is 4-8 L / h, for example, 4 L / h, 5 L / h, 6 L / h, 7 L / h or 8 L / h, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0031] Preferably, the pH value of the first stage co-precipitation is 11.0-12.0, such as 11.0, 11.1, 11.3, 11.5, 11.6, 11.8 or 12.0, but is not limited to the listed values, and other values not listed within the above range are also applicable.
[0032] Preferably, the ammonia concentration of the first stage co-precipitation is 3-5 g / L, for example 3 g / L, 3.5 g / L, 4 g / L, 4.5 g / L or 5 g / L, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0033] Preferably, the first target particle size is 1.5-2 μm, such as 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm or 2 μm, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0034] As a preferred technical solution of the present invention, the niobium salt in the niobium salt solution includes at least one of niobium oxalate, niobium sulfate, niobium nitrate, niobium tetrachloride, niobium pentachloride, niobium tetrafluoride, niobium pentafluoride, niobium pentoxide or niobium oxyphosphate, preferably niobium nitrate.
[0035] Preferably, the concentration of niobium salt in the niobium salt-containing solution is 10-200 g / L, for example, 10 g / L, 30 g / L, 50 g / L, 80 g / L, 100 g / L, 130 g / L, 150 g / L, 170 g / L or 200 g / L, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0036] Preferably, in the second stage of co-precipitation, the doping amount of niobium is controlled to be 0.05-5% of the total mass of the ternary nickel, cobalt and manganese elements, such as 0.05%, 0.1%, 0.5%, 1%, 2%, 3%, 4% or 5%, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0037] It should be noted that the doping amount of niobium in the present invention is controlled according to 0.05-5% of the total mass of the ternary nickel, cobalt and manganese elements after the entire high-nickel precursor material is prepared.
[0038] As a preferred technical solution of the present invention, in the second stage co-precipitation, the injection flow rate of the complexing agent solution is 600-800 mL / h, such as 600 mL / h, 650 mL / h, 700 mL / h, 750 mL / h or 800 mL / h, and the injection flow rate of the precipitant solution is 2.2-3.0 L / h, such as 2.2 L / h, 2.4 L / h, 2.5 L / h, 2.6 L / h, 2.8 L / h or 3.0 L / h etc., the injection flow rate of the nickel-cobalt-manganese ternary solution is 8-10 L / h, such as 8 L / h, 8.5 L / h, 9 L / h, 9.5 L / h or 10 L / h, etc., the injection flow rate of the niobium salt solution is 100-500 mL / h, such as 100 mL / h, 200 mL / h, 300 mL / h, 400 mL / h or 500 mL / h, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0039] Preferably, the pH value of the second stage co-precipitation is 9.5-10.5, such as 9.5, 9.7, 9.8, 10.0, 10.1, 10.3 or 10.5, but is not limited to the listed values, and other values not listed within the above range are also applicable.
[0040] Preferably, the ammonia concentration of the second stage co-precipitation is 4-6 g / L, for example 4 g / L, 4.5 g / L, 5 g / L, 5.5 g / L or 6 g / L, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0041] Preferably, the second target particle size is 3-3.5 μm, such as 3 μm, 3.1 μm, 3.2 μm, 3.3 μm, 3.4 μm or 3.5 μm, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0042] As a preferred technical solution of the present invention, in the third stage co-precipitation, the injection flow rate of the complexing agent solution is 800-900mL / h, such as 800mL / h, 820mL / h, 830mL / h, 850mL / h, 870mL / h or 900mL / h, the injection flow rate of the precipitant solution is 3.0-4.0L / h, such as 3.0L / h, 3.1L / h, 3.3L / h, 3.5L / h, 3.6L / h, 3.8L / h or 4.0L / h, and the injection flow rate of the nickel-cobalt-manganese ternary solution is 10-15L / h, such as 10L / h, 11L / h, 12L / h, 13L / h, 14L / h or 15L / h, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0043] Preferably, the pH value of the third stage co-precipitation is 10.2-11.0, such as 10.2, 10.4, 10.6, 10.8 or 11.0, but is not limited to the listed values, and other values not listed within the above range are also applicable.
[0044] Preferably, the ammonia concentration of the third stage co-precipitation is 6-8 g / L, for example 6 g / L, 6.5 g / L, 7 g / L, 7.5 g / L or 8 g / L, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0045] Preferably, the third target particle size is 4-4.5 μm, such as 4 μm, 4.1 μm, 4.2 μm, 4.3 μm, 4.4 μm or 4.5 μm, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0046] As a preferred technical solution of the present invention, the concentration of the coating agent solution is 10-50g / L, for example, 10g / L, 20g / L, 30g / L, 40g / L or 50g / L, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0047] Preferably, the dispersant in the dispersant solution is at least one of tetramethylammonium hydroxide, diethylene glycol, polyvinyl pyrrolidone (PVP), sodium polyacrylate, triethanolamine, alkyl glycoside, maleic acid-acrylic acid copolymer (MA-AA), polyethylene glycol or polypropylene alcohol, preferably tetramethylammonium hydroxide.
[0048] It should be noted that the degree of polymerization of the polyvinyl pyrrolidone of the present invention is n=250-300, the degree of polymerization of sodium polyacrylate is n=3000-5000, the degree of polymerization of maleic acid-acrylic acid copolymer is n=20-30, the degree of polymerization of alkyl glycoside is n=1.4-1.6, the degree of polymerization of polyethylene glycol is n=1000-2000, and the degree of polymerization of polypropylene alcohol is n=1000-2000.
[0049] Preferably, the dispersant concentration in the dispersant solution is 20-100 g / L, for example 20 g / L, 40 g / L, 60 g / L, 80 g / L or 100 g / L, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0050] As a preferred technical solution of the present invention, in the fourth stage co-precipitation, the injection flow rate of the complexing agent solution is 900-1000mL / h, such as 900mL / h, 910mL / h, 930mL / h, 950mL / h, 970mL / h, 990mL / h or 1000mL / h, etc., the injection flow rate of the precipitant solution is 4.0-4.5L / h, such as 4.0L / h, 4.1L / h, 4.2L / h, 4.3L / h, 4.4L / h or 4.5L / h, etc., and the injection flow rate of the nickel-cobalt-manganese ternary solution is 10-15L / h, such as 1 0L / h, 11L / h, 12L / h, 13L / h, 14L / h or 15L / h, etc., the injection flow rate of the coating agent solution is 200-400mL / h, such as 200mL / h, 250mL / h, 300mL / h, 350mL / h or 400mL / h, etc., the injection flow rate of the dispersant solution is 200-400mL / h, such as 200mL / h, 250mL / h, 300mL / h, 350mL / h or 400mL / h, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are equally applicable.
[0051] Preferably, the pH value of the fourth stage co-precipitation is 10.2-11.0, such as 10.2, 10.4, 10.6, 10.8 or 11.0, but is not limited to the listed values, and other values not listed within the above range are also applicable.
[0052] Preferably, the ammonia concentration of the fourth stage co-precipitation is 6-8 g / L, for example 6 g / L, 6.5 g / L, 7 g / L, 7.5 g / L or 8 g / L, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0053] Preferably, the fourth target particle size is 4.5-5 μm, such as 4.5 μm, 4.6 μm, 4.7 μm, 4.8 μm, 4.9 μm or 5 μm, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0054] As a preferred technical solution of the present invention, the reaction temperatures of the first stage co-precipitation, the second stage co-precipitation, the third stage co-precipitation and the fourth stage co-precipitation are the same, which are 40-60°C, for example, 40°C, 45°C, 50°C, 55°C or 60°C, etc., but are not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0055] Preferably, the stirring speeds of the first stage co-precipitation, the second stage co-precipitation, the third stage co-precipitation and the fourth stage co-precipitation are the same, which are all 250-380r / min, for example, 250r / min, 280r / min, 300r / min, 310r / min, 330r / min, 350r / min or 380r / min, etc., but are not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0056] Preferably, the washing comprises: washing at least three times with sodium hydroxide solution and hot water respectively.
[0057] Preferably, the drying temperature is 100-150°C, such as 100°C, 110°C, 120°C, 130°C, 140°C or 150°C, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0058] Preferably, the slurrying treatment obtains a slurry with a solid content of 20-40wt%, for example 20wt%, 25wt%, 30wt%, 35wt% or 40wt%, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0059] Preferably, the sand grinding includes: using zirconium balls with a diameter of 0.1-1 mm, such as 0.1 mm, 0.3 mm, 0.5 mm, 0.6 mm, 0.8 mm or 1 mm, etc., and sand grinding for 2-10 hours, such as 2 hours, 4 hours, 6 hours, 8 hours or 10 hours, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0060] Preferably, the inlet temperature of the spray pyrolysis is 200-300°C, for example, 200°C, 210°C, 230°C, 250°C, 260°C, 280°C or 300°C, and the outlet temperature is 80-150°C, for example, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0061] The second object of the present invention is to provide a high-nickel precursor material with a multilayer structure, which is prepared by the preparation method described in the first object.
[0062] The third object of the present invention is to provide an application of a high-nickel precursor material with a multilayer structure, wherein the high-nickel precursor material with a multilayer structure is mixed with a lithium source and sintered to obtain a high-nickel positive electrode material;
[0063] Among them, the high-nickel precursor material with a multi-layer structure is prepared by the preparation method described in purpose one, or the high-nickel precursor material with a multi-layer structure is the high-nickel precursor material with a multi-layer structure described in purpose two.
[0064] Preferably, the ratio of the total molar amount of nickel, cobalt and manganese in the high-nickel precursor material with a multilayer structure to the molar amount of lithium element in the lithium source is 1:(1-1.1), for example 1:1, 1:1.01, 1:1.03, 1:1.05, 1:1.07 or 1:1, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0065] Preferably, the sintering includes a first sintering and a second sintering performed sequentially.
[0066] Preferably, the heating rate of the first sintering is 2-6°C / min, for example, 2°C / min, 3°C / min, 4°C / min, 5°C / min or 6°C / min, etc., the target temperature is 400-700°C, for example, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C or 700°C, etc., and the holding time is 3-6h, for example, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0067] Preferably, the heating rate of the second sintering is 2-6°C / min, for example, 2°C / min, 3°C / min, 4°C / min, 5°C / min or 6°C / min, etc., the target temperature is 700-1000°C, for example, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C or 1000°C, etc., and the holding time is 10-20h, for example, 10h, 12h, 14h, 16h, 18h or 20h, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0068] Compared with the prior art solutions, the present invention has at least the following beneficial effects:
[0069] (1) The preparation method of the present invention adopts a coprecipitation method and is divided into four stages. In the first stage of coprecipitation, nucleation is completed to generate a loose and porous ternary nickel-cobalt-manganese core. In the second stage of coprecipitation, a niobium doping layer is formed. In the third stage of coprecipitation, a dense ternary nickel-cobalt-manganese shell is formed. In the fourth stage of coprecipitation, a coating layer containing metal M is formed in the outermost layer, thereby obtaining a high-nickel precursor material with uniform particle size distribution, high sphericity, uniform doping, a certain gradient distribution, and a multilayer structure;
[0070] (2) The preparation method of the present invention obtains a high-nickel precursor material with a multilayer structure, and a loose and porous structure is formed at the internal nucleation site, which is beneficial to relieve the stress concentration of the material during the electrochemical reaction and improve the cycle performance. The surface structure of the outer shell is dense, which is beneficial to improve the tap density of the material, and the gradient distribution structure improves the electrochemical performance of the material.
[0071] (3) The preparation method of the present invention performs niobium doping by coprecipitation in the second stage. During the reaction, niobium oxide is precipitated on the surface of the primary particles to reduce the interface resistance, avoid the occurrence of polarization behavior, and facilitate the rapid transmission of lithium ions. At the same time, the Ni-O structure formed on the surface is also conducive to the stability of the structure and improves the electrochemical cycle performance.
[0072] (4) In the preparation method of the present invention, a surface dispersant is added in the fourth stage of coprecipitation. Due to the steric hindrance, the surface dispersant aggregates with the enrichment of particles and increases the surface charge, which repel each other and promotes deagglomeration, making the particles more evenly dispersed. When the positive electrode slurry is applied, the particles will not clump, thereby improving the capacity of the battery;
[0073] (5) The preparation method of the present invention performs slurry treatment, sand milling, and spray pyrolysis before sintering. The sand milling treatment makes the co-precipitation doping reaction more uniform. At the same time, the spray pyrolysis method effectively reduces the particle size. The granulation forms more evenly dispersed particle balls, avoiding agglomeration. It is also beneficial to the synthesis of single crystals in the subsequent sintering process, thereby improving the performance of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0074] Figure 1 is an EDS graph of the niobium-containing precursor hydroxide obtained by drying in Example 1 for the Nb element;
[0075] Figure 2 is a SEM image of the niobium-containing precursor hydroxide obtained by drying in Example 1;
[0076] Figure 3 is a cross-sectional SEM image of the niobium-containing precursor hydroxide obtained by drying in Example 1;
[0077] Figure 4 3 is a SEM image of the niobium-containing precursor oxide obtained by spray pyrolysis in Example 1. DETAILED DESCRIPTION
[0078] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0079] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0080] Example 1
[0081] This embodiment provides a method for preparing a high-nickel precursor material with a multilayer structure, the preparation method comprising the following steps:
[0082] A nickel-cobalt-manganese ternary solution, a precipitant solution, a complexing agent solution, a niobium salt solution, a coating agent solution, and a dispersant solution are prepared; the molar ratio of the three elements Ni, Co, and Mn in the nickel-cobalt-manganese ternary solution is 0.83:0.12:0.05, and the total concentration of metal ions in the nickel-cobalt-manganese ternary solution is 80 g / L; the precipitant solution is a NaOH solution with a mass concentration of 30 wt%; the complexing agent solution is an ammonia solution with a mass concentration of 12 wt%; the niobium salt solution is a niobium nitrate solution with a concentration of 50 g / L; the coating agent solution is an aluminum sulfate solution with a concentration of 20 g / L; and the dispersant solution is a tetramethylammonium hydroxide solution with a concentration of 50 g / L;
[0083] To 10m 3 Add 6.7m 3 Pure water, a certain amount of NaOH solution and ammonia water were used as the reaction base liquid, and 1m 3 / h rate of nitrogen into the reaction bottom liquid, stirring at a speed of 100r / min to make it evenly mixed, then heating to 55°C, adjusting the pH value of the reaction bottom liquid to 11.5-11.8, the ammonia concentration to 5g / L, and controlling the total alkalinity to 18g / L;
[0084] The nickel-cobalt-manganese ternary solution, the precipitant solution and the complexing agent solution are injected into the reaction bottom liquid in parallel, the injection flow rate of the complexing agent solution is 600 mL / h, the injection flow rate of the precipitant solution is 2.0 L / h, and the injection flow rate of the nickel-cobalt-manganese ternary solution is 6 L / h, and the first stage of coprecipitation is carried out, and the pH value of the first stage of coprecipitation is controlled to be 11.5, the ammonia concentration is 4 g / L, and the first stage of coprecipitation is completed after the first target particle size of 2 μm is reached, and nucleation is completed;
[0085] Further parallel injection of niobium salt solution, the injection flow rate of the complexing agent solution is 800 mL / h, the injection flow rate of the precipitant solution is 2.5 L / h, the injection flow rate of the nickel-cobalt-manganese ternary solution is 8 L / h, the injection flow rate of the niobium salt solution is 300 mL / h, the addition amount of niobium nitrate is controlled so that the doping amount of niobium is 2% of the total mass of the ternary nickel-cobalt-manganese elements, the four parallel injections are maintained for the second stage of co-precipitation, the pH value of the second stage of co-precipitation is controlled to be 10.0, the ammonia concentration is controlled to be 6 g / L, and the second stage of co-precipitation is terminated after the second target particle size of 3.5 μm is reached;
[0086] Stop the injection of the niobium salt solution, the injection flow rate of the complexing agent solution is 800 mL / h, the injection flow rate of the precipitant solution is 4.0 L / h, and the injection flow rate of the nickel-cobalt-manganese ternary solution is 12 L / h, and the three parallel flows are maintained for the third stage of co-precipitation. The pH value of the third stage of co-precipitation is controlled to be 10.5, the ammonia concentration is 8 g / L, and the third stage of co-precipitation ends after the third target particle size of 4 μm is reached;
[0087] Further parallel injection of coating agent solution and dispersant solution, the injection flow rate of complexing agent solution is 1000mL / h, the injection flow rate of precipitant solution is 4.0L / h, the injection flow rate of nickel-cobalt-manganese ternary solution is 15L / h, the injection flow rate of coating agent solution is 300mL / h, the injection flow rate of dispersant solution is 300mL / h, and the five parallel injections are maintained for the fourth stage of co-precipitation, the pH value of the fourth stage of co-precipitation is controlled to be 10.5, the ammonia concentration is 8g / L, the ammonia concentration and pH value in the reaction system are maintained constant, and when the particle D50 of the reaction product reaches the final target particle size of 4.5μm, the feeding is stopped;
[0088] The product is sequentially subjected to solid-liquid separation, washing and drying, wherein the washing comprises four times of alkaline washing with sodium hydroxide solution and five times of water washing with hot water, and the drying comprises drying at 90°C. The obtained precursor powder is transferred to a slurrying kettle for slurrying treatment to obtain a slurry with a solid content of 20wt%, and is sand-milled for 8 hours using a zirconium ball with a diameter of 0.5mm. The obtained slurry is pumped into a spray dryer for spray pyrolysis, and the inlet temperature is controlled at 250°C and the outlet temperature is controlled at 100°C to obtain a high-nickel precursor material with a multilayer structure.
[0089] For the niobium-containing precursor hydroxide obtained by drying in this embodiment, Figure 1 The EDS image for the Nb element is shown. It can be seen that the Nb element is uniformly doped inside the particles and forms a ring with a certain thickness; Figure 2 and Figure 3 The SEM image and the cross-sectional SEM image are shown respectively. It can be seen that a loose and porous structure is formed at the nucleation site inside the particle, which is beneficial to alleviate the stress concentration of the material during the electrochemical reaction and to improve the cycle performance. The external surface structure is dense and the gradient distribution structure improves the electrochemical performance of the material.
[0090] Figure 4 3 is a SEM image of the niobium-containing precursor oxide obtained by spray pyrolysis in this embodiment. It can be seen from the image that the spray pyrolysis method effectively reduces the particle size and avoids agglomeration. It is also beneficial to the synthesis of single crystals in the subsequent sintering process, thereby improving the performance of the positive electrode material.
[0091] Example 2
[0092] This embodiment provides a method for preparing a high-nickel precursor material with a multilayer structure. Compared with Embodiment 1, the only difference is that in the second stage of co-precipitation, the doping amount of niobium is controlled to be 0.1% of the total mass of the ternary nickel, cobalt and manganese elements.
[0093] Example 3
[0094] This embodiment provides a method for preparing a high-nickel precursor material with a multilayer structure. Compared with Embodiment 1, the only difference is that in the second stage of co-precipitation, the doping amount of niobium is controlled to be 0.2% of the total mass of the ternary nickel, cobalt and manganese elements.
[0095] Example 4
[0096] This embodiment provides a method for preparing a high-nickel precursor material with a multilayer structure. Compared with Embodiment 1, the only difference is that in the second stage of co-precipitation, the doping amount of niobium is controlled to be 0.5% of the total mass of the ternary nickel, cobalt and manganese elements.
[0097] Example 5
[0098] This embodiment provides a method for preparing a high-nickel precursor material with a multilayer structure. Compared with Embodiment 1, the only difference is that in the second stage of co-precipitation, the doping amount of niobium is controlled to be 1% of the total mass of the ternary nickel, cobalt and manganese elements.
[0099] Example 6
[0100] This embodiment provides a method for preparing a high-nickel precursor material with a multilayer structure. Compared with Embodiment 1, the only difference is that in the second stage of co-precipitation, the doping amount of niobium is controlled to be 5% of the total mass of the ternary nickel, cobalt and manganese elements.
[0101] Example 7
[0102] This embodiment provides a method for preparing a high-nickel precursor material with a multilayer structure. Compared with Embodiment 1, the only difference is that in the second stage of co-precipitation, the doping amount of niobium is controlled to be 8% of the total mass of the ternary nickel, cobalt and manganese elements.
[0103] Example 8
[0104] This embodiment provides a method for preparing a high-nickel precursor material with a multilayer structure. Compared with Embodiment 1, the only difference is that in the second stage of co-precipitation, the doping amount of niobium is controlled to be 10% of the total mass of the ternary nickel, cobalt and manganese elements.
[0105] Comparative Example 1
[0106] This comparative example provides a method for preparing a high-nickel precursor material with a multilayer structure. Compared with Example 1, the only difference is that in the fourth stage of co-precipitation, no dispersant solution is added.
[0107] Comparative Example 2
[0108] This comparative example provides a method for preparing a high-nickel precursor material with a multilayer structure. Compared with Example 1, the only difference is that no niobium salt solution is injected into the second stage of co-precipitation, that is, no niobium doping is performed.
[0109] Comparative Example 3
[0110] This comparative example provides a method for preparing a high-nickel precursor material with a multilayer structure. Compared with Example 1, the only difference is that slurry treatment, sand milling, and spray pyrolysis are completely omitted, and the obtained niobium-containing precursor hydroxide is directly used as the high-nickel precursor material with a multilayer structure.
[0111] Comparative Example 4
[0112] This comparative example provides a method for preparing a high-nickel precursor material with a multilayer structure. Compared with Example 1, the only difference is that sand milling is completely omitted, that is, the slurry obtained by slurry treatment is directly subjected to spray pyrolysis.
[0113] The high-nickel precursor material with a multilayer structure prepared in the above embodiments and comparative examples and lithium hydroxide are put into a high-speed mixer for batch mixing, and the ratio of the total molar amount of nickel, cobalt and manganese to the molar amount of lithium hydroxide in the high-nickel precursor material with a multilayer structure is controlled to be 1:1.05. The obtained mixture is put into a box furnace for sequentially performing a first sintering and a second sintering, wherein the heating rate of the first sintering is 4°C / min, the target temperature is 450°C, and the holding time is 5h, and the heating rate of the second sintering is 4°C / min, the target temperature is 850°C, and the holding time is 20h. The sintered material is cooled, crushed and sieved to obtain a high-nickel positive electrode material; the high-nickel positive electrode material and the conductive The electrolyte and binder PVP were mixed in a mass ratio of 8:1:1, and added to nitrogen methyl pyrrolidone (NMP) to prepare a positive electrode slurry. The positive electrode slurry was scraped onto an aluminum foil, and the coated electrode was placed in a vacuum oven at 120°C for drying, and then cut into discs with a diameter of 12 mm as the positive electrode, a metal lithium sheet as the negative electrode, and a diaphragm to separate the positive and negative electrodes. The solute of the electrolyte was a ternary commercial electrolyte 1MLiPF6, and the solvent was a mixture of ethylene carbonate, dimethyl carbonate and diethyl carbonate in a volume ratio of 1:1:1. The negative electrode shell, negative electrode, electrolyte, diaphragm, electrolyte, positive electrode, current collector and positive electrode shell were stacked and pressed in sequence to assemble into a button lithium-ion battery.
[0114] The prepared button lithium-ion battery was subjected to electrochemical performance testing at a test voltage of 3.0 to 4.3 V. The first discharge specific capacity and first coulombic efficiency were measured at 0.1 C. The capacity retention rate of the battery after 100 charge and discharge cycles was tested at 1 C. The test results are shown in Table 1.
[0115] Table 1
[0116] project First discharge specific capacity (mAh / g) First coulombic efficiency (%) Capacity retention rate (%) Example 1 203.2 93.7 91.4 Example 2 197.5 91.4 87.8 Example 3 202.6 92.8 89.7 Example 4 202.1 91.9 91.0 Example 5 199.3 91.4 89.9 Example 6 202.1 92.7 91.1 Example 7 198.9 91.7 90.9 Example 8 200.2 91.5 90.3 Comparative Example 1 195.2 90.1 88.7 Comparative Example 2 189.7 88.3 83.9 Comparative Example 3 192.4 89.2 85.8 Comparative Example 4 193.6 89.8 86.2
[0117] It can be seen from Table 1 that the first discharge capacity and capacity retention rate in Example 1 are the highest, indicating that the best electrochemical performance can be obtained when the mass percentage of niobium nitrate doping is controlled to be about 2%; at the same time, by comparing the data of Example 1 and Comparative Example 1, it can be seen that the use of adding a dispersant can make the particles more evenly dispersed and improve the capacity of the battery.
[0118] In summary, the preparation method of the present invention adopts a co-precipitation method and is divided into four stages. Through the first stage of co-precipitation, nucleation is completed to generate a loose and porous ternary nickel-cobalt-manganese inner core. Through the second stage of co-precipitation, a niobium-doped layer is formed. Through the third stage of co-precipitation, a dense ternary nickel-cobalt-manganese outer shell is formed. Through the fourth stage of co-precipitation, a coating layer containing metal M is formed in the outermost layer, thereby obtaining a high-nickel precursor material with uniform particle size distribution, high sphericity, uniform doping, a certain gradient distribution, and a multi-layer structure. The prepared positive electrode material can improve the discharge capacity, rate performance, and cycle performance of lithium-ion batteries.
[0119] The present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0120] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0121] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0122] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing a high-nickel precursor material with a multilayer structure, characterized in that: The preparation method comprises the following steps: The nickel-cobalt-manganese ternary solution, the precipitant solution and the complexing agent solution are injected into the reaction bottom solution in parallel to carry out the first stage of coprecipitation; After reaching the first target particle size, further parallel injection of the niobium salt solution is performed, and four parallel injections are maintained to perform the second stage of co-precipitation; After reaching the second target particle size, the injection of the niobium salt solution is stopped, and the three parallel injections are maintained to carry out the third stage of co-precipitation; After reaching the third target particle size, the coating agent solution and the dispersant solution are further injected in parallel, and five parallel injections are maintained to carry out the fourth stage of co-precipitation; After reaching the final target particle size, solid-liquid separation, washing, drying, slurry treatment, sand milling, and spray pyrolysis are sequentially performed to obtain a high-nickel precursor material with a multilayer structure; The coating agent in the coating agent solution is a compound containing a metal M, and the metal M includes at least one of aluminum, titanium, niobium, zirconium, tungsten, vanadium, strontium or gallium.
2. The preparation method according to claim 1, characterized in that: The molar ratio of the three elements Ni, Co and Mn in the nickel-cobalt-manganese ternary solution is x:y:(1-xy); wherein 0.8<x<1.0, 0<y<0.2; Preferably, after the fourth stage co-precipitation and before the solid-liquid separation, the general formula of the niobium-containing precursor in the system is Ni a Co b Mn c Nb d M e (OH)2, wherein 0.6<a<0.9, 0<b<0.2, 0<c<0.1, 0<d<0.1, 0<e<0.1, a+b+c+d+e=1; Preferably, the total concentration of metal ions in the nickel-cobalt-manganese ternary solution is 20-120 g / L; Preferably, in the first stage of co-precipitation, the injection flow rate of the complexing agent solution is 500-700 mL / h, the injection flow rate of the precipitant solution is 1.6-2.0 L / h, and the injection flow rate of the nickel-cobalt-manganese ternary solution is 4-8 L / h; Preferably, the pH value of the first stage coprecipitation is 11.0-12.0; Preferably, the ammonia concentration of the first stage co-precipitation is 3-5 g / L; Preferably, the first target particle size is 1.5-2 μm.
3. The preparation method according to claim 1 or 2, characterized in that: The niobium salt in the niobium salt solution includes at least one of niobium oxalate, niobium sulfate, niobium nitrate, niobium tetrachloride, niobium pentachloride, niobium tetrafluoride, niobium pentafluoride, niobium pentoxide or niobium oxyphosphate; Preferably, the concentration of niobium salt in the niobium salt-containing solution is 10-200 g / L; Preferably, in the second stage of co-precipitation, the doping amount of niobium is controlled to be 0.05-5% of the total mass of the ternary nickel, cobalt and manganese elements.
4. The preparation method according to any one of claims 1 to 3, characterized in that: In the second stage of co-precipitation, the injection flow rate of the complexing agent solution is 600-800 mL / h, the injection flow rate of the precipitant solution is 2.2-3.0 L / h, the injection flow rate of the nickel-cobalt-manganese ternary solution is 8-10 L / h, and the injection flow rate of the niobium salt solution is 100-500 mL / h; Preferably, the pH value of the second stage co-precipitation is 9.5-10.5; Preferably, the ammonia concentration of the second stage co-precipitation is 4-6 g / L; Preferably, the second target particle size is 3-3.5 μm.
5. The preparation method according to any one of claims 1 to 4, characterized in that: In the third stage of co-precipitation, the injection flow rate of the complexing agent solution is 800-900 mL / h, the injection flow rate of the precipitant solution is 3.0-4.0 L / h, and the injection flow rate of the nickel-cobalt-manganese ternary solution is 10-15 L / h; Preferably, the pH value of the third stage co-precipitation is 10.2-11.0; Preferably, the ammonia concentration of the third stage co-precipitation is 6-8 g / L; Preferably, the third target particle size is 4-4.5 μm.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The concentration of the coating agent solution is 10-50 g / L; Preferably, the dispersant in the dispersant solution is at least one of tetramethylammonium hydroxide, diethylene glycol, polyvinyl pyrrolidone, sodium polyacrylate, triethanolamine, alkyl glycoside, maleic acid-acrylic acid copolymer, polyethylene glycol or polypropylene alcohol; Preferably, the dispersant concentration in the dispersant solution is 20-100 g / L.
7. The preparation method according to any one of claims 1 to 6, characterized in that: In the fourth stage of co-precipitation, the injection flow rate of the complexing agent solution is 900-1000 mL / h, the injection flow rate of the precipitating agent solution is 4.0-4.5 L / h, the injection flow rate of the nickel-cobalt-manganese ternary solution is 10-15 L / h, the injection flow rate of the coating agent solution is 200-400 mL / h, and the injection flow rate of the dispersant solution is 200-400 mL / h; Preferably, the pH value of the fourth stage co-precipitation is 10.2-11.0; Preferably, the ammonia concentration of the fourth stage co-precipitation is 6-8 g / L; Preferably, the fourth target particle size is 4.5-5 μm.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The reaction temperatures of the first stage co-precipitation, the second stage co-precipitation, the third stage co-precipitation and the fourth stage co-precipitation are the same, which are 40-60° C.; Preferably, the slurry treatment obtains a slurry having a solid content of 20-40 wt%; Preferably, the sand grinding comprises: using a zirconium ball with a diameter of 0.1-1 mm, sand grinding for 2-10 hours; Preferably, the inlet temperature of the spray pyrolysis is 200-300°C, and the outlet temperature is 80-150°C.
9. A high nickel precursor material with a multilayer structure, characterized in that: The preparation method is described in any one of claims 1 to 8.
10. An application of a high nickel precursor material with a multilayer structure, characterized in that: A high-nickel precursor material having a multilayer structure is mixed with a lithium source and sintered to obtain a high-nickel positive electrode material; Wherein, the high-nickel precursor material with a multi-layer structure is prepared by the preparation method described in any one of claims 1 to 8, or the high-nickel precursor material with a multi-layer structure is the high-nickel precursor material with a multi-layer structure described in claim 9.
Citation Information
Patent Citations
Preparation method of lithium phosphate coated lithium-ion battery ternary positive electrode material
CN110190254A
High-nickel ternary precursor material, preparation method thereof and high-nickel ternary anode material
CN113651371A
Doped positive electrode material precursor and preparation method and application thereof, doped positive electrode material and preparation method and application thereof
CN112794370A
Quaternary-doped ternary positive electrode material precursor, preparation method thereof and positive electrode material
CN113571696A
Multi-layer aluminum-doped nickel-cobalt-manganese precursor and preparation method thereof
CN113603159A
Cited By
Preparation method for preventing ternary battery positive electrode precursor from agglomeration
CN121005424A
Three-section type core-shell structure ternary precursor, positive electrode material, preparation method and positive electrode
CN121269833A