Polypropylene composite material as well as preparation method and application thereof

Through the blending and filling modification methods of polypropylene resin, maleic anhydride grafted polypropylene, polyolefin elastomer and chopped glass fiber, the low density, low shrinkage and high impact resistance of polypropylene materials are solved. , achieving both low density, high impact resistance and good mechanical properties of polypropylene materials.

CN118994779APending Publication Date: 2024-11-22CHINA ENERGY GRP NINGXIA COAL IND CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411131041.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing polypropylene materials cannot take into account the problems of low density, low shrinkage and high impact resistance. The addition of high inorganic fillers in traditional methods leads to increased density, decreased mechanical properties and reduced gloss.

Method used

By using the blending and filling modification method of polypropylene resin, maleic anhydride grafted polypropylene, polyolefin elastomer and chopped glass fiber, the molding shrinkage rate of polypropylene is reduced and the Impact resistance.

Benefits of technology

On the basis of maintaining low density, the forming shrinkage and impact resistance of polypropylene materials are significantly improved, and its mechanical properties are improved while avoiding the reduction of density and gloss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004997816670000061
    Figure BDA0004997816670000061
  • Figure BDA0004997816670000071
    Figure BDA0004997816670000071
  • Figure BDA0004997816670000081
    Figure BDA0004997816670000081
Patent Text Reader

Abstract

The invention provides a polypropylene composite material as well as a preparation method and application thereof. The polypropylene composite material comprises the following raw materials: polypropylene resin, maleic anhydride grafted polypropylene, a polyolefin elastomer, chopped glass fibers and an inorganic filler. Wherein the weight ratio of the polypropylene resin to the polyolefin elastomer is (70-85): (10-15); and the inorganic filler accounts for less than or equal to 8% of the polypropylene composite material by weight. By adopting a method of combining blending modification and filling modification, the molding shrinkage rate of the polypropylene material can be reduced on the basis of not greatly increasing the density of the polypropylene material, and meanwhile, the mechanical properties such as impact resistance and the like of the polypropylene material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plastic processing, and in particular to a polypropylene composite material, a preparation method and application thereof. Background Art

[0002] Polypropylene (PP) is a common thermoplastic material with abundant raw material sources, low price, easy processing and molding, and excellent product comprehensive performance. It is widely used in the fields of automobiles, home appliances, construction, medical treatment and packaging. However, PP also has some shortcomings. The biggest disadvantage is poor cold resistance and easy brittle fracture at low temperature; followed by large shrinkage, poor creep resistance, poor product dimensional stability, and easy warping deformation. Compared with traditional engineering plastics, PP also has defects such as poor weather resistance, poor light resistance, heat resistance and aging resistance. The performance of PP is not only related to the chemical structure, but also depends to a large extent on the aggregate structure produced by the raw materials during the preparation process. For crystalline PP, crystallization is one of the main reasons for the shrinkage of PP products. During the molding process, PP products will undergo flow-induced crystallization. After crystallization, the polymer molecular chains are closely arranged and the structure is orderly and regular. The macroscopic performance is the reduction of product size. After demolding, the product will continue to crystallize due to the existence of residual stress and temperature changes, thus further shrinking; at the same time, orientation is also an important reason for PP shrinkage.

[0003] The existing technology uses different methods to reduce the molding shrinkage of PP and improve its mechanical properties, mainly chemical modification, blending modification, filling modification and other methods. Among them, physical blending and filling modification are widely favored by researchers due to their advantages of low cost, simple operation, and the ability to obtain PP compounds with specific optimized performance. With the expansion of PP application fields, the requirements for PP performance are gradually increasing. At present, it is generally required to reduce PP molding shrinkage, improve dimensional stability and improve its mechanical properties at the same time.

[0004] Chinese patent CN115181361A discloses a low shrinkage polypropylene material and a preparation method thereof, wherein glass fiber, calcium carbonate, talcum powder, compatibilizer, toughening agent, coupling agent, heat stabilizer, and lubricant are added to improve the molding shrinkage of polypropylene. Chinese patent CN113321873B discloses a low shrinkage high toughness modified polypropylene material and a preparation method thereof, wherein inorganic salt whiskers, inorganic fillers, toughening agents, high-density polyethylene, nucleating agents, lubricants, and antioxidants are used to prepare low shrinkage high toughness polypropylene materials. Chinese patent CN115873338A discloses a low shrinkage polypropylene composite material and a preparation method thereof, wherein SiO2 is coated with expanded perlite, coupling agents, heat stabilizers, and lubricants to prepare low shrinkage polypropylene materials.

[0005] However, the above-mentioned prior art generally adopts adding a large amount of low-shrinkage inorganic mineral materials to reduce the shrinkage of polypropylene, and the amount of inorganic mineral materials added usually needs to reach 40-50%. Although these methods improve the shrinkage of polypropylene to a certain extent, such a high amount of inorganic material added will greatly increase the density of polypropylene, and at the same time greatly reduce the mechanical properties of polypropylene, resulting in a significant decrease in the impact strength of the material and a relatively brittle product; at the same time, the large amount of inorganic fillers usually reduces the gloss of polypropylene. Summary of the invention

[0006] The main purpose of the present invention is to provide a polypropylene composite material, a preparation method and application thereof, so as to solve the problem that the polypropylene material in the prior art cannot have low density, low shrinkage and high impact resistance.

[0007] In order to achieve the above-mentioned object, according to one aspect of the present invention, a polypropylene composite material is provided, wherein the raw materials include polypropylene resin, maleic anhydride grafted polypropylene, polyolefin elastomer, chopped glass fibers and inorganic filler; wherein the weight ratio of the polypropylene resin to the polyolefin elastomer is (70-85):(10-15); and the weight percentage of the inorganic filler in the polypropylene composite material is ≤8%.

[0008] Furthermore, the weight ratio of the chopped glass fiber to the polyolefin elastomer is 1:(1-1.5); and / or the weight ratio of the chopped glass fiber to the inorganic filler is 1:(0.5-0.9); preferably, the raw materials of the polypropylene composite material include, by weight, 70-85 parts of polypropylene resin, 3-8 parts of maleic anhydride grafted polypropylene, 10-15 parts of polyolefin elastomer, 8-15 parts of chopped glass fibers and 5-7 parts of inorganic filler.

[0009] Furthermore, the polypropylene resin includes one or more of copolymer polypropylene resin, isotactic homopolymer polypropylene resin and atactic homopolymer polypropylene resin; preferably, the weight average molecular weight of the polypropylene resin is 2×10 5 ~5×10 5 , the melt flow rate is 1.5 to 2.5 g / 10 min; and / or the weight average molecular weight of maleic anhydride grafted polypropylene is 8×10 4 ~2×10 5 , the grafting rate is 0.8 to 0.9; and / or the polyolefin elastomer includes one or more of POE elastomer, TPU elastomer and EVA elastomer; preferably, the weight average molecular weight of the polyolefin elastomer is 4×10 4 ~1.3×10 5 , density is 0.8~0.9g / cm 3 ; and / or the density of chopped glass fibers is 2 to 3 g / cm 3, the fiber length is 4-6 mm, the fiber diameter is 10-15 μm; and / or the inorganic filler includes one or more of talc, calcium carbonate and mica; preferably, the particle size of talc is 3-5 μm, and the density is 2-4 g / cm 3 .

[0010] Furthermore, the raw material of the polypropylene composite material also includes, by weight, 0.2 to 0.8 parts of an antioxidant and 0.5 to 2.0 parts of a lubricant; preferably, the antioxidant includes one or more of antioxidant 1010, antioxidant 1076 and antioxidant 1098; and / or the lubricant includes dimethyl silicone oil and / or mineral oil.

[0011] According to another aspect of the present invention, a method for preparing the above-mentioned polypropylene composite material of the present invention is provided, comprising the following steps: step S1, mixing and drying polypropylene resin, maleic anhydride grafted polypropylene, polyolefin elastomer, chopped glass fibers and inorganic filler to obtain a dried mixture; step S2, melt-extruding and granulating the dried mixture to obtain a molten blend; step S3, injection molding the molten blend to obtain a polypropylene composite material.

[0012] Furthermore, in step S1, the drying temperature is 70-80°C and the drying time is 5-8h.

[0013] Furthermore, in step S2, the temperature of melt extrusion granulation is 180-200°C; preferably, the melt extrusion granulation includes six stages of heating performed in sequence, and the heating temperatures are 180°C, 180°C, 185°C, 190°C, 195°C, and 200°C, respectively; preferably, the melt extrusion granulation is carried out in a twin-screw extruder; more preferably, the aspect ratio of the twin-screw extruder is 32-40, the screw speed is 140-160r / min, and the feeder speed is 20-40r / min.

[0014] Furthermore, step S2 also includes the following steps: mixing the dried mixed material with an antioxidant and a lubricant, and then performing melt extrusion granulation.

[0015] Further, in step S3, the temperature of the injection molding process is 180-200°C; preferably, the injection molding process includes four stages of heating performed in sequence, and the heating temperatures are 185°C, 190°C, 195°C, and 200°C, respectively; and / or the injection molding pressure of the injection molding process is 60-100MPa, the holding time is 30-60s, and the cooling time is 30-40s.

[0016] According to another aspect of the present invention, a plastic product is provided, wherein the raw material of the plastic product comprises the polypropylene composite material of the present invention.

[0017] By applying the technical solution of the present invention, short glass fibers are used to reduce the molding shrinkage of polypropylene and improve its strength at the same time; maleic anhydride grafted polypropylene is used to improve the compatibility of short glass fibers with polypropylene resin, so that the effect of short glass fibers can be fully exerted; a small amount of inorganic fillers and short glass fibers are used to coordinate the filler modification effect, which can effectively reduce the molding shrinkage of polypropylene and further improve the bending and impact properties of polypropylene; an appropriate amount of low molding shrinkage polyolefin elastomer and short glass fibers are used to coordinate the blending modification effect, which can effectively reduce the molding shrinkage of polypropylene while improving its toughness, thereby reducing the molding shrinkage of polypropylene materials without significantly increasing the density of polypropylene materials, and improving the impact resistance of polypropylene materials. In summary, the present invention adopts a method combining blending modification and filling modification, which significantly improves the mechanical properties of the material such as molding shrinkage and impact resistance on the basis of maintaining the low density of polypropylene materials. DETAILED DESCRIPTION

[0018] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0019] As described in the background of the present invention, the prior art has the problem that polypropylene materials cannot take into account low density, low shrinkage and high impact resistance. In order to solve the above problems, in a typical embodiment of the present invention, a polypropylene composite material is provided, the raw materials include polypropylene resin, maleic anhydride grafted polypropylene, polyolefin elastomer, chopped glass fiber and inorganic filler; wherein the weight ratio of polypropylene resin to polyolefin elastomer is (70-85): (10-15); and the weight percentage of inorganic filler in the polypropylene composite material is ≤8%.

[0020] The present invention mainly aims at the shortcomings of large shrinkage and poor dimensional stability of polypropylene. On the basis of not significantly increasing the density of polypropylene, the above shortcomings are improved by blending modification and filling modification methods, while improving or maintaining the good mechanical properties of polypropylene.

[0021] Among them, short glass fibers can effectively reduce the molding shrinkage of polypropylene while improving its strength. However, the compatibility of short glass fibers with polypropylene is poor, and the improvement effect on the performance of polypropylene is not significant. It is necessary to add an additive to improve the compatibility. Maleic anhydride grafted polypropylene as a compatibilizer can effectively improve the compatibility of short glass fibers with polypropylene, so that polypropylene can better adhere to the surface of short glass fibers, further reduce the molding shrinkage, and improve the mechanical properties. The flaky structure of a small amount of inorganic filler can affect the crystallization and orientation of polypropylene, and synergize with short glass fibers to play a filler modification role. Due to the small amount of addition, the density of polypropylene materials will not increase significantly. At the same time, it can effectively reduce the molding shrinkage of polypropylene and further improve the bending and impact properties of polypropylene. The molding shrinkage of polyolefin elastomers themselves is very low, and polyolefin elastomers can hinder the crystallization of polypropylene. Therefore, polyolefin elastomers and short glass fibers synergistically play a blending modification role, which can effectively reduce the molding shrinkage of polypropylene while improving its toughness.

[0022] In summary, the present invention achieves the best combination of good blending modification and low-cost filling modification by controlling the addition amount of polyolefin elastomer and inorganic filler, and significantly improves the mechanical properties of the material such as molding shrinkage and impact resistance while maintaining the low density of the polypropylene material. In addition, the raw material source of the polypropylene composite material of the present invention is abundant, simple and easy to purchase, and convenient for large-scale industrial production.

[0023] The density of the polypropylene composite material of the present invention is 0.9-1.1 g / cm 3 , molding shrinkage is 0.6-1%, tensile strength is 24-40MPa, flexural modulus is 1200-2200MPa, notched impact strength is ≥12kJ / m 2 , preferably 12 to 28 kJ / m 2 .

[0024] In a preferred embodiment, the weight ratio of chopped glass fibers to polyolefin elastomer is 1:(1-1.5); and / or the weight ratio of chopped glass fibers to inorganic fillers is 1:(0.5-0.9). Under the above conditions, the polyolefin elastomer can better cooperate with the chopped glass fibers to play a blending modification role, and the inorganic filler can better cooperate with the chopped glass fibers to play a filler modification role, thereby further reducing the molding shrinkage of polypropylene and further improving the impact resistance of polypropylene. Preferably, by weight, the raw materials of the polypropylene composite material include 70-85 parts of polypropylene resin, 3-8 parts of maleic anhydride grafted polypropylene, 10-15 parts of polyolefin elastomer, 8-15 parts of chopped glass fibers and 5-7 parts of inorganic fillers. The polypropylene composite material composed above can better balance low density, low shrinkage and high impact resistance.

[0025] The specific types and characteristic parameters of each component can be selected according to actual needs. In a preferred embodiment, the polypropylene resin includes one or more of copolymer polypropylene resin, isotactic homopolymer polypropylene resin and atactic homopolymer polypropylene resin; preferably, the weight average molecular weight of the polypropylene resin is 2×10 5 ~5×10 5 , the melt flow rate is 1.5 to 2.5 g / 10 min, and the most preferred is a copolymerized polypropylene resin with a grade of 2500H; and / or a weight average molecular weight of maleic anhydride grafted polypropylene is 8×10 4 ~2×10 5 , the grafting rate is 0.8 to 0.9; and / or the polyolefin elastomer includes one or more of POE elastomer, TPU elastomer and EVA elastomer; preferably, the weight average molecular weight of the polyolefin elastomer is 4×10 4 ~1.3×10 5 , density is 0.8~0.9g / cm 3 ; and / or the density of chopped glass fibers is 2 to 3 g / cm 3 , the fiber length is 4-6 mm, the fiber diameter is 10-15 μm; and / or the inorganic filler includes one or more of talc, calcium carbonate and mica; preferably, the particle size of talc is 3-5 μm, and the density is 2-4 g / cm 3 Under the above conditions, the role of each component can be better exerted, and it is more conducive to the synergistic effect of blending modification and filler modification, improving the shrinkage performance and mechanical properties of polypropylene composite materials while maintaining low density.

[0026] In order to further improve the long-term stability of the polypropylene composite material and facilitate industrial preparation, in a preferred embodiment, the raw material of the polypropylene composite material also includes 0.2 to 0.8 parts of an antioxidant and 0.5 to 2.0 parts of a lubricant, by weight; preferably, the antioxidant includes one or more of antioxidant 1010 (tetrakis(methyl-β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) pentaerythritol ester), antioxidant 1076 and antioxidant 1098; and / or the lubricant includes dimethyl silicone oil and / or mineral oil.

[0027] In another typical embodiment of the present invention, a method for preparing the above-mentioned polypropylene composite material of the present invention is also provided, comprising the following steps: step S1, mixing and drying polypropylene resin, maleic anhydride grafted polypropylene, polyolefin elastomer, chopped glass fibers and inorganic filler to obtain a dried mixture; step S2, melt-extruding and granulating the dried mixture to obtain a molten blend; step S3, injection molding the molten blend to obtain a polypropylene composite material.

[0028] The present invention first mixes polypropylene resin, maleic anhydride grafted polypropylene, polyolefin elastomer, chopped glass fibers and inorganic fillers and dries them in a vacuum drying oven, so that the polypropylene resin and the added materials are fully dried, and bubbles, surface silver streaks and streaks are avoided in the product during the extrusion process, which affect the product appearance and use performance, and obtain a dried mixed material. Then the dried mixed material is melt-extruded and granulated, and in this process, under the action of the compatibilizer maleic anhydride grafted polypropylene, the interaction between the inorganic filler or the chopped glass fibers and the polypropylene resin is greatly increased, and the addition of the inorganic filler or the chopped glass fibers has an inhibitory effect on the crystallization behavior of the polypropylene resin, thereby reducing the molding shrinkage of the polypropylene resin, while the polyolefin elastomer itself has a low shrinkage, and can also hinder the crystallization of the polypropylene resin, thereby further reducing the effect of the molding shrinkage, and obtain a melt blend. Finally, the melt blend is injection molded, and in this process, through the feeding plasticization process, the materials can be mixed and reacted again, and the inorganic filler and the like can affect the crystallization behavior of polypropylene through the above-mentioned mechanism again, and a polypropylene composite material is obtained. The preparation method is simple and easy to operate. The prepared polypropylene composite material can have low density, low shrinkage and high impact resistance, and is suitable for industrial production and application.

[0029] In a preferred embodiment, in step S1, the drying temperature is 70-80°C and the drying time is 5-8 hours. The above conditions are conducive to further drying of the polypropylene resin and the additives, and do not affect their processing and use performance.

[0030] In order to make the polypropylene composite material fully melt-mixed during extrusion, a suitable melting temperature is required. In a preferred embodiment, in step S2, the temperature of melt extrusion granulation is 180-200°C; preferably, melt extrusion granulation includes six stages of heating in sequence, and the heating temperatures are 180°C, 180°C, 185°C, 190°C, 195°C, and 200°C respectively; preferably, melt extrusion granulation is carried out in a twin-screw extruder, the head heating temperature is 195°C, and the material temperature is 200°C; more preferably, the aspect ratio of the twin-screw extruder is 32-40, the screw speed is 140-160r / min, and the feeder speed is 20-40r / min. Under the above conditions, the residual crystal nuclei will not be reduced due to the excessively high melting temperature, so that the crystal nuclei are mainly formed in a homogeneous phase during cooling and the crystal size increases, and the residual crystal nuclei will not be too much due to the low melting temperature, causing heterogeneous nucleation, which is more conducive to making the crystal size small and uniform, and is conducive to improving the mechanical properties of the composite material.

[0031] In a preferred embodiment, step S2 further comprises the following steps: mixing the dried mixed material with an antioxidant and a lubricant, and then performing melt extrusion granulation. The antioxidant can further improve the long-term stability of the composite material, and the lubricant can enter the non-continuous micropores uniformly distributed inside the polypropylene resin during extrusion, thereby further improving the fluidity and demoulding properties of the molten material during the preparation of the composite material, and improving the processing performance of the product.

[0032] In order to further melt and plasticize the polypropylene composite material again, the material temperature should not be too low, which may easily cause material shortage, welding marks, etc., and the production cycle is long; the material temperature should not be too high, which may easily cause plastic degradation and reduce the physical and mechanical properties of the product. Based on this, in a preferred embodiment, in step S3, the temperature of the injection molding process is 180-200°C; preferably, the injection molding process includes four stages of heating in sequence, and the heating temperatures are 185°C, 190°C, 195°C, and 200°C respectively; and / or the injection molding pressure of the injection molding process is 60-100MPa, the holding time is 30-60s, and the cooling time is 30-40s. Among them, the injection molding process can be carried out in an injection molding machine. The above conditions can also further guarantee product quality and production cycle.

[0033] In another typical embodiment of the present invention, a plastic product is provided. The raw material of the plastic product includes the above-mentioned polypropylene composite material of the present invention, which has a significantly reduced shrinkage rate, a low density, and high impact resistance. It can be widely used in the fields of automobiles, home appliances, construction, medical treatment, packaging, etc.

[0034] Typically but not limiting, the weight ratio of the chopped glass fibers to the polyolefin elastomer is 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5 or a boundary value consisting of any two of them.

[0035] Typically but not limiting, the weight ratio of the chopped glass fibers to the inorganic filler is 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9 or a boundary value consisting of any two of them.

[0036] Typically but not limiting, the raw materials of the polypropylene composite material include, by weight, 70, 72, 75, 78, 80, 82, 85 parts of polypropylene resin or the boundary value composed of any two of their numerical values, 3, 4, 5, 6, 7, 8 parts of maleic anhydride grafted polypropylene or the boundary value composed of any two of their numerical values, 10, 11, 12, 13, 14, 15 parts of polyolefin elastomer or the boundary value composed of any two of their numerical values, 8, 9, 10, 11, 12, 13, 14, 15 parts of chopped glass fibers or the boundary value composed of any two of their numerical values, and 5, 6, 7 parts or the boundary value composed of any two of their numerical values ​​of inorganic filler.

[0037] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0038] Example 1

[0039] The components of polypropylene composite materials are shown in Table 1:

[0040] Table 1

[0041]

[0042] The preparation method is as follows:

[0043] Step S1, mixing polypropylene resin, maleic anhydride grafted polypropylene, polyolefin elastomer, chopped glass fibers and inorganic filler and drying them in a vacuum drying oven at a temperature of 75° C. for 6 hours to obtain a dried mixture;

[0044] Step S2, mixing the dried mixed material with an antioxidant and a lubricant, and then performing melt extrusion granulation in a twin-screw extruder, including six-stage heating, the heating temperatures are 180° C., 180° C., 185° C., 190° C., 195° C., and 200° C., the aspect ratio is 36, the screw speed is 150 r / min, and the feeder speed is 30 r / min, to obtain a molten blend;

[0045] Step S3, injection molding the molten blend in an injection molding machine, including four-stage heating, the heating temperatures are 185° C., 190° C., 195° C., and 200° C., the injection pressure is 80 MPa, the holding time is 30 s, and the cooling time is 35 s, to obtain a polypropylene composite material.

[0046] Example 2

[0047] The components of polypropylene composite materials are shown in Table 2:

[0048] Table 2

[0049]

[0050] The preparation method is as follows:

[0051] Step S1, mixing polypropylene resin, maleic anhydride grafted polypropylene, polyolefin elastomer, chopped glass fibers and inorganic filler and drying them in a vacuum drying oven at a temperature of 75° C. for 6 hours to obtain a dried mixture;

[0052] Step S2, mixing the dried mixed material with an antioxidant and a lubricant, and then performing melt extrusion granulation in a twin-screw extruder, including six-stage heating, the heating temperatures are 180° C., 180° C., 185° C., 190° C., 195° C., and 200° C., the aspect ratio is 36, the screw speed is 150 r / min, and the feeder speed is 30 r / min, to obtain a molten blend;

[0053] Step S3, injection molding the molten blend in an injection molding machine, including four-stage heating, the heating temperatures are 185° C., 190° C., 195° C., and 200° C., the injection pressure is 80 MPa, the holding time is 30 s, and the cooling time is 35 s, to obtain a polypropylene composite material.

[0054] Example 3

[0055] The components of polypropylene composite materials are shown in Table 3:

[0056] Table 3

[0057]

[0058] The preparation method is as follows:

[0059] Step S1, mixing polypropylene resin, maleic anhydride grafted polypropylene, polyolefin elastomer, chopped glass fibers and inorganic filler and drying them in a vacuum drying oven at a temperature of 75° C. for 6 hours to obtain a dried mixture;

[0060] Step S2, mixing the dried mixed material with an antioxidant and a lubricant, and then performing melt extrusion granulation in a twin-screw extruder, including six-stage heating, the heating temperatures are 180° C., 180° C., 185° C., 190° C., 195° C., and 200° C., the aspect ratio is 36, the screw speed is 150 r / min, and the feeder speed is 30 r / min, to obtain a molten blend;

[0061] Step S3, injection molding the molten blend in an injection molding machine, including four-stage heating, the heating temperatures are 185° C., 190° C., 195° C., and 200° C., the injection pressure is 80 MPa, the holding time is 30 s, and the cooling time is 35 s, to obtain a polypropylene composite material.

[0062] Example 4

[0063] The components of polypropylene composite materials are shown in Table 4:

[0064] Table 4

[0065]

[0066] The preparation method is as follows:

[0067] Step S1, mixing polypropylene resin, maleic anhydride grafted polypropylene, polyolefin elastomer, chopped glass fibers and inorganic filler and drying them in a vacuum drying oven at a temperature of 75° C. for 6 hours to obtain a dried mixture;

[0068] Step S2, mixing the dried mixed material with an antioxidant and a lubricant, and then performing melt extrusion granulation in a twin-screw extruder, including six-stage heating, the heating temperatures are 180° C., 180° C., 185° C., 190° C., 195° C., and 200° C., the aspect ratio is 36, the screw speed is 150 r / min, and the feeder speed is 30 r / min, to obtain a molten blend;

[0069] Step S3, injection molding the molten blend in an injection molding machine, including four-stage heating, the heating temperatures are 185° C., 190° C., 195° C., and 200° C., the injection pressure is 80 MPa, the holding time is 30 s, and the cooling time is 35 s, to obtain a polypropylene composite material.

[0070] Example 5

[0071] The components of the polypropylene composite material are shown in Table 5:

[0072] Table 5

[0073]

[0074] The preparation method is as follows:

[0075] Step S1, mixing polypropylene resin, maleic anhydride grafted polypropylene, polyolefin elastomer, chopped glass fibers and inorganic filler and drying them in a vacuum drying oven at a temperature of 75° C. for 6 hours to obtain a dried mixture;

[0076] Step S2, mixing the dried mixed material with an antioxidant and a lubricant, and then performing melt extrusion granulation in a twin-screw extruder, including six-stage heating, the heating temperatures are 180° C., 180° C., 185° C., 190° C., 195° C., and 200° C., the aspect ratio is 36, the screw speed is 150 r / min, and the feeder speed is 30 r / min, to obtain a molten blend;

[0077] Step S3, injection molding the molten blend in an injection molding machine, including four-stage heating, the heating temperatures are 185° C., 190° C., 195° C., and 200° C., the injection pressure is 80 MPa, the holding time is 30 s, and the cooling time is 35 s, to obtain a polypropylene composite material.

[0078] Example 6

[0079] The components of the polypropylene composite material are shown in Table 6:

[0080] Table 6

[0081]

[0082] The preparation method is as follows:

[0083] Step S1, mixing polypropylene resin, maleic anhydride grafted polypropylene, polyolefin elastomer, chopped glass fibers and inorganic filler and drying them in a vacuum drying oven at a temperature of 75° C. for 6 hours to obtain a dried mixture;

[0084] Step S2, mixing the dried mixed material with an antioxidant and a lubricant, and then performing melt extrusion granulation in a twin-screw extruder, including six-stage heating, the heating temperatures are 180° C., 180° C., 185° C., 190° C., 195° C., and 200° C., the aspect ratio is 36, the screw speed is 150 r / min, and the feeder speed is 30 r / min, to obtain a molten blend;

[0085] Step S3, injection molding the molten blend in an injection molding machine, including four-stage heating, the heating temperatures are 185° C., 190° C., 195° C., and 200° C., the injection pressure is 80 MPa, the holding time is 30 s, and the cooling time is 35 s, to obtain a polypropylene composite material.

[0086] Examples 7 to 8

[0087] The difference from Example 1 is that the components of the polypropylene composite material are different, see Table 7:

[0088] Table 7

[0089] Weight Example 7 Example 8 Polypropylene resin 70 85 Maleic Anhydride Grafted Polypropylene 3 8 Polyolefin elastomer 10 15 Chopped Glass Fiber 8 15 Inorganic fillers 5 7 Antioxidants 0.2 0.8 Lubricants 0.5 2 Polypropylene resin: polyolefin elastomer 70:10 85:15 Inorganic filler ratio 5.2 5.3 Chopped glass fibers: Polyolefin elastomers 1:1.3 1:1.0 Chopped glass fiber: inorganic filler 1:0.6 1:0.5

[0090] Examples 9 to 10

[0091] The difference from Example 1 is that the component characteristics of the polypropylene composite material are different, see Table 8:

[0092] Table 8

[0093]

[0094]

[0095] Embodiment 11

[0096] The difference from Example 1 is that the preparation method of the polypropylene composite material is different, as follows:

[0097] Step S1, mixing polypropylene resin, maleic anhydride grafted polypropylene, polyolefin elastomer, chopped glass fibers and inorganic filler and drying them in a vacuum drying oven at a temperature of 70° C. for 8 hours to obtain a dried mixture;

[0098] Step S2, mixing the dried mixed material with an antioxidant and a lubricant, and then performing melt extrusion granulation in a twin-screw extruder, including six-stage heating, the heating temperatures are 180° C., 180° C., 185° C., 190° C., 195° C., and 200° C., the aspect ratio is 32, the screw speed is 140 r / min, and the feeder speed is 20 r / min, to obtain a molten blend;

[0099] Step S3, injection molding the molten blend in an injection molding machine, including four stages of heating, with heating temperatures of 185° C., 190° C., 195° C., and 200° C., respectively, an injection molding pressure of 60 MPa, a holding time of 60 s, and a cooling time of 40 s to obtain a polypropylene composite material.

[0100] Example 12

[0101] The difference from Example 1 is that the preparation method of the polypropylene composite material is different, as follows:

[0102] Step S1, mixing polypropylene resin, maleic anhydride grafted polypropylene, polyolefin elastomer, chopped glass fibers and inorganic filler and drying them in a vacuum drying oven at a temperature of 80° C. for 5 hours to obtain a dried mixture;

[0103] Step S2, mixing the dried mixed material with an antioxidant and a lubricant, and then performing melt extrusion granulation in a twin-screw extruder, including six-stage heating, the heating temperatures are 180° C., 180° C., 185° C., 190° C., 195° C., and 200° C., the aspect ratio is 40, the screw speed is 160 r / min, and the feeder speed is 40 r / min, to obtain a molten blend;

[0104] Step S3, injection molding the molten blend in an injection molding machine, including four-stage heating, the heating temperatures are 185° C., 190° C., 195° C., and 200° C., the injection pressure is 100 MPa, the holding time is 30 s, and the cooling time is 30 s to obtain a polypropylene composite material.

[0105] Example 13

[0106] The difference from Example 1 is that no antioxidant and lubricant are added.

[0107] Comparative Example 1

[0108] The difference from Example 1 is that the polypropylene composite material includes 100 parts of polypropylene and 0.5 parts of antioxidant 1010.

[0109] Comparative Examples 2 to 3

[0110] The difference from Example 1 is that the components of the polypropylene composite material are different, see Table 9:

[0111] Table 9

[0112]

[0113] Comparative Example 4

[0114] Example 2 of Chinese patent CN 109762256A.

[0115] The polypropylene materials of the above embodiments and comparative examples were subjected to performance tests, and the results are shown in Table 10.

[0116] Performance Test:

[0117] Molding shrinkage: According to the ASTM D955-08 shrinkage test standard, the PP-based composite material was molded into a 60mm×60mm×2mm standard specimen using an injection molding machine, and the specimen size was tested after the specimen was placed at room temperature for 24 hours;

[0118] Tensile strength: According to GB / T1040.2 standard, the tensile properties of PP-based composite materials were tested at a test speed of 50 mm / min;

[0119] Flexural modulus: The flexural properties of PP-based composite materials were tested according to ASTM D790, with a test speed of 2 mm / min, and the weight and volume of the standard bending specimen were measured to calculate its theoretical density;

[0120] Notched impact strength: The notched impact strength of PP-based composites was tested according to ISO 180-1992 standard.

[0121] Table 10

[0122]

[0123]

[0124] It can be seen from the above that: compared with the pure polypropylene material of Comparative Example 1, the molding shrinkage of the polypropylene composite materials of each embodiment of the present invention is significantly reduced, the density is slightly increased (but still at a lower level compared with Comparative Examples 2 to 3), the tensile strength, flexural modulus and notched impact strength are significantly increased, and the comprehensive performance is significantly better than that of Comparative Example 4, which fully meets the requirements of actual use of the material.

[0125] As can be seen from the above, compared with the comparative example, each embodiment of the present invention uses short glass fibers to reduce the molding shrinkage of polypropylene and improve its strength at the same time; maleic anhydride grafted polypropylene is used to improve the compatibility of short glass fibers with polypropylene resin, so that the effect of short glass fibers can be fully exerted; a small amount of inorganic fillers and short glass fibers are used to synergistically play the role of filler modification, which can effectively reduce the molding shrinkage of polypropylene and further improve the bending and impact properties of polypropylene; an appropriate amount of low molding shrinkage polyolefin elastomer and short glass fibers are used to synergistically play the role of blending modification, which can effectively reduce the molding shrinkage of polypropylene while improving its toughness, thereby reducing the molding shrinkage of polypropylene materials without significantly increasing the density of polypropylene materials, and improving the impact resistance of polypropylene materials. In summary, the present invention adopts a method combining blending modification and filling modification, which significantly improves the mechanical properties of the material such as molding shrinkage and impact resistance while maintaining the low density of the polypropylene material. In addition, it can be seen that when each process parameter is within the preferred range of the present invention, the comprehensive performance of the material is better.

[0126] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A polypropylene composite material, characterized in that: The raw materials include polypropylene resin, maleic anhydride grafted polypropylene, polyolefin elastomer, chopped glass fiber and inorganic filler; Wherein, the weight ratio of the polypropylene resin to the polyolefin elastomer is (70-85):(10-15); and the weight percentage of the inorganic filler in the polypropylene composite material is ≤8%.

2. The polypropylene composite material according to claim 1, characterized in that: The weight ratio of the chopped glass fibers to the polyolefin elastomer is 1:(1-1.5); and / or the weight ratio of the chopped glass fibers to the inorganic filler is 1:(0.5-0.9); Preferably, the raw materials of the polypropylene composite material include, by weight, 70 to 85 parts of the polypropylene resin, 3 to 8 parts of the maleic anhydride grafted polypropylene, 10 to 15 parts of the polyolefin elastomer, 8 to 15 parts of the chopped glass fibers and 5 to 7 parts of the inorganic filler.

3. The polypropylene composite material according to claim 1 or 2, characterized in that: The polypropylene resin includes one or more of copolymer polypropylene resin, isotactic homopolymer polypropylene resin and atactic homopolymer polypropylene resin; preferably, the weight average molecular weight of the polypropylene resin is 2×10 5 ~5×10 5 , a melt flow rate of 1.5 to 2.5 g / 10 min; and / or The weight average molecular weight of the maleic anhydride grafted polypropylene is 8×10 4 ~2×10 5 , the grafting rate is 0.8 to 0.9; and / or The polyolefin elastomer includes one or more of POE elastomer, TPU elastomer and EVA elastomer; preferably, the weight average molecular weight of the polyolefin elastomer is 4×10 4 ~1.3×10 5 , density is 0.8~0.9g / cm 3 ; and / or The density of the chopped glass fibers is 2 to 3 g / cm 3 , the fiber length is 4 to 6 mm, the fiber diameter is 10 to 15 μm; and / or The inorganic filler includes one or more of talc, calcium carbonate and mica; preferably, the talc has a particle size of 3 to 5 μm and a density of 2 to 4 g / cm 3 .

4. The polypropylene composite material according to any one of claims 1 to 3, characterized in that The raw material of the polypropylene composite material further includes 0.2 to 0.8 parts of an antioxidant and 0.5 to 2.0 parts of a lubricant by weight; Preferably, the antioxidant includes one or more of antioxidant 1010, antioxidant 1076 and antioxidant 1098; and / or the lubricant includes dimethyl silicone oil and / or mineral oil.

5. The method for preparing the polypropylene composite material according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step S1, mixing and drying polypropylene resin, maleic anhydride grafted polypropylene, polyolefin elastomer, chopped glass fibers and inorganic filler to obtain a dried mixture; Step S2, melt-extruding and granulating the dried mixed material to obtain a molten blend; Step S3, injection molding the molten blend to obtain the polypropylene composite material.

6. The preparation method according to claim 5, characterized in that: In the step S1, the drying temperature is 70-80° C. and the drying time is 5-8 hours.

7. The preparation method according to claim 5 or 6, characterized in that: In the step S2, the temperature of the melt extrusion granulation is 180-200°C; preferably, the melt extrusion granulation includes six stages of heating performed in sequence, and the heating temperatures are 180°C, 180°C, 185°C, 190°C, 195°C, and 200°C respectively; Preferably, the melt extrusion granulation is carried out in a twin-screw extruder; More preferably, the aspect ratio of the twin-screw extruder is 32-40, the screw speed is 140-160 r / min, and the feeder speed is 20-40 r / min.

8. The preparation method according to any one of claims 5 to 7, characterized in that: The step S2 further comprises the following steps: mixing the dried mixed material with an antioxidant and a lubricant, and then performing the melt extrusion granulation.

9. The preparation method according to any one of claims 5 to 8, characterized in that: In step S3, the temperature of the injection molding process is 180-200°C; preferably, the injection molding process includes four stages of heating performed in sequence, and the heating temperatures are 185°C, 190°C, 195°C, and 200°C, respectively; and / or the injection molding pressure of the injection molding process is 60-100MPa, the holding time is 30-60s, and the cooling time is 30-40s.

10. A plastic product, characterized in that: The raw material of the plastic product comprises the polypropylene composite material according to any one of claims 1 to 4.