Foam stabilizers for phenolic foams
By optimizing the structure and proportion of polyether siloxane and combining with ethoxylated vegetable oil, the problem of cyclic siloxane formation in phenolic foam is solved, excellent thermal insulation performance and low-defect foam structure are achieved, and emissions are reduced , meets the performance requirements of phenolic foam.
Patent Information
- Application Number
- CN202410613757.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-19
- Filing Date
- 2024-05-17
- Publication Date
- 2024-11-22
AI Technical Summary
When using polyether modified silicones as foam stabilizers, existing phenolic foams are prone to form unfavorable cyclic silicones, resulting in emission problems and performance degradation, and lack effective methods to reduce or avoid these emissions.
Using a specific polyether siloxane composition as foam stabilizer, by optimizing its structure and proportion, reducing the formation of cyclic siloxane, and combining ethoxylated vegetable oil and other ingredients, it can prepare excellent thermal insulation performance and low thermal insulation performance. Phenolic foam with defective foam structure.
Excellent thermal insulation properties and long-term characteristics of the phenolic foam are achieved, while reducing the formation of cyclic siloxanes, reducing emissions, and obtaining a low-defect fine cell structure without damaging other properties of the material.
Smart Images

Figure BDA0004844442640000021 
Figure BDA0004844442640000031 
Figure BDA0004844442640000061
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of phenolic foams. In particular, the present invention relates to a composition for preparing phenolic foams, a method for preparing phenolic foams, phenolic foams prepared according to the invention and their use. In the context of the present invention, phenolic foams are understood to mean in particular foams obtained by reacting phenolic resins with acids as catalysts and adding blowing agents and foam stabilizers. Phenolic foams are known to the person skilled in the art and are described, for example, in EP 3830174 A1, DE 602004006376 T2, EP 2898005 A1, EP 1922357 A1, WO 2022043561 A1, EP 4073155 A1, AU 2021238847 A1 or WO 2006114777 A1. Phenolic foams are also referred to as phenolic resin foams. This also applies to the present invention. Background Art
[0002] In the preparation of phenolic foams, cell stabilizing additives or foam stabilizing additives can generally be used, which ensure fine cells with a low defect level, a uniform foam structure, and thus have a substantially positive effect on the performance characteristics of the foam, in particular, for example, the thermal insulation capacity. For this purpose, foam stabilizers can generally be used, for example, foam stabilizers based on ethoxylated vegetable oils such as castor oil, as described in EP 3830174 A1. It has been found that the use of polyether-modified siloxanes (PES), as described, for example, in WO 2022043561 A1, is particularly effective for further improving the performance characteristics. In particular, the combination of ethoxylated vegetable oils and polyether-modified siloxanes produces excellent performance characteristics. Therefore, this combination constitutes a class of foam stabilizers that is generally preferred in the preparation of phenolic foams.
[0003] WO 2004 / 056911 A2 describes, inter alia, the preparation of closed-cell phenolic foams using polyethersiloxane copolymers as foam stabilizers for improving thermal conductivity after aging, the latter being described using typical polysiloxane, polyethylene oxide and polypropylene oxide contents.
[0004] WO 2022 / 043561 A1 describes, inter alia, the preparation of phenolic foams using foam stabilizers based on a mixture of ethoxylated castor oil and polyether siloxane copolymers having a polyethylene oxide content of less than 50%, wherein preference is given to using those polyether siloxane copolymers having a molecular weight of 9500 to 25000 g / mol and an HLB value of 9 to 13.
[0005] There has been no description to date of the influence of foam stabilizers and their structure on foam emissions and of ways to reduce or avoid these emissions.
[0006] The use of polyether-modified siloxanes as foam stabilizers in the presence of acids as catalysts can lead to degradation of the polyether-modified siloxanes and ultimately to the formation of cyclic siloxanes, preferably octamethylcyclotetrasiloxane (D4), decamethylcyclopentasiloxane (D5) and dodecamethylcyclohexasiloxane (D6), especially D4 and D5, which have an adverse effect on the properties of the phenolic foams, especially on emissions.
[0007] Against this background, it was an object of the present invention to provide phenolic foams which have similar performance characteristics, in particular thermal insulation properties, to phenolic foams prepared with conventional polyether-modified siloxanes, but which, with regard to emissions relating to the formation of cyclic siloxanes, have zero or lower formation of D4, D5 and / or D6, in particular D4 and / or D5. Summary of the invention
[0008] This object is achieved by the subject matter of the present invention. The present invention provides a composition for preparing a phenolic foam, comprising at least one phenolic resin, at least one blowing agent, at least one catalyst and at least one polyether siloxane of formula 1:
[0009] M a M 1 b D c D 1 d (Formula 1)
[0010] in
[0011]
[0012] a=0 to 2,
[0013] b = 0 to 2,
[0014] c=0 to 100, preferably 0 to 75, more preferably 0 to 50,
[0015] d=1 to 100, preferably 1 to 75, more preferably 1 to 50,
[0016] in
[0017] a+b=2,
[0018] a+b+c+d>4, preferably>7,
[0019] (a+b+c+d) / (b+d)<5, preferably 1 to 4, more preferably 1 to 3, R=each independently the same or different alkyl group having 1 to 16 carbon atoms, the same or different aryl group having 6 to 16 carbon atoms, H or -OR 2 , preferably methyl, ethyl, phenyl or H, especially methyl,
[0020] R 2 = each independently the same or different alkyl group having 1 to 16 carbon atoms, the same or different aryl group having 6 to 16 carbon atoms or H,
[0021] R 1 = each independently the same or different alkyl group having 6 to 18 carbon atoms or the same or different polyether group, preferably the same or different alkyl group having 6 to 18 carbon atoms or the same or different polyether group of formula 2:
[0022]
[0023] R 3 = each independently the same or different divalent alkyl radical having 2 to 15 carbon atoms, preferably the same or different divalent alkyl radical having 3 to 6 carbon atoms, particularly preferably -(CH 2 ) 3 –,
[0024] R 4 = each independently the same or different alkyl radicals having 1 to 18 carbon atoms and optionally having an ether function, or the same or different aryl radicals having 6 to 18 carbon atoms and optionally having an ether function, or H, preferably H, methyl, ethyl or benzyl,
[0025] R 5 = each independently the same or different group selected from the following: R 2 and C(O)R 2 , preferably methyl, butyl, H or C(O)Me,
[0026] e=0 to 100, preferably 0 to 80, especially 0 to 60,
[0027] f=0 to 100, preferably 0 to 80, in particular 0 to 60,
[0028] g=0 to 100, preferably 0 to 80, especially 0 to 60,
[0029] h=0 to 100, preferably 0 to 60, more preferably 0,
[0030] where at least one of the values e, f, g and h is > 0,
[0031] wherein not more than 50% of the polyether siloxane of formula 1 is R 1 The groups are each independently the same or different alkyl groups having 6 to 18 carbon atoms, and the total amount of at least one polyether siloxane of formula 1 present is 0.1 to 20 parts by weight, preferably 0.5 to 10 parts by weight, more preferably 0.5 to 8 parts by weight, based on 100 parts by weight of the total amount of the phenolic resin used.
[0032] The subject matter of the invention is associated with a number of benefits. For example, it makes it possible to provide phenolic foams which meet the known requirements. In particular, the phenolic foams have very good insulating properties and show excellent long-term properties and a high surface quality. Advantageously, this can be achieved without impairing the other properties of the material and with only relatively little formation of cyclic siloxanes, if any, preferably D4, D5 and / or D6, in particular D4 and / or D5. Furthermore, particularly fine-celled, homogeneous foam structures with a low level of defects can be achieved. The invention likewise allows the use in combination with alkoxylated vegetable oils known from the prior art.
[0033] The composition according to the invention comprises at least one polyether siloxane of the formula 1. Polyether siloxanes used with particular preference in the context of the present invention are described below in three preferred embodiments of the invention.
[0034] A particularly preferred embodiment of the present invention is when the composition according to the invention has the following characteristics: for R 1 , at least one polyether siloxane of formula 1 contains at least one polyether group of general formula 2, wherein:
[0035] e = 6 to 16,
[0036] f=g=h=0
[0037] or
[0038] e+f+g=8 to 50,
[0039] h=0,
[0040] (f+g) / (e+f+g)>0 to 0.9, more preferably 0.1 to 0.6.
[0041] It is another particularly preferred embodiment of the present invention when the composition according to the invention has the following characteristics: 1 , at least one polyether siloxane of formula 1 comprises at least two different polyether groups of formula 2, wherein at least one polyether corresponds to class 1 and at least one polyether corresponds to class 2, wherein:
[0042] a=0 to 2, more preferably 2,
[0043] b = 0 to 2, more preferably 0,
[0044] c=0 to 10, preferably 0 to 5, more preferably 0,
[0045] d = 1 to 80, preferably 1 to 50, more preferably 5 to 40,
[0046] in
[0047] a+b=2,
[0048] a+b+c+d>4, preferably>7
[0049] and
[0050] Category 1:
[0051] e+f+g=10 to 60, more preferably 14 to 40,
[0052] h=0,
[0053] (f+g) / (e+f+g)≥0.6, more preferably≥0.8, especially=1,
[0054] and
[0055] Category 2:
[0056] e = 6 to 16,
[0057] f=g=h=0,
[0058] or
[0059] e+f+g=8 to 50,
[0060] h=0,
[0061] (f+g) / (e+f+g)>0 to 0.5, more preferably 0.1 to 0.3,
[0062] And the preferred ratio of the first type of polyether to the second type of polyether in the polysiloxane is 10:
[0063] 90 wt % to 90:10 wt %, more preferably 20:80 wt % to 80:20 wt %,
[0064] In particular, it is 25:75% by weight to 75:25% by weight.
[0065] In a further particularly preferred embodiment of the present invention, the composition according to the invention has the following features: at least one polyether siloxane of the formula 1 contains at least two different R 1 A group in which at least one R 1 The group is a polyether group of formula 2, and one R 1 The group is an alkyl group having 6 to 18 carbon atoms, wherein not more than 50% of the R 1 The group is an alkyl group having 6 to 18 carbon atoms.
[0066] The composition according to the invention comprises at least one blowing agent.
[0067] Another particularly preferred embodiment of the present invention is when the at least one blowing agent is selected from the group consisting of:
[0068] - hydrocarbons having 3, 4 or 5 carbon atoms, preferably cyclopentane, isopentane and / or n-pentane, and
[0069] - halogenated hydrocarbons having 3, 4 or 5 carbon atoms, preferably isopropyl chloride, hydrofluoroolefins and / or hydrohaloolefins, preferably 1234ze, 1234yf, 1224yd, 1233zd(E) and / or 1336mzz.
[0070] The composition according to the invention may preferably additionally contain at least one silicon-free surfactant. In a particularly preferred embodiment of the present invention, at least one silicon-free surfactant is additionally present in the composition according to the invention in a total amount of 0.1 to 15 parts by weight, preferably 1 to 10 parts by weight, based on 100 parts by weight of the total amount of phenolic resin used.
[0071] The composition according to the invention may preferably additionally contain at least one alkoxylated, preferably ethoxylated vegetable oil, preferably castor oil. In a particularly preferred embodiment of the present invention, at least one alkoxylated, preferably ethoxylated, vegetable oil, preferably castor oil, is additionally present in the composition according to the invention in an amount of 0.1 to 15 parts by weight, preferably 1 to 10 parts by weight, based on 100 parts by weight of the total amount of phenolic resin used.
[0072] The composition according to the invention comprises at least one catalyst. In a further particularly preferred embodiment of the invention, the at least one catalyst is selected from the group consisting of organic acids and inorganic acids, the at least one catalyst is preferably selected from the group consisting of sulfuric acid, phosphoric acid, benzenesulfonic acid, xylenesulfonic acid, p-toluenesulfonic acid, ethylbenzenesulfonic acid, naphtholsulfonic acid, isopropylbenzenesulfonic acid and phenolsulfonic acid.
[0073] Furthermore, in a particularly preferred embodiment of the present invention, the at least one catalyst is present in a total amount of 1 to 30 parts by weight, preferably 1 to 25 parts by weight, more preferably 3 to 20 parts by weight, based on 100 parts by weight of the total amount of phenolic resin used.
[0074] The composition according to the invention comprises at least one phenolic resin. A further particularly preferred embodiment of the invention is that the at least one phenolic resin has a water content of 1% to 25% by weight, preferably 4% to 19% by weight, based on the total amount of phenolic resin used.
[0075] Particularly preferred phenolic foam formulations for the purposes of the present invention have a weight range of 5 to 900 kg / m 3 The foam density is preferably 1.5 g / cm2 and preferably has the composition shown in Table 1, which corresponds to a preferred embodiment of the present invention:
[0076] Table 1: Composition of preferred phenolic foam formulations
[0077]
[0078] The present invention also provides a method for preparing a phenolic foam, which is carried out using a reaction mixture comprising the above-mentioned composition of the present invention, especially the composition defined in any one of claims 1 to 10.
[0079] With regard to further preferred embodiments and configurations of the method according to the invention, reference is also made to the statements already given above regarding the composition according to the invention.
[0080] The present invention also provides a phenolic foam prepared by the above-mentioned process of the present invention, preferably using the composition of the present invention, in particular the composition as defined in any one of claims 1 to 10.
[0081] Particularly preferred phenolic foams have a density of 5 to 500 kg / m 3 , preferably 10 to 200 kg / m 3 , particularly preferably 12 to 100 kg / m 3 This is a particularly preferred embodiment of the invention.
[0082] The invention also provides the use of the phenolic foam according to the invention for thermal insulation.
[0083] Particularly preferred compositions of the present invention are described in more detail below.
[0084] Particularly preferred compositions of the present invention comprise the following components:
[0085] - at least one phenolic resin,
[0086] - at least one blowing agent,
[0087] - at least one catalyst,
[0088] - at least one polyether siloxane of the formula 1 as foam stabilizer,
[0089] - other optional additives etc.
[0090] The preparation of phenolic foams (these are also synonymously referred to as phenolic resin foams) is known per se. For the preparation of phenolic foams, one or more phenolic resins are used, preferably one or more types known as resols. The correspondingly usable phenolic resins, preferably resols, are known per se. In particular, they can be prepared in a known manner by condensation of phenol or phenol-based compounds (e.g. cresols, xylenols, p-alkylphenols, p-phenylphenol, resorcinol, etc.) with aldehydes (e.g. formaldehyde, furfural, acetaldehyde, etc.), preferably under alkaline conditions, for example by using catalytic amounts of alkali metal hydroxides (e.g. sodium hydroxide, potassium hydroxide or calcium hydroxide) or aliphatic amines (e.g. trimethylamine or triethylamine), preferably with an excess of aldehyde. This represents a common method for preparing phenolic resins, preferably resols, although the invention is not limited to the chemicals listed just above.
[0091] The molar ratio of phenolic groups to aldehyde groups is not subject to any restrictions. Preferably, the ratio is in the range of 1:1 to 1:3, more preferably in the range of 1:1.5 to 1:2.5. The free aldehyde content of the phenolic resin is preferably, but not limited to, 0.1% to 0.5% by weight. This can be determined by potentiometric titration with hydroxylamine hydrochloride according to ISO 11402:2004.
[0092] Preferred phenolic resins which can be used for foam preparation are liquid at 25° C. and standard pressure, preferably have a water concentration of about 1% to 25% by weight, preferably 5% to 20% by weight, and have hydroxymethyl groups as reactive substituents, as described in EP 0 170 357 B1. If desired, the viscosity of the phenolic resins can be adjusted, inter alia, via the water content. Thus, a high water content generally leads to a lower viscosity, which facilitates the handling of the resin and its mixing during the foam preparation process.
[0093] The viscosity of the preferred phenolic resins at 25° C. and standard pressure is preferably in the range of 1000 mPa*s to 28000 mPa*s and can be determined by conventional methods known to those skilled in the art, for example using a Brookfield viscometer. The basic principles regarding the preparation and composition of phenolic resins can be found in the prior art, in particular described in, for example, EP 3830174 A1, EP 2898005 A1, WO 2022043561 A1 or EP 4073155 A1.
[0094] Blowing agents and their use in the preparation of phenolic foams are known to those skilled in the art. The use of one or more blowing agents depends in principle on the nature of the system and the use of the resulting phenolic foam. Depending on the amount of blowing agent used, foams with high or low density can be prepared. For example, a foam with a density of preferably 5 kg / m can be prepared according to ASTM D1622-20. 3 Up to 900kg / m3 , preferably 5kg / m 3 Up to 500kg / m 3 , more preferably 10kg / m 3 Up to 200kg / m 3 , especially 12kg / m 3 Up to 100kg / m 3 of foam.
[0095] Blowing agents which are particularly preferably used have already been described above. Blowing agents which may be used may be one or more suitable compounds with a suitable boiling point, for example hydrocarbons having 3, 4 or 5 carbon atoms, preferably cyclopentane, isopentane or n-pentane, halogenated hydrocarbons, for example chlorinated hydrocarbons, such as ethylene dichloride, 1,2-dichloroethylene, n-propyl chloride, isopropyl chloride, butyl chloride, isobutyl chloride, amyl chloride, isopentyl chloride, 1,1-dichloroethylene, trichloroethylene or vinyl chloride, or hydrofluorocarbons (HFCs), for example HFC 245fa, HFC 134a or HFC 365mfc, hydrofluoroolefins (HFOs) or hydrohaloolefins, preferably 1234ze, 1234yf, 1224yd, 1233zd(E) or 1336mzz or mixtures thereof.
[0096] Particularly preferably usable catalysts have already been described above. Catalysts which can be used for the preparation of phenolic foams are known to the person skilled in the art from the prior art and are described, for example, in EP 0170357A1 or DE 602004006376 T2. For this purpose, conventional organic and inorganic acids known in the prior art can preferably be used. One or more acids can be used. The following substances are particularly preferably used: sulfuric acid, phosphoric acid, benzenesulfonic acid, xylenesulfonic acid, p-toluenesulfonic acid, ethylbenzenesulfonic acid, naphtholsulfonic acid, isopropylbenzenesulfonic acid and / or phenolsulfonic acid. In particular, the catalyst used can be a mixture of a plurality of these compounds. The preferred amount of catalyst for the complete reaction is influenced in particular by the water content of the phenolic resin and / or - when the catalyst is present as an aqueous solution - also by its water content. For example, a higher water content may require a higher acid concentration.
[0097] Phenolic foams can be formed in a known manner, namely in particular by reaction of a mixture comprising a phenolic resin, a blowing agent, a foam stabilizer and a catalyst. When the catalyst is added to the mixture of phenolic resin, blowing agent and foam stabilizer, an exothermic reaction occurs between the methylol groups and the phenol, leading to the formation of methylene bridges and crosslinking. Condensation is accompanied by the release of water. The exothermicity of the reaction and the foam formation is influenced by the nature and amount of the acid used, the nature of the blowing agent and the structure of the foam stabilizer.
[0098] As mentioned above, foam stabilizers and their use in the preparation of phenolic foams are well known to the person skilled in the art. According to the invention, at least one polyether siloxane of formula 1 is used. At least one polyether siloxane of formula 1 is used as foam stabilizer. In addition, additional foam stabilizers which assist in the generation of foam can also be used. These compounds are sufficiently known in the prior art. For example, EP 3830174A1 describes the use of ethoxylated castor oil.
[0099] The optional additives may be one or more substances known in the prior art and commonly used for preparing phenolic foams, such as viscosity reducers, plasticizers, hardeners, flame retardants, cell refining additives, fillers, dyes, pigments and / or fragrances. Suitable optional additives are described, for example, in EP 3830174A1, US 4444912A and EP 1922357A1.
[0100] Optionally used solid fillers can be, for example, metal hydroxides, such as aluminum hydroxide, magnesium hydroxide, metal carbonates, such as calcium carbonate, magnesium carbonate, barium carbonate or zinc carbonate, metal oxides, such as aluminum oxide or zinc oxide, or metal powders, such as zinc. The viscosity of the phenolic resin can optionally be reduced using, for example, monoethylene glycol or polyester polyols. Optionally present hardeners can be, for example, compounds with amino groups, such as urea or dicyandiamide. Urea is preferably used. These can additionally be used for foaming and for the preparation of phenolic resins.
[0101] The process for preparing phenolic foam according to the invention can be carried out by any known methods. These are known to the person skilled in the art and are described, for example, in EP 3830174 A1.
[0102] Unless the contrary is apparent from the present description, any preferred or particularly preferred embodiment of the present invention may be combined with one or more other preferred or particularly preferred embodiments of the present invention. DETAILED DESCRIPTION
[0103] The subject matter of the present invention is described below by way of example, without any intention to limit the present invention, and the scope of application of the present invention is apparent from the entire description and claims of these exemplary embodiments. When the scope, general formula or category of a compound is given, these include not only the corresponding scope or group of the compound explicitly mentioned, but also all sub-scopes and subgroups of the compound obtained by selecting a single value (scope) or compound. When a document is cited in the context of this specification, its entirety, especially with respect to the subject matter forming the context in which the document is cited, is intended to form an integral part of the disclosure of the present invention. Unless otherwise stated, the average values reported are all digital average values. Unless otherwise stated, when describing the parameters determined by measurement, the measurement is carried out at a temperature of 23°C and standard pressure (1atm=101325Pa).
[0104] Example
[0105] Synthesis of polyether siloxane foam stabilizer (PES) (=polyether siloxane of formula 1 and comparative example)
[0106] The Pt catalyst used for the preparation of the polyether siloxanes was a xylene solution of Karstedt's catalyst (platinum (0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (CAS 68478-92-2)). The Pt content of the solution was 2% by weight. The catalyst was obtained from Merck and used without further treatment.
[0107] For the synthesis of polyether siloxanes, allyl polyethers or allyl hydrocarbons according to the composition specified in Table 2 and 10 ppm of Pt, based on the total weight, in the form of the above-mentioned Pt catalyst are initially charged in a three-necked flask with a precision glass stirrer and a reflux condenser. The apparatus is inertized with nitrogen and the mixture is heated to 80° C. Subsequently, the SiH-functionalized siloxane is metered in according to the composition specified in Table 2. The ratio of allyl polyether / allyl hydrocarbon to SiH-functionalized siloxane is selected so that 1.4 moles of double bonds from allyl polyether / allyl hydrocarbon are present per mole of SiH functional group. An exothermic reaction begins. Cooling is used to keep the temperature below 110° C. The reaction mixture is then stirred at 100° C. for 3 hours. A clear to slightly turbid product is always obtained.
[0108] The polyether siloxanes corresponding to Formula 1 and Formula 2 shown in Table 2 were prepared and tested for performance. For PES 1 to 14, R = methyl, R 3 =–(CH 2 ) 3 – and h = 0. PES 1 to 3 are considered as comparative examples not according to the invention.
[0109] Table 2: Composition of polyether siloxane foam stabilizer (PES)
[0110]
[0111]
[0112] *For PES14, R 1 As follows: 50% Polyether 1, 25% Polyether 2 and 25% Hexadecyl.
[0113] Preparation of phenolic foam
[0114] For the comparison of properties, the formulations shown in Table 3 were used. The comparative foaming operation was carried out by manual mixing. For this purpose, the phenolic resin (amount per batch: 180 ± 5 g) and the foam stabilizer were weighed into a beaker and mixed with a disc stirrer (diameter 6 cm) at 20°C and 500 rpm for 15 minutes. The blowing agent was then added and the mixture was mixed at 1500 rpm for 30 seconds and then cooled to 18°C. The acid was then added and the mixture was stirred at 2000 rpm for 45 seconds and transferred to a 25 cm × 25 cm × 7 cm aluminum mold lined with a polyethylene film and maintained at 50°C by a thermostat. After 1 hour, the foam was demoulded and hardened in an oven heated to 60°C for 18 hours.
[0115] The pore structure was evaluated subjectively on a scale of 1 to 10, with 10 representing an (idealized) flawless, very fine foam and 1 representing a very clearly defective, coarse foam. The thermal conductivity (λ value in mW / m·K) was measured on 2.5 cm thick disks at an average temperature of 10° C. using an instrument of the Hesto Lambda Control type (type HLC X206) according to the specifications of standard EN 12667:2001. The density was determined according to ASTM D1622-20. The total emissions of the D4 and D5 cycles were measured in samples of dimensions 7x7x7 cm, expressed in toluene equivalent, according to DIN EN ISO 16000-9:2006, by the chamber method, sampling after 24 hours and evaluation according to DIN ISO 16000-6:2022.
[0116] The polyether siloxane foam stabilizers according to the invention were tested alone and in combination with alkoxylated castor oil. For this purpose, a 1.200 % suds stabilizer from Evonik Operations GmbH was used. CH 40 was used as the ethoxylated castor oil. The results are shown in Tables 3 and 4.
[0117] Table 3: Formulations for preparing phenolic foam
[0118]
[0119]
[0120] *Cellobond J6014L phenolic resin from Bakelite
[0121] Table 4: Properties of phenolic foam
[0122]
[0123] Table 4: Properties of phenolic foam
[0124]
[0125]
[0126]
[0127] The results show that with all foam stabilizers according to the invention, the same level of foam quality or slightly better can be achieved than with foam stabilizers not according to the invention. It is also shown that all foam stabilizers according to the invention achieve a clear improvement in the emissions of D4 and D5. The foam stabilizers according to the invention have only a negligible effect, if any, on all other application-relevant foam properties.
Claims
1. A composition for preparing a phenolic foam, comprising at least one phenolic resin, at least one blowing agent, at least one catalyst and at least one polyether siloxane of formula 1: M a M 1 b D c D 1 d (Formula 1) in a=0 to 2, b = 0 to 2, c=0 to 100, preferably 0 to 75, more preferably 0 to 50, d=1 to 100, preferably 1 to 75, more preferably 1 to 50, in a+b=2, a+b+c+d>4, preferably>7, (a+b+c+d) / (b+d)<5, preferably 1 to 4, more preferably 1 to 3, R = each independently the same or different alkyl group having 1 to 16 carbon atoms, the same or different aryl group having 6 to 16 carbon atoms, H or -OR 2 , preferably methyl, ethyl, phenyl or H, especially methyl, R 2 = each independently the same or different alkyl group having 1 to 16 carbon atoms, the same or different aryl group having 6 to 16 carbon atoms or H, R 1 = each independently the same or different alkyl radicals having 6 to 18 carbon atoms or the same or different polyether radicals, preferably the same or different alkyl radicals having 6 to 18 carbon atoms or the same or different polyether radicals of formula 2: R 3 = each independently the same or different divalent alkyl radical having 2 to 15 carbon atoms, preferably the same or different divalent alkyl radical having 3 to 6 carbon atoms, particularly preferably -(CH 2 ) 3 –, R 4 = each independently the same or different alkyl radicals having 1 to 18 carbon atoms and optionally having an ether function, or the same or different aryl radicals having 6 to 18 carbon atoms and optionally having an ether function, or H, preferably H, methyl, ethyl or benzyl, R 5 = each independently selected from the following identical or different groups: R 2 and C(O)R 2 , preferably methyl, butyl, H or C(O)Me, e=0 to 100, preferably 0 to 80, especially 0 to 60, f=0 to 100, preferably 0 to 80, in particular 0 to 60, g=0 to 100, preferably 0 to 80, especially 0 to 60, h=0 to 100, preferably 0 to 60, more preferably 0, where at least one of the values e, f, g and h is > 0, wherein not more than 50% of the polyether siloxane of formula 1 is R 1 The groups are each independently the same or different alkyl groups having 6 to 18 carbon atoms, and The total amount of the at least one polyether siloxane of Formula 1 is 0.1 to 20 parts by weight, preferably 0.5 to 10 parts by weight, and more preferably 0.5 to 8 parts by weight, based on 100 parts by weight of the total amount of the phenolic resin used.
2. The composition according to claim 1, It is characterized in that The at least one polyether siloxane of formula 1 is characterized in that, for R 1 , which contains at least one polyether group of formula 2, wherein: e = 6 to 16, f=g=h=0 or e+f+g=8 to 50, h=0, (f+g) / (e+f+g)>0 to 0.9, more preferably 0.1 to 0.
6.
3. The composition according to claim 1, It is characterized in that The at least one polyether siloxane of formula 1 is characterized in that, for R 1 , which contains at least two different polyether groups of the general formula 2, wherein at least one polyether corresponds to class 1 and at least one polyether corresponds to class 2, wherein: a=0 to 2, more preferably 2, b = 0 to 2, more preferably 0, c=0 to 10, preferably 0 to 5, more preferably 0, d = 1 to 80, preferably 1 to 50, more preferably 5 to 40, in a+b=2, a+b+c+d>4, preferably>7 and Category 1: e+f+g=10 to 60, more preferably 14 to 40, h=0, (f+g) / (e+f+g)≥0.6, more preferably≥0.8, especially=1, and Category 2: e = 6 to 16, f=g=h=0, or e+f+g=8 to 50, h=0, (f+g) / (e+f+g)>0 to 0.5, more preferably 0.1 to 0.3, And the preferred ratio of the first type of polyether to the second type of polyether in the polysiloxane is 10:90 to 90:10 weight percent, more preferably 20:80 to 80:20 weight percent, and especially 25:75 to 75:25 weight percent.
4. A composition according to any one of claims 1 to 3, It is characterized in that The at least one polyether siloxane of formula 1 is characterized in that it contains at least two different R 1 A group in which at least one R 1 The group is a polyether group of formula 2 and one R 1 The group is an alkyl group having 6 to 18 carbon atoms, wherein not more than 50% of the R 1 The group is an alkyl group having 6 to 18 carbon atoms.
5. The composition according to any one of claims 1 to 4, It is characterized in that The at least one blowing agent is selected from the group consisting of: - hydrocarbons having 3, 4 or 5 carbon atoms, preferably cyclopentane, isopentane and / or n-pentane, and - halogenated hydrocarbons having 3, 4 or 5 carbon atoms, preferably isopropyl chloride, hydrofluoroolefins and / or hydrohaloolefins, preferably 1234ze, 1234yf, 1224yd, 1233zd(E) and / or 1336mzz.
6. The composition according to any one of claims 1 to 5, It is characterized in that At least one silicon-free surfactant is additionally present in a total amount of 0.1 to 15 parts by weight, preferably 1 to 10 parts by weight, based on 100 parts by weight of the total amount of phenolic resin used.
7. A composition according to any one of claims 1 to 6, It is characterized in that It further comprises at least one alkoxylated, preferably ethoxylated, vegetable oil, preferably castor oil, in a total amount of 0.1 to 15 parts by weight, preferably 1 to 10 parts by weight, based on 100 parts by weight of the total amount of phenolic resin used.
8. A composition according to any one of claims 1 to 7, It is characterized in that The at least one catalyst is selected from the group consisting of organic acids and inorganic acids, preferably the at least one catalyst is selected from the group consisting of sulfuric acid, phosphoric acid, benzenesulfonic acid, xylenesulfonic acid, p-toluenesulfonic acid, ethylbenzenesulfonic acid, naphtholsulfonic acid, cumenesulfonic acid and phenolsulfonic acid.
9. The composition according to any one of claims 1 to 8, It is characterized in that The at least one catalyst is present in a total amount of 1 to 30 parts by weight, preferably 1 to 25 parts by weight, more preferably 3 to 20 parts by weight, based on 100 parts by weight of the total amount of phenolic resin used.
10. The composition according to any one of claims 1 to 9, It is characterized in that The at least one phenolic resin has a water content of 1% to 25% by weight, preferably 4% to 19% by weight, based on the total amount of phenolic resin used.
11. A method for preparing a phenolic foam, It is characterized in that The method is carried out by using a reaction mixture comprising a composition as defined in any one of claims 1 to 10.
12. Phenolic foam prepared according to the method of claim 11.
13. The phenolic foam according to claim 12, It is characterized in that The phenolic foam has a density of 5 to 500 kg / m 3 , preferably 10 to 200 kg / m 3 , particularly preferably 12 to 100 kg / m 3 .
14. Use of a phenolic foam according to any one of claims 12 and 13 for thermal insulation.
Citation Information
Patent Citations
Phenolic foam and method of manufacture thereof
AU2021238847A1
phenolic foam
DE602004006376T2
A process for producing phenolic foams
EP0170357A1
A process for producing phenolic foams
EP0170357B1
Phenolic foam
EP1922357A1