Lithium battery BOPP electrolyte-resistant adhesive tape and preparation method thereof

By using a specific combination of BOPP electrolyte-resistant tape in lithium battery packaging materials, the penetration risk of lithium battery packaging materials in the lithium battery electrolyte environment is solved, the electrolyte resistance and insulation performance are significantly improved, and the battery safety is enhanced sex.

CN118995062AInactive Publication Date: 2024-11-22SHENZHEN WANGLITONG ELECTRONIC TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411177469.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing lithium battery packaging materials are prone to penetration, swelling, and rupture in the environment of lithium battery electrolyte, resulting in electrolyte leakage, which in turn causes safety accidents, making it difficult to meet the high corrosion resistance requirements of lithium batteries for packaging materials.

Method used

It uses polypropylene resin, vinyl resin, epoxy resin curing agent, nitrite promoter, magnesium oxide filler, calcium carbonate filler, aluminum oxide filler, zinc oxide antioxidant, iron oxide antioxidant, polyurethane BOPP electrolyte-resistant tape with sealant, nano-silver preservative and other components is prepared by specific stirring and surface treatment methods, and is combined with BOPP film.

Benefits of technology

It significantly improves the electrolyte resistance and insulation performance of the tape, effectively prevents the penetration of the electrolyte, and enhances the safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995062A_ABST
    Figure CN118995062A_ABST
Patent Text Reader

Abstract

The invention discloses a lithium battery BOPP electrolyte-resistant adhesive tape and a preparation method thereof, and belongs to the technical field of adhesive tapes. The invention discloses an electrolyte-resistant adhesive tape. Comprising the following raw materials in parts by weight: 70-90 parts of polypropylene resin, 5-15 parts of vinyl resin, 5-20 parts of an epoxy resin curing agent, 1-5 parts of a nitrite accelerant, 1.5-10 parts of a magnesium oxide filling agent, 1.5-10 parts of a calcium carbonate filling agent, 1.5-10 parts of an aluminum oxide filling agent, 0.05-1 part of a zinc oxide antioxidant, 0.05-1 part of an iron oxide antioxidant, 5-10 parts of a polyurethane sealant, 0.01-0.03 part of a hydrogen peroxide catalyst and 0.01-0.03 part of an ozone catalyst. And 0.1 to 0.8 part of a nano-silver preservative. According to the invention, the BOPP film is further subjected to surface treatment, so that not only is the bonding performance of the BOPP film and the adhesive improved, but also the stability of the adhesive tape in the use process is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adhesive tapes, and in particular relates to a lithium battery BOPP electrolyte-resistant adhesive tape and a preparation method thereof. Background Art

[0002] With the urgent global demand for clean energy and sustainable development, lithium batteries, as an efficient and environmentally friendly energy storage device, have been widely used in electric vehicles, portable electronic devices, energy storage systems and other fields. However, the performance and safety of lithium batteries depend to a large extent on the performance of their packaging materials. In particular, the electrolyte of lithium batteries usually contains highly corrosive components such as organic solvents and lithium salts, which places extremely high demands on the corrosion resistance of packaging materials.

[0003] Traditional packaging materials, such as polyethylene (PE) and polypropylene (PP), show good performance under normal conditions, but often have problems such as penetration, swelling, and rupture under the action of lithium battery electrolyte, leading to electrolyte leakage, which in turn causes safety accidents such as battery short circuit, fire, and even explosion. Therefore, developing a packaging material that can withstand corrosion from lithium battery electrolyte is of great significance to improving the safety and reliability of lithium batteries.

[0004] As a high-performance packaging material, biaxially oriented polypropylene (BOPP) tape has been widely used in the packaging industry due to its excellent mechanical properties, chemical stability and good processing performance. BOPP tape has the characteristics of high strength, high transparency, low air permeability and low hygroscopicity, and is very suitable for lithium battery packaging. However, ordinary BOPP tape still has a certain penetration risk in the lithium battery electrolyte environment, and it is difficult to meet the high requirements of lithium batteries for packaging materials. Therefore, the present invention proposes a lithium battery BOPP electrolyte-resistant tape and a preparation method thereof to solve the problems existing in the prior art. Summary of the invention

[0005] The object of the present invention is to provide a lithium battery BOPP electrolyte resistant tape and a preparation method thereof, so as to solve the technical problem that the electrolyte resistance of lithium battery electrolyte packaging materials in the prior art is poor.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions: The invention provides a lithium battery BOPP electrolyte resistant tape. The electrolyte resistant tape comprises the following raw materials in parts by weight: 70-90 parts of polypropylene resin, 5.2-15 parts of vinyl resin, 5-20 parts of epoxy resin curing agent, 1-5 parts of nitrite accelerator, 1-7 parts of magnesium oxide filler, 1-7 parts of calcium carbonate filler, 2-14 parts of aluminum oxide filler, 0.05-1 parts of zinc oxide antioxidant, 0.05-1 parts of iron oxide antioxidant, 5-10 parts of polyurethane sealant, 0.01-0.03 parts of hydrogen peroxide catalyst, 0.01-0.03 parts of ozone catalyst and 0.08-0.23 parts of nano silver preservative.

[0007] The present invention also provides a method for preparing a lithium battery BOPP electrolyte-resistant adhesive tape, comprising the following steps: (1) preparing an adhesive: placing a vinyl resin into a mixing reactor, opening it, sequentially adding an epoxy resin curing agent, a nitrite accelerator, a hydrogen peroxide catalyst and an ozone catalyst, stirring and mixing them for the first time, then adding a magnesium oxide filler, a calcium carbonate filler, an aluminum oxide filler and a polyurethane sealant, stirring and mixing them for the second time, and finally adding a zinc oxide antioxidant, an iron oxide antioxidant and a nano silver preservative, stirring them evenly, and performing vacuum degassing to obtain an adhesive; (2) Preparation of BOPP film: placing polypropylene resin into a casting machine to obtain a biaxially oriented polypropylene (BOPP) film, and then treating the surface of the biaxially oriented polypropylene (BOPP) film, and then winding the film after the treatment to obtain a BOPP film; (3) Combined molding: The adhesive is applied to the back of the BOPP film to obtain a BOPP film coated with the adhesive, which is then combined with an anti-adhesive material to obtain a lithium battery BOPP electrolyte-resistant tape.

[0008] Furthermore, in step (1), the time for the first stirring and mixing and the second stirring and mixing are both 1 to 2 hours; the weight ratio of the magnesium oxide filler, the calcium carbonate filler and the aluminum oxide filler is 1:1:2; and the weight ratio of the vinyl resin to the nano silver preservative is 65:1.

[0009] Furthermore, in step (2), the surface of the BOPP film is treated by corona or plasma; the thickness of the BOPP film is 0.005-0.01 mm.

[0010] Furthermore, in step (3), the anti-sticking material is one of release paper or release film; the anti-sticking material is release paper or release film, and its thickness is 0.01~0.1mm.

[0011] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are: 1. The present invention uses vinyl resin as an adhesive, and adds epoxy resin curing agent, nitrite accelerator, hydrogen peroxide catalyst, ozone catalyst, magnesium oxide filler, calcium carbonate filler, aluminum oxide filler, polyurethane sealant, zinc oxide antioxidant, iron oxide antioxidant and nano silver preservative, so that the prepared adhesive has excellent electrolyte resistance and can meet the bonding requirements of electronic products in an electrolyte environment. When combined with a BOPP film, it can effectively prevent electrolyte penetration, so that the tape has excellent electrolyte resistance and further improves the safety performance of the battery.

[0012] 2. The present invention improves the bonding performance between the BOPP film and the adhesive by surface treatment of the BOPP film, thereby ensuring the stability of the tape during use. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0014] Figure 1 A preparation flow chart of a method for preparing a lithium battery BOPP electrolyte-resistant tape provided by an embodiment of the present invention; Figure 2 A schematic longitudinal section diagram of a lithium battery BOPP electrolyte-resistant tape provided in an embodiment of the present invention; Wherein, the figure marks are: 1: BOPP film; 2: adhesive; 3: anti-sticking material. DETAILED DESCRIPTION

[0015] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1

[0016] This embodiment discloses a lithium battery BOPP electrolyte-resistant tape, which includes: Figure 2 Shown are BOPP film 1, adhesive 2, and release material 3.

[0017] Specifically, the electrolyte resistant tape includes the following raw materials in parts by weight: 70 parts of polypropylene resin, 5.2 parts of vinyl resin, 5 parts of epoxy resin curing agent, 1 part of nitrite accelerator, 1 part of magnesium oxide filler, 1 part of calcium carbonate filler, 2 parts of aluminum oxide filler, 0.05 parts of zinc oxide antioxidant, 0.05 parts of iron oxide antioxidant, 5 parts of polyurethane sealant, 0.01 parts of hydrogen peroxide catalyst, 0.01 parts of ozone catalyst, and 0.08 parts of nano silver preservative.

[0018] This embodiment also discloses a method for preparing a lithium battery BOPP electrolyte-resistant tape, comprising the following steps: (1) Preparing an adhesive: placing a vinyl resin into a mixing reactor, opening it, and sequentially adding an epoxy resin curing agent, a nitrite accelerator, a hydrogen peroxide catalyst, and an ozone catalyst, stirring and mixing for the first time for 1 hour, then adding a magnesium oxide filler, a calcium carbonate filler, an aluminum oxide filler, and a polyurethane sealant, stirring and mixing for the second time for 1 hour, and finally adding a zinc oxide antioxidant, an iron oxide antioxidant, and a nano silver preservative, stirring evenly, and performing vacuum degassing to obtain an adhesive; (2) Preparation of BOPP film: placing polypropylene resin into a casting machine to obtain a biaxially oriented polypropylene BOPP film, and then treating the surface of the biaxially oriented polypropylene BOPP film by corona treatment, and then winding the film after treatment to obtain a BOPP film with a thickness of 0.005 mm; (3) Combination molding: The adhesive is coated on the back of the BOPP film to obtain a BOPP film coated with the adhesive, and then the BOPP film is combined with a release paper of an anti-adhesive material with a thickness of 0.01 mm to obtain a lithium battery BOPP electrolyte-resistant tape. Example 2

[0019] The present embodiment discloses a lithium battery BOPP electrolyte-resistant tape, which includes the following raw materials in parts by weight: 80 parts of polypropylene resin, 6.5 parts of vinyl resin, 6 parts of epoxy resin curing agent, 2 parts of nitrite accelerator, 1.5 parts of magnesium oxide filler, 1.5 parts of calcium carbonate filler, 3 parts of aluminum oxide filler, 0.06 parts of zinc oxide antioxidant, 0.06 parts of iron oxide antioxidant, 6 parts of polyurethane sealant, 0.01 parts of hydrogen peroxide catalyst, 0.02 parts of ozone catalyst, and 0.1 parts of nano silver preservative.

[0020] This embodiment also discloses a method for preparing a lithium battery BOPP electrolyte-resistant tape, comprising the following steps: (1) preparing an adhesive: placing a vinyl resin into a mixing reactor, opening it, and sequentially adding an epoxy resin curing agent, a nitrite accelerator, a hydrogen peroxide catalyst, and an ozone catalyst, and performing a first stirring and mixing process for 1.5 hours, then adding a magnesium oxide filler, a calcium carbonate filler, an aluminum oxide filler, and a polyurethane sealant, and performing a second stirring and mixing process for 1.5 hours, and finally adding a zinc oxide antioxidant, an iron oxide antioxidant, and a nano-silver preservative, stirring evenly, and performing vacuum degassing to obtain an adhesive; (2) Preparation of BOPP film: placing polypropylene resin into a casting machine to obtain a biaxially oriented polypropylene (BOPP) film, and then treating the surface of the biaxially oriented polypropylene (BOPP) film by corona treatment, and then winding the film after treatment to obtain a BOPP film with a thickness of 0.008 mm; (3) Combination molding: The adhesive is applied to the back of the BOPP film to obtain a BOPP film coated with the adhesive, and then the BOPP film is combined with an anti-adhesive release film, the thickness of the anti-adhesive material is 0.012 mm to obtain a lithium battery BOPP electrolyte resistant tape.

[0021] Example 3 The present embodiment discloses a lithium battery BOPP electrolyte-resistant tape, which includes the following raw materials in parts by weight: 90 parts of polypropylene resin, 15 parts of vinyl resin, 20 parts of epoxy resin curing agent, 5 parts of nitrite accelerator, 7 parts of magnesium oxide filler, 7 parts of calcium carbonate filler, 14 parts of aluminum oxide filler, 1 part of zinc oxide antioxidant, 1 part of iron oxide antioxidant, 10 parts of polyurethane sealant, 0.03 parts of hydrogen peroxide catalyst, 0.03 parts of ozone catalyst, and 0.23 parts of nano silver preservative.

[0022] This embodiment also discloses a method for preparing a lithium battery BOPP electrolyte-resistant tape, comprising the following steps: (1) preparing an adhesive: placing a vinyl resin into a mixing reactor, opening it, and sequentially adding an epoxy resin curing agent, a nitrite accelerator, a hydrogen peroxide catalyst, and an ozone catalyst, stirring and mixing for the first time for 2 hours, then adding a magnesium oxide filler, a calcium carbonate filler, an aluminum oxide filler, and a polyurethane sealant, stirring and mixing for the second time for 2 hours, and finally adding a zinc oxide antioxidant, an iron oxide antioxidant, and a nano silver preservative, stirring evenly, and performing vacuum degassing to obtain an adhesive; (2) Preparation of BOPP film: placing polypropylene resin into a casting machine to obtain a biaxially oriented polypropylene (BOPP) film, then treating the surface of the biaxially oriented polypropylene (BOPP) film by plasma, and then winding the film after treatment to obtain a BOPP film with a thickness of 0.01 mm; (3) Combination molding: The adhesive is coated on the back of the BOPP film to obtain a BOPP film coated with the adhesive, and then the BOPP film is combined with an anti-adhesive material release film with a thickness of 0.1 mm to obtain a lithium battery BOPP electrolyte-resistant tape.

[0023] Comparative Example 1 Compared with Example 2, in the process of preparing the lithium battery BOPP electrolyte-resistant tape in Comparative Example 1, no zinc oxide antioxidant and no iron oxide antioxidant were added, and other conditions remained unchanged.

[0024] Comparative Example 2 Comparative Example 2 Compared with Example 2, in the process of preparing the lithium battery BOPP electrolyte-resistant tape in Comparative Example 2, no nano silver preservative is added, and other conditions remain unchanged.

[0025] Experimental example The following performance tests were performed on the electrolyte-resistant tapes prepared in Examples 1-3 and Comparative Examples 1-2: 1. Electrolyte resistance test The electrolyte resistant tape was attached to aluminum foil at 80°C and immersed in electrolyte for 10 hours. The 180° peeling force of the electrolyte resistant tape before and after immersion was tested according to GB / T2792-2014 standard, and the retention rate of the 180° peeling force after immersion was calculated. The electrolyte was produced by Guangzhou Tianci Materials Co., Ltd.

[0026] 2. Insulation performance test The insulation resistance of the electrolyte resistant tape was tested according to the IEC 61215 standard. The tape was subjected to an aging test using a constant temperature and humidity aging test chamber. The damp heat aging conditions were set to 85% relative humidity, 85°C ambient temperature, and 1000h aging time. The insulation resistance of the tape was tested before and after aging, and the insulation resistance attenuation rate was calculated.

[0027] The results of electrolyte resistance test and insulation performance test are shown in Table 1: surface Figure 1

[0028] According to the test results in Table 1, it can be seen that the lithium battery BOPP electrolyte-resistant tape prepared in Examples 1-3 of the present invention significantly enhances the retention rate of the 180° peeling force after immersion and reduces the insulation resistance attenuation, that is, the electrolyte resistance and insulation performance of the tape are improved. By comparing Comparative Examples 1-2 with Examples 1-4, it can be seen that the addition of zinc oxide antioxidants, iron oxide antioxidants and nano-silver preservatives can improve the electrolyte resistance and insulation performance of the tape.

[0029] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

[0030] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. Lithium battery BOPP electrolyte resistant tape, characterized in that: The electrolyte-resistant adhesive tape comprises the following raw materials in parts by weight: 70-90 parts of polypropylene resin, 5.2-15 parts of vinyl resin, 5-20 parts of epoxy resin curing agent, 1-5 parts of nitrite accelerator, 1-7 parts of magnesium oxide filler, 1-7 parts of calcium carbonate filler, 2-14 parts of aluminum oxide filler, 0.05-1 parts of zinc oxide antioxidant, 0.05-1 parts of iron oxide antioxidant, 5-10 parts of polyurethane sealant, 0.01-0.03 parts of hydrogen peroxide catalyst, 0.01-0.03 parts of ozone catalyst, and 0.08-0.23 parts of nano silver preservative.

2. A method for preparing a lithium battery BOPP electrolyte-resistant tape, characterized in that: The steps include: (1) preparing an adhesive: placing a vinyl resin into a mixing reactor, opening it, sequentially adding an epoxy resin curing agent, a nitrite accelerator, a hydrogen peroxide catalyst and an ozone catalyst, stirring and mixing them for the first time, then adding a magnesium oxide filler, a calcium carbonate filler, an aluminum oxide filler and a polyurethane sealant, stirring and mixing them for the second time, and finally adding a zinc oxide antioxidant, an iron oxide antioxidant and a nano silver preservative, stirring them evenly, and performing vacuum degassing to obtain an adhesive; (2) Preparation of BOPP film: placing polypropylene resin into a casting machine to obtain a biaxially oriented polypropylene (BOPP) film, and then treating the surface of the biaxially oriented polypropylene (BOPP) film, and then winding the film after the treatment to obtain a BOPP film; (3) Combined molding: The adhesive is applied to the back of the BOPP film to obtain a BOPP film coated with the adhesive, which is then combined with an anti-adhesive material to obtain a lithium battery BOPP electrolyte-resistant tape.

3. The method for preparing the lithium battery BOPP electrolyte resistant tape according to claim 2, characterized in that: In step (1), the time for the first stirring and mixing and the second stirring and mixing are both 1 to 2 hours.

4. The method for preparing the lithium battery BOPP electrolyte resistant tape according to claim 2, characterized in that: In step (1), the weight ratio of the magnesium oxide filler, the calcium carbonate filler and the aluminum oxide filler is 1:1:

2.

5. The method for preparing the lithium battery BOPP electrolyte resistant tape according to claim 2, characterized in that: In step (1), the weight ratio between the vinyl resin and the nano silver preservative is 65:

1.

6. The method for preparing the lithium battery BOPP electrolyte resistant tape according to claim 2, characterized in that: In step (2), the surface of the BOPP film is treated by corona or plasma; the thickness of the BOPP film is 0.005~0.01mm.

7. The method for preparing the lithium battery BOPP electrolyte resistant tape according to claim 2, characterized in that: In step (3), the anti-sticking material is a release paper or a release film.

8. The method for preparing the lithium battery BOPP electrolyte resistant tape according to claim 2, characterized in that: In step (3), the thickness of the anti-sticking material is 0.01-0.1 mm.