Ethylene polymerization catalyst system
By using a catalyst system with porous support materials and metallocene compounds in ethylene polymerization, the problem of difficult ethylene polymerization catalysts in the prior art is solved, and the mechanical properties and density of polyethylene are improved, and the membrane is satisfied. High quality demand for manufacturing.
Patent Information
- Application Number
- CN202380033484.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-14
- Filing Date
- 2023-04-07
- Publication Date
- 2024-11-22
AI Technical Summary
The existing ethylene polymerization catalyst system is difficult to achieve high productivity, high monomer conversion and prevent reactor scaling at the same time, while meeting the high mechanical properties and density requirements of polyethylene films.
A porous support material is used as the support of the catalyst system, including a metallocene compound and methylaluminoxane of a specific structure, and a catalyst is prepared through specific compositional ratios and process steps for polymerization of ethylene.
High-efficiency ethylene polymerization is achieved, the molecular weight distribution and mechanical properties of polyethylene are improved, the use of catalyst amount is reduced, the reactor is prevented, and the high-quality requirements of membrane manufacturing are met.
Smart Images

Figure CN119013313A_ABST
Abstract
Description
[0001] The present invention relates to a catalyst system for the polymerization of ethylene. The present invention further relates to a process for preparing such a catalyst system. The present invention also relates to a process for the polymerization of ethylene using such a catalyst system.
[0002] As is well known, polymers produced from ethylene are the most versatile polymer materials available. They can be produced in an economical manner with high and consistent product quality and, by varying inter alia the polymerization conditions and the feedstock formulation, in various grades (each grade meeting certain application requirements), suitable for use in the production of a wide variety of articles.
[0003] Such polymer produced by ethylene, also referred to as polyethylene, can be a homopolymer of ethylene, or can use other monomers other than ethylene as a part of the raw material preparation for polymerization reaction to produce in some cases. Typical other monomers are referred to as comonomers, and can include alpha-olefins, particularly alpha-olefins with 3 to 10 carbon atoms. Such alpha-olefins comprising 3 to 10 carbon atoms can be selected from propylene, 1-butene, 1-pentene, 1-hexene, 1-octene and 4-methyl-1-pentene. The particularly suitable compound to be used as comonomer is 1-butene, 1-hexene and 1-octene.
[0004] In the ethylene-α-olefin copolymer according to the present invention, a single comonomer can be used, or a combination of multiple comonomers can be used. Preferably, a single comonomer is used. Therefore, preferably, the ethylene-α-olefin copolymer according to the present invention comprises a structural part derived from ethylene and a structural part derived from a single comonomer.
[0005] Among the particular types of applications where polyethylene is widely used is in films and laminates of films. There are various techniques for making films from polyethylene, including cast film production, blown film production and oriented film production. In each of these techniques, the polyethylene material is first placed in a molten state, and then the molten material is converted into a film shape and solidified, typically by forcing the molten material through a die having such a size to allow the desired film to be obtained from the method, and then cooled to below the melting point to solidify the film.
[0006] In order to adequately manufacture such films and ensure that the films meet the desired properties, stringent conditions are set for the characteristics of the polyethylene material. Current trends in polyethylene film applications, such as the combination of increased production speeds, smaller film reductions to reduce the amount of material used, and increased mechanical property requirements, have become a driving force for the polymer industry to continue to develop polyethylene materials that meet these standards.
[0007] One particular aspect of ethylene polymerization that reflects the properties of the polymer produced and the efficiency of the polymerization process is the catalyst system used in the polymerization.
[0008] A particular family of catalysts that may be suitable for use in the production of polyethylene via a catalytic polymerization process are the so-called single-site catalysts, a well-known group of which are the catalysts known as metallocene catalysts. While such catalysts are widely used in the manufacture of polyethylene products, there continues to be a desire to develop catalysts that allow the production of polymers having desired properties, such as desired density, molecular weight distribution (M), and molecular weight distribution (MWD). w / M n ) and high molecular weight M w A catalyst system for producing polyethylene which can polymerize at a high productivity, a high monomer conversion rate per amount of catalyst supplied, and wherein reactor fouling due to excessive heat generation is prevented.
[0009] According to the present invention, this is now provided by a catalyst system for the polymerization of ethylene comprising a porous support material, wherein the support material comprises, preferably on its surface and in its pores:
[0010] (i) a certain amount of compound (a) of formula (I)
[0011]
[0012] in:
[0013] ●Z is selected from MX 2 wherein X is selected from halogen, alkyl, aryl and aralkyl, and wherein M is selected from Zr, Hf and Ti;
[0014] ●R2 is a silane bridging structure;
[0015] ● each of R1, R1', R3, R3', R4, R4', R5 and R5' is hydrogen or a hydrocarbon moiety containing 1 to 20 carbon atoms; and
[0016] (ii) a certain amount of methylaluminoxane;
[0017] Wherein, the catalyst system comprises:
[0018] ≥2.5×10 -5 mol / g, preferably ≥2.5×10 -5 and ≤10.0×10 -5 mol / g, more preferably ≥2.7×10 -5 and ≤10.0×10 -5 mol / g of M, relative to the total weight of the catalyst system, and
[0019] ≥ 5.0 wt. %, preferably ≥ 5.0 and ≤ 20.0 wt. %, of aluminum, relative to the total weight of the catalyst system.
[0020] The silane bridging moiety may, for example, be a moiety of the formula:
[0021]
[0022] Wherein each structural part R12 is a hydrocarbon group, preferably a C1-C4 alkyl group. For example, each R12 can be a structural part selected from methyl, ethyl, n-propyl, isopropyl, n-butyl or isobutyl, preferably each R12 is a methyl structural part. The silane bridging structural part is preferably a dimethylsilane structural part.
[0023] The catalyst system may, for example, comprise preferably ≥5.0 and ≤10.0 wt. % aluminum, relative to the total weight of the catalyst system.
[0024] Compound (a) may be a compound of the following formula:
[0025]
[0026] Wherein, each R13 is hydrogen or a hydrocarbon structure containing 1 to 20 carbon atoms.
[0027] Preferably, compound (a) comprises a (2,3,4,5-tetramethyl-1-cyclopentadienyl) group bridged to a 1-indenyl group via a dihydrocarbylsilyl bridge, the 1-indenyl group being substituted by one or more substituents. R12 is preferably a C1-C4 alkyl group, most preferably a methyl group.
[0028] In a preferred embodiment, R1 is selected from isopropyl, phenyl, 3,5-dialkyl-1-phenyl, preferably 3,5-dimethyl-1-phenyl, 3,5-diethyl-1-phenyl, 3,5-diisopropyl-1-phenyl or 3,5-di-tert-butyl-1-phenyl. For example, R1 can be isopropyl or phenyl. For example, R1 can be isopropyl. For example, R1 can be phenyl.
[0029] Compound (a) is preferably a compound according to the following formula:
[0030]
[0031] More preferably, compound (a) is a compound according to the following formula:
[0032]
[0033] wherein R14 and R15 are selected from H and C1-C10 alkyl groups. Most preferably, R14 and R15 are selected from H, methyl, ethyl, propyl, isopropyl or tert-butyl groups. Most preferably, each R13 is H.
[0034] Preferably, X is Cl.
[0035] The catalyst system may, for example, comprise an amount of complex (b) obtained by reacting an amount of an aluminum compound of formula (II) with an amount of an amine compound of formula (III) in a hydrocarbon solvent;
[0036]
[0037] wherein R6 is hydrogen or a hydrocarbon moiety containing 1 to 30 carbon atoms; each R7 and R8 are the same or different and are hydrocarbon moieties containing 1 to 30 carbon atoms; R9 is hydrogen or a functional moiety containing at least one active hydrogen; R10 is hydrogen or a hydrocarbon moiety containing 1 to 30 carbon atoms; and R11 is a hydrocarbon moiety containing 1 to 30 carbon atoms. Preferably, complex (b) is a triisobutylaluminum / cyclohexylamine complex.
[0038] The porous support material may be selected, for example, from cross-linked polystyrene or functionalized polystyrene, polyvinyl chloride, cross-linked polyethylene, silica, MgCl 2 , talc and zeolite, preferably wherein the support material has an average particle size of 1 to 120 μm, more preferably 20 to 80 μm, even more preferably 40 to 50 μm. Preferably, the porous support material is silica. Preferably, the porous support material comprises ≤ 0.1 wt. % aluminum relative to the weight of the porous support material, more preferably the porous support material contains no aluminum.
[0039] In the catalyst system according to the present invention, it is preferred that the molar ratio of methylaluminoxane to compound (a) is ≥50 and ≤500, preferably ≥100 and ≤300, more preferably ≥150 and ≤300.
[0040] In the catalyst system according to the invention, it is preferred that the weight ratio of methylaluminoxane to support material is ≥0.1 and ≤0.8, preferably ≥0.2 and ≤0.6, more preferably ≥0.3 and ≤0.6.
[0041] In the catalyst system according to the invention, it is preferred that the weight ratio of compound (a) to support material is ≥0.005 and ≤0.08, preferably ≥0.01 and ≤0.05, more preferably ≥0.01 and ≤0.03.
[0042] Preferred compounds (a) that can be used in the catalyst system according to the present invention can be selected from:
[0043] ● dichloro[[(1,2,3,3a,7a-η)-2-(1-methylethyl)-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-zirconium;
[0044] ● dichloro[[(1,2,3,3a,7a-η)-2-phenyl-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-zirconium;
[0045] ● dichloro[[(1,2,3,3a,7a-η)-2-methyl-4-phenyl-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-zirconium;
[0046] ● dichloro[[(1,2,3,3a,7a-η)-3-phenyl-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-zirconium;
[0047] ● dichloro[[(1,2,3,3a,7a-η)-2-phenyl-3-methyl-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-zirconium;
[0048] ● dichloro[[(1,2,3,3a,7a-η)-2-phenyl-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,3a,7a-η)-1H-inden-2-ylidene]]-zirconium;
[0049] ● dichloro[[(1,2,3,3a,7a-η)-2-(3,5-dimethylphenyl)-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,3a,7a-η)-1,3-dimethyl-1H-inden-2-ylidene]]-zirconium;
[0050] ● dichloro[[(1,2,3,3a,7a-η)-2-tert-butyl-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,3a,7a-η)-1,3-dimethyl-1H-inden-2-ylidene]]-zirconium;
[0051] ● dichloro[[(1,2,3,3a,7a-η)-1H-inden-2-ylidene](dimethylsilylene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-zirconium;
[0052] ● dichloro[[(1,2,3,3a,7a-η)-2-(1-methylethyl)-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,3a,7a-η)-1,3-dimethyl-1H-inden-2-ylidene]]-zirconium;
[0053] ● dichloro[[(1,2,3,3a,7a-η)-2-phenyl-3-methyl-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,3a,7a-η)-1,3-dimethyl-1H-inden-2-ylidene]]-zirconium;
[0054] ● [[(1,2,3,3a,7a-η)-2-(1-methylethyl)-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-hafnium; and
[0055] ●Dichloro[[(1,2,3,3a,7a-η)-2-phenyl-1H-inden-1-ylidene](dimethylsilanylidene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-hafnium.
[0056] Particularly preferably, compound (a) is selected from
[0057] ● dichloro[[1,2,3,3a,7a-η)-2-(1-methylethyl)-1H-inden-1-ylidene](dimethylsilanylidene)[1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-zirconium;
[0058] ● dichloro[[(1,2,3,3a,7a-η)-2-phenyl-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-zirconium;
[0059] ● dichloro[[(1,2,3,3a,7a-η)-2-methyl-4-phenyl-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-zirconium;
[0060] ● dichloro[[(1,2,3,3a,7a-η)-3-phenyl-1H-inden-1-ylidene](dimethylsilanylidene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-zirconium; and
[0061] ●Dichloro[[(1,2,3,3a,7a-η)-2-phenyl-3-methyl-1H-indene-1-ylidene](dimethylsilylene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-zirconium dichloride.
[0062] In compound (a), moieties R4 and R5 may be fused to form a ring structure, and / or moieties R4' and R5' may be fused to form a ring structure, and / or moieties R3 and R4 may be fused to form a ring structure, and / or moieties R3' and R4' may be fused to form a ring structure. When such moieties are fused to form a ring structure, it is preferred that the formed ring structure forms an indenyl structure together with the pentadienyl moiety. Such an indenyl structure may be substituted or unsubstituted.
[0063] An embodiment of the present invention also relates to a process for preparing the catalyst system according to the present invention, wherein the process comprises the following steps in this order:
[0064] (i) preparing a first mixture by reacting an amount of compound (a) with an amount of methylaluminoxane as a solution in a hydrocarbon solvent, preferably at a temperature of 20-80° C. for a period of 0.1-2.0 hours;
[0065] (ii) preparing a second mixture by reacting a certain amount of triisobutylaluminum with a certain amount of cyclohexylamine in a hydrocarbon solvent;
[0066] (iii) providing an amount of support material into a reaction vessel;
[0067] (iv) providing a certain amount of hydrocarbon solvent into the reaction vessel;
[0068] (v) supplying the first mixture and the second mixture to a reaction vessel;
[0069] (vi) subjecting the contents of the reaction vessel to a temperature of >60°C for a period of >3 hours, preferably >3 hours and <10 hours, to obtain the catalyst system; and
[0070] (vii) Removal of hydrocarbon solvent from the catalyst system.
[0071] Preferably, the temperature in step (vi) is >90°C, more preferably >90°C and <110°C.
[0072] The present invention also relates to a process for the polymerization of ethylene, wherein the polymerization is carried out in the presence of a catalyst system according to the invention or a catalyst system produced by the process according to the invention.
[0073] In a certain embodiment, the present invention also relates to a polyethylene composition comprising the catalyst system of the present invention, preferably wherein the polyethylene composition comprises polyethylene and the catalyst system of the present invention.
[0074] The invention will now be illustrated by the following non-limiting examples.
[0075] Material
[0076] The following materials were used in the experiments to demonstrate the present invention. All materials were handled using Schlenk techniques or a nitrogen-filled glove box under nitrogen atmosphere. 955W silica (available from WR Grace & Co.). Methylaluminoxane (MAO) was used as a 10 wt % solution in toluene (available from WR Grace & Co.). As compound (a), dimethylsilyl (2,3,4,5-tetramethylcyclopentadienyl) (2-isopropyl-inden-1-yl) zirconium chloride, CAS Reg. No. 2247072-26-8, was used. Triisobutylaluminum (TIBAL) was purchased from Sigma-Aldrich. Toluene (HPLC grade, 99.9%) and cyclohexylamine (99.9%) were purchased from Sigma-Aldrich and purged with nitrogen before use. A mixture of TIBAL and cyclohexylamine in hexane ( PA 4276, purchased from Lanxess) was used for polymerization experiments.
[0077] Catalyst system preparation
[0078] The support was pre-dehydrated at 600°C for 4 hours. Under a nitrogen atmosphere, 2.5 g of the pre-dehydrated support was loaded into a 100 ml double-necked Schlenk flask in a glove box, followed by the addition of 15 ml of toluene. After shaking, a suspension was obtained. A given amount of compound (a) (also referred to as metallocene) was activated by mixing with a given amount of MAO in toluene in a 25 ml vial at room temperature (23°C) in a glove box for 10 minutes. The amounts of compound (a) and MAO used in the examples are shown in the table below.
[0079] Example A1 A2 A3 A4 B1 B2 Metallocene(g) 0.020 0.030 0.042 0.080 0.022 0.034 MAO solution (ml) 5.9 6.0 6.0 6.1 9.9 10.0 Example B3 B4 C1 C2 C3 C4 Metallocene(g) 0.047 0.090 0.024 0.036 0.050 0.096 MAO solution (ml) 10.0 10.2 12.3 12.4 12.4 12.6
[0080] The activated metallocene is transferred to the suspension. 0.0064 g of TIBAL and 0.0032 g of cyclohexylamine are mixed in 10 ml toluene in another 25 ml vial at room temperature (23° C.) in a glove box for 10 min and then transferred to the suspension. The final mixture is heated to 95° C. and maintained at this temperature for 5 hours. Subsequently, the product is dried at 75° C. under vacuum to obtain a catalyst system, which is isolated as a free-flowing powder.
[0081] Example A1 A2 A3 A4 B1 B2 Zr (wt%) 0.12 0.18 0.249 0.473 0.12 0.18 <![CDATA[Zr(×10 -5 mol / g catalyst)]]> 1.31 1.97 2.73 5.19 1.31 1.97 Al (wt%) 8.0 8.0 8.0 8.0 12.0 12.0 <![CDATA[Al(×10 -2 mol / g catalyst)]]> 0.30 0.30 0.30 0.30 0.44 0.44 Molar ratio Al / Zr 226 150 109 57 338 225 Example B3 B4 C1 C2 C3 C4 Zr (wt%) 0.249 0.473 0.12 0.18 0.249 0.473 <![CDATA[Zr(×10 -5 mol / g catalyst)]]> 2.73 5.19 1.31 1.97 2.73 5.19 Al (wt%) 12.0 12.0 14.0 14.0 14.0 14.0 <![CDATA[Al(×10 -2 mol / g catalyst)]]> 0.44 0.44 0.52 0.52 0.52 0.52 Molar ratio Al / Zr 163 86 396 262 190 100
[0082] Polymerization experiment: Ethylene homopolymerization
[0083] A 1.6 l stainless steel reactor vessel equipped with a helical stirrer and a heating / cooling control unit was heated to 110° C. for 2 hours at a nitrogen flow rate of 100 g / h. The reactor was then purged with nitrogen pressure and then with ethylene. This purge cycle was repeated three times.
[0084] The reactor was then cooled to 88° C. under ethylene pressurized to 10 bar. After venting, 4 ml of PA 4276. Nitrogen was introduced to maintain a nitrogen pressure of 8 bar. Ethylene was then introduced into the reactor under control of mass flow parameters to maintain the ethylene pressure in the reactor at 10 bar. After reaching a stable temperature and pressure level, 80 mg of the catalyst system was injected via a catalyst injection pump and the reaction was started. After 1 hour, the ethylene supply was stopped and the reactor was cooled to 40°C. The reactor was opened after venting. The polyethylene product was collected in a sample tray and dried at ambient temperature under atmospheric pressure.
[0085] experiment catalyst Productivity (g PE / g catalyst) BD <![CDATA[M n ]]> <![CDATA[M w ]]> <![CDATA[M w / M n ]]> D1 A1 297 0.238 90 270 3.00 D2 A2 312 0.267 85 257 3.01 D3 A3 349 0.260 86 243 2.84 D4 A4 393 0.270 78 236 3.01 D5 B1 316 0.297 81 243 2.99 D6 B2 358 0.327 72 224 3.11 D7 B3 520 0.331 67 206 3.05 D8 B4 651 0.315 66 216 3.26 D9 C1 329 0.324 75 221 2.94 D10 C2 424 0.351 68 214 3.16 D11 C3 533 0.348 67 203 3.04 D12* C4 683 0.330 82 253 3.08
[0086] in:
[0087] The productivity is the amount of polyethylene (PE) obtained per amount of catalyst supplied, expressed as g PE / g catalyst;
[0088] ●BD is the bulk density, in g / cm 3 It means that it is measured according to ASTM D1895-17;
[0089] ●Weight average molecular weight (M w ) and number average molecular weight (M n ) is expressed in kg / mol and is determined according to ASTM D6474 (2012)
[0090] * In experiment D12, the amount of catalyst system supplied was 40 mg to prevent agglomerate formation in the reactor and reactor overheating, which was caused by high catalyst productivity.
[0091] The catalyst containing a relatively low content of Al (D1) shows high initial activity and low peak activity, while the catalysts containing a relatively high content of Al (D5 and D9) show low initial activity and high peak activity as well as high overall activity, which is preferred for gas phase olefin polymerization processes.
[0092] Polymerization experiment: Ethylene / 1-hexene copolymerization
[0093] A 1.6 l stainless steel reactor vessel equipped with a helical stirrer and a heating / cooling control unit was heated to 110° C. for 2 hours at a nitrogen flow rate of 100 g / h. The reactor was then purged with nitrogen pressure and then with ethylene. This purge cycle was repeated three times.
[0094] The reactor was then cooled to 88°C under ethylene pressurized to 10 bar. After venting, 4 ml of PA 4276. Nitrogen was introduced to maintain a nitrogen pressure of 8 bar. Ethylene and 1-hexene were then introduced into the reactor in the given molar ratios in the table below while controlling the mass flow parameters to maintain a total pressure of 10 bar for ethylene and 1-hexene in the reactor. After reaching a stable temperature and pressure level, 80 mg of the catalyst system was injected via a catalyst injection pump and the reaction was started. After 1 hour, the ethylene and 1-hexene supply was stopped and the reactor was cooled to 40° C. The reactor was opened after venting. The polyethylene product was collected in a sample tray and dried at ambient temperature under atmospheric pressure.
[0095]
[0096]
[0097] The concepts in this table are as defined in the section related to homopolymerization experiments, except that:
[0098] C6 / C2 is the molar ratio of 1-hexene to ethylene in the reactor feed; and
[0099] • Density is the density of the polyethylene product measured according to ASTM D1505-18.
[0100] * In experiments D25-D30 and D34-D39, the amount of catalyst system supplied was 40 mg to prevent agglomerate formation in the reactor and reactor overheating, which was caused by high catalyst productivity.
Claims
1. A catalyst system for the polymerization of ethylene comprising a porous support material, wherein the support material preferably comprises on its surface and in its pores: (i) a certain amount of compound (a) of formula (I) in: ● Z is a moiety selected from M-X2, wherein X is selected from halogen, alkyl, aryl and aralkyl, and wherein M is selected from Zr, Hf and Ti; ●R2 is a silane bridging structure; ● each of R1, R1', R3, R3', R4, R4', R5 and R5' is hydrogen or a hydrocarbon moiety containing 1 to 20 carbon atoms; and (ii) a certain amount of methylaluminoxane; Wherein, the catalyst system comprises: ≥2.5×10 -5 mol / g, preferably ≥2.5×10 -5 and ≤10.0×10 -5 mol / g, more preferably ≥2.7×10 -5 and ≤10.0×10 -5 mol / g of M, relative to the total weight of the catalyst system, and ≥ 5.0 wt. %, preferably ≥ 5.0 and ≤ 20.0 wt. %, of aluminum, relative to the total weight of the catalyst system.
2. The catalyst system according to claim 1, wherein the silane bridging moiety is a moiety of the following formula: in, Each moiety R12 is a hydrocarbon group, preferably a C1-C4 alkyl group.
3. The catalyst system of claim 2, wherein each R12 is a moiety selected from methyl, ethyl, n-propyl, isopropyl, n-butyl or isobutyl.
4. The catalyst system according to any one of claims 1 to 3, wherein the silane bridging moiety is a dimethylsilane moiety.
5. The catalyst system according to any one of claims 1 to 4, wherein the catalyst system comprises an amount of complex (b) obtained by reacting an amount of an aluminum compound of formula (II) with an amount of an amine compound of formula (III) in a hydrocarbon solvent; in, R6 is hydrogen or a hydrocarbon moiety containing 1 to 30 carbon atoms; each R7 and R8 is the same or different and is a hydrocarbon moiety containing 1 to 30 carbon atoms; R9 is hydrogen or a functional moiety containing at least one active hydrogen; R10 is hydrogen or a hydrocarbon moiety containing 1 to 30 carbon atoms; R11 is a hydrocarbon moiety containing 1 to 30 carbon atoms.
6. The catalyst system according to claim 5, wherein the complex (b) is a triisobutylaluminum / cyclohexylamine complex.
7. The catalyst system according to any one of claims 1 to 6, wherein the porous support material is selected from crosslinked polystyrene or functionalized polystyrene, polyvinyl chloride, crosslinked polyethylene, silica, MgCl2, talc and zeolites, preferably wherein the support material has an average particle size of 1 to 120 μm, more preferably 20 to 80 μm, even more preferably 40 to 50 μm.
8. The catalyst system according to any one of claims 1 to 7, wherein ● the molar ratio of the methylaluminoxane to the compound (a) is ≥50 and ≤500, preferably ≥100 and ≤300, more preferably ≥200 and ≤300; and / or ● the weight ratio of the methylaluminoxane to the support material is ≥0.1 and ≤0.8, preferably ≥0.2 and ≤0.6, more preferably ≥0.3 and ≤0.6; and / or The weight ratio of the compound (a) to the support material is ≥0.005 and ≤0.08, preferably ≥0.01 and ≤0.05, more preferably ≥0.01 and ≤0.
03.
9. The catalyst system according to any one of claims 1 to 8, wherein the porous support material comprises ≤ 0.1 wt.-% aluminum, relative to the weight of the porous support material, preferably wherein the porous support material is free of aluminum.
10. The catalyst system according to any one of claims 1 to 9, wherein the compound (a) is selected from: ● dichloro[[(1,2,3,3a,7a-η)-2-(1-methylethyl)-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-zirconium; ● dichloro[[(1,2,3,3a,7a-η)-2-phenyl-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-zirconium; ● dichloro[[(1,2,3,3a,7a-η)-2-methyl-4-phenyl-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-zirconium; ● dichloro[[(1,2,3,3a,7a-η)-3-phenyl-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-zirconium; ● dichloro[[(1,2,3,3a,7a-η)-2-phenyl-3-methyl-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-zirconium; ● dichloro[[(1,2,3,3a,7a-η)-2-phenyl-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,3a,7a-η)-1H-inden-2-ylidene]]-zirconium; ● dichloro[[(1,2,3,3a,7a-η)-2-(3,5-dimethylphenyl)-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,3a,7a-η)-1,3-dimethyl-1H-inden-2-ylidene]]-zirconium; ● dichloro[[(1,2,3,3a,7a-η)-2-tert-butyl-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,3a,7a-η)-1,3-dimethyl-1H-inden-2-ylidene]]-zirconium; ● dichloro[[(1,2,3,3a,7a-η)-1H-inden-2-ylidene](dimethylsilylene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-zirconium; ● dichloro[[(1,2,3,3a,7a-η)-2-(1-methylethyl)-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,3a,7a-η)-1,3-dimethyl-1H-inden-2-ylidene]]-zirconium; ● dichloro[[(1,2,3,3a,7a-η)-2-phenyl-3-methyl-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,3a,7a-η)-1,3-dimethyl-1H-inden-2-ylidene]]-zirconium; ● [[(1,2,3,3a,7a-η)-2-(1-methylethyl)-1H-inden-1-ylidene](dimethylsilylene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-hafnium; and ●Dichloro[[(1,2,3,3a,7a-η)-2-phenyl-1H-inden-1-ylidene](dimethylsilanylidene)[(1,2,3,4,5-η)-2,3,4,5-tetramethyl-2,4-cyclopentadien-1-ylidene]]-hafnium.
11. The catalyst system according to any one of claims 1 to 10, wherein the moieties R4 and R5 are fused to form a ring structure, and / or wherein the moieties R4' and R5' are fused to form a ring structure, and / or wherein the moieties R3' and R4' are fused to form a ring structure, and / or wherein the moieties R3 and R4 are fused to form a ring structure.
12. A process for preparing a catalyst system according to any one of claims 1 to 11, wherein the process comprises the following steps in this order: (i) preparing a first mixture by reacting a certain amount of compound (a) with a certain amount of said methylaluminoxane as a solution in a hydrocarbon solvent, preferably at a temperature of 20-80° C. for a period of 0.1-2.0 hours; (ii) preparing a second mixture by reacting a certain amount of triisobutylaluminum with a certain amount of cyclohexylamine in a hydrocarbon solvent; (iii) providing a certain amount of the support material into a reaction vessel; (iv) providing a certain amount of hydrocarbon solvent into the reaction vessel; (v) supplying the first mixture and the second mixture to the reaction vessel; (vi) subjecting the contents of the reaction vessel to a temperature of >60°C for a period of >3 hours, preferably >3 hours and <10 hours, to obtain a catalyst system; and (vii) removing the hydrocarbon solvent from the catalyst system.
13. The process according to claim 12, wherein the temperature in step (vi) is >90°C, more preferably >90°C and <110°C.
14. Process for the polymerisation of ethylene, wherein the polymerisation is carried out in the presence of a catalyst system according to any one of claims 1 to 11 or a catalyst system produced according to a process according to any one of claims 12 to 13.
15. A polyethylene composition comprising the catalyst system according to any one of claims 1 to 11.