Polycarbonate / polyester compositions and parts with high comparative tracking index

CN119013350APending Publication Date: 2024-11-22COVESTRO DEUTSCHLAND AG
16 Cites 0 Cited by

Patent Information

Application Number
CN202380029177.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-16
Publication Date
2024-11-22

Smart Images

  • Figure BDA0005052421460000051
    Figure BDA0005052421460000051
  • Figure BDA0005052421460000052
    Figure BDA0005052421460000052
  • Figure BDA0005052421460000091
    Figure BDA0005052421460000091
Patent Text Reader

Abstract

The invention relates to compositions comprising A) 60 to 93% by weight of at least one aromatic polycarbonate, polyester carbonate or mixtures thereof, B) 2 to 20% by weight of a polyester based on aromatic or cycloaliphatic dicarboxylic acids or mixtures thereof and cyclohexanedimethanol and optionally other aliphatic glycols, C) 1 to 10% by weight of at least one flame retardant containing phosphorus, the invention also relates to a component comprising the composition and to the use of the components B and C in the indicated amounts for improving the CTI and flame retardancy of polycarbonate compositions.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to flame retardant polycarbonate / polyester compositions, parts comprising the compositions having a high comparative tracking index, and the use of specific polyesters and flame retardants for improving the comparative tracking index and flame retardancy of polycarbonate compositions.

[0002] Polycarbonate and polycarbonate blend compositions have been used for many years in numerous applications such as automotive construction, the electronics sector and the construction industry. Polycarbonate and polycarbonate blends are known for their high heat deformation resistance and high toughness. In particular, the choice and amount of the polymer blending partners make it possible to vary the overall property profile within a wide range and to adapt it to the respective requirements.

[0003] For electronic applications, good insulating properties and high flame retardancy are closely related to safety. Such requirements are also becoming increasingly important in the field of electric vehicles, for example. A high relative tracking index is also important if the polymer material is in direct contact with current-carrying components, such as conductor strips. Otherwise, leakage currents can cause the charge to be transferred over a greater distance via the plastic surface than directly through the air at the same voltage. This is the case even for materials that originally have high insulating properties, such as plastics. The tendency to form leakage currents should therefore be as low as possible in order to reduce the risk of short circuits and thus avoid fires. In addition, a high relative tracking index makes it possible to reduce the distance between, for example, electrical conductor strips, thereby achieving smaller component sizes or operating the components at higher operating voltages.

[0004] CTI ("Comparative Tracking Index") is a measure of the comparative tracking index of a plastic. It indicates to what extent a plastic surface can form a leakage current due to the influence of dirt or liquids when a voltage is applied. The higher the comparative tracking index, the more suitable the material is for parts that are subject to high voltages and / or that may become dirty or come into contact with moisture during use. CTI is expressed in volts and indicates the voltage below which no appreciable leakage current will occur when a certain amount of electrolyte solution is added.

[0005] Compared to other polymers such as polyethylene, polycarbonate has only a low comparative tracking index, with a CTI value of about 250 V. However, for some high-voltage applications such as in the field of electric vehicles, CTI values ​​of up to 600 V must be achieved. In addition, materials for such applications should have very high flame retardancy according to UL 94V, preferably a V0 rating at thin wall thicknesses such as 1.5 mm.

[0006] The flame retardancy of polycarbonate and polycarbonate blends is usually improved by adding flame retardants.

[0007] US2007 / 197722 A1 discloses a thermoplastic molding compound with improved impact resistance and flame retardancy, wherein the composition comprises (a) aromatic polycarbonate, (b) thermoplastic polyester, (c) halogenated acrylate, (d) impact modifier, (e) phosphorus-containing compound and (f) fluorinated polyolefin.

[0008] US 2012 / 231278 discloses a composition with improved flame retardancy for extrusion applications, which contains an aromatic polycarbonate, an acrylate-based scattering additive, a brominated flame retardant, and a phosphorus-based flame retardant.

[0009] However, some flame retardants increase the tendency of leakage current to form, which leads to an undesirable decrease in the CTI value. In addition, flame retardants generally have a negative impact on heat deformation resistance and toughness (such as impact toughness).

[0010] EP 3560997 A2 discloses a thermoplastic resin composition having excellent properties such as high CTI, comprising: (A) 100 parts by weight of polycarbonate; (B) 2 to 6 parts by weight of a cyclic phosphazene compound flame retardant; (C) 0.1 to 5 parts by weight of an impact modifier; and (D) 1 to 3 parts by weight of a fluorinated polyolefin.

[0011] US2012 / 0248384 A1 discloses polycarbonate compositions, methods and articles of manufacture that meet at least certain requirements for comparative tracking index. The compositions, methods and articles of manufacture that meet these requirements comprise at least polycarbonate, polysiloxane block copolycarbonate and a transition metal oxide, such as titanium dioxide.

[0012] The relationship between the burning behaviour (GWFI) and the comparative tracking index (CTI) is discussed in the publication “Glow wire ignition temperature (GWIT) and comparative tracking index (CTI) of glass fibre filled engineering polymers, blends and flame retarded formulations” (Polymer Degradation and Stability, Vol. 96, No. 12, December 2011, pp. 2098-2103).

[0013] It is also desirable to provide a polycarbonate composition that can be used to make molded articles, which has a combination of high CTI, high flame retardancy, high heat deformation resistance and toughness. In particular, it is desirable that the molded article has a CTI of 600V (preferably determined according to the rapid test method based on IEC 60112:2009 described in the Examples section), a UL 94V0 rating at 1.5mm, and further preferably also has a Vicat softening temperature of at least 105°C measured according to DIN ISO 306 (2013 Edition, Method B / 120), and no fracture in the Izod impact toughness test according to ISO 180-U (2019 Edition).

[0014] Surprisingly, it has been found that a composition has the desired properties, which comprises

[0015] A) 60 to 93% by weight, preferably 65 to 90% by weight, particularly preferably 70 to 90% by weight, of at least one aromatic polycarbonate, polyester carbonate or a mixture thereof,

[0016] B) 2 to 20% by weight, preferably 3 to 18% by weight, particularly preferably 4 to 16% by weight, of a polyester based on at least one aromatic or at least one cycloaliphatic dicarboxylic acid or a mixture thereof and cyclohexanedimethanol and optionally at least one further aliphatic diol,

[0017] C) 1 to 10% by weight, preferably 2 to 9% by weight, particularly preferably 3 to 9% by weight, of at least one phosphorus-containing flame retardant.

[0018] In addition to components A, B and C, the composition may also comprise one or more polymer additives, fillers and reinforcing agents, dyes, pigments, impact modifiers and / or polymers other than components A and B as blending partners as component D, wherein the amount of component D is preferably from 0.1 to 20% by weight, based on the composition.

[0019] The composition preferably consists of at least 90% by weight, further preferably at least 95% by weight, of components A to D. Particularly preferably, the composition consists of components A to D exclusively.

[0020] Another subject of the present invention is the use of 2 to 20% by weight of polyesters based on aromatic or cycloaliphatic dicarboxylic acids or mixtures thereof and cyclohexanedimethanol and optionally other aliphatic diols and 1 to 10% by weight of at least one phosphorus-containing flame retardant for improving the CTI and the flame retardancy according to UL 94 V of polycarbonate compositions, preferably for achieving a CTI of 600 V (preferably determined according to the rapid test method based on IEC 60112:2009 as described in the Examples section) and a UL 94 V0 rating at a specimen thickness of 1.5 mm for polycarbonate compositions comprising 60 to 93% by weight of polycarbonate.

[0021] Due to the good properties of the composition, it is also suitable for manufacturing components that have a small distance between the electrical conductor strips.

[0022] Accordingly, another subject matter of the present invention is a component, preferably an electrical / electronic component, which comprises

[0023] a first electrical conductor L1 and a second electrical conductor L2, which have a first distance d1 and a second distance d2 between each other,

[0024] which are connected by a thermoplastic material M in direct contact with the first electrical conductor and the second electrical conductor,

[0025] wherein the distance d1 is the shortest distance between the first electrical conductor and the second electrical conductor along the surface of the thermoplastic material M, and

[0026] wherein the distance d2 is the shortest distance between the first electrical conductor and the second electrical conductor through air,

[0027] wherein d2 is selected to prevent arcing through air at the respective operating voltage U of the component,

[0028] wherein d1 has the following values at the operating voltages U listed below:

[0029] d1(0V ≤ U ≤ 250V): 1.3 mm to <4.0 mm

[0030] d1(250V < U ≤ 500V) = 2.5 mm to <8.0 mm

[0031] d1(500V < U ≤ 1000V) = 5.0 mm to <16 mm

[0032] and wherein the thermoplastic material M comprises the following components

[0033] A) 60 to 93% by weight of at least one aromatic polycarbonate, polyester carbonate or a mixture thereof,

[0034] B) 2 to 20% by weight of a polyester based on at least one aromatic or at least one alicyclic dicarboxylic acid or a mixture thereof and cyclohexanedimethanol and optionally at least one other aliphatic diol,

[0035] C) 1 to 10% by weight of at least one phosphorus-containing flame retardant.

[0036] Preferably, the component is a component having an IP6K9K protection rating according to ISO 20653:2013, i.e., a protection rating against contact, foreign object intrusion and water. For such components, d1 has the following values at the operating voltages U listed below:

[0037] d1(0V ≤ U ≤ 250V): 1.3 mm to < 2.5 mm, more preferably 1.3 mm to < 1.8 mm

[0038] d1(250V < U ≤ 500V) = 2.5 mm to < 5.0 mm, more preferably 2.5 mm to < 3.6 mm

[0039] d1(500V < U ≤ 1000V) = 5.0 mm to < 10.0 mm, more preferably 5.0 mm to < 7.1 mm

[0040] Here, d2 is preferably at least 1.2 mm, more preferably 1.2 to 10.0 mm. A person skilled in the art can determine the distance to prevent arcing through air.

[0041] The features mentioned as preferred, particularly preferred, etc. for the composition also apply to the use according to the invention and the components according to the invention.

[0042] Component A

[0043] The aromatic polycarbonates and / or aromatic polyester carbonates of component A suitable according to the invention are known from the literature or can be prepared by methods known from the literature (for the preparation of aromatic polycarbonates, see, for example, Schnell, "Chemistry and Physics of Polycarbonates", Interscience Publishers, 1964 and DE-AS 1495626, DE-A 2232877, DE-A 2703376, DE-A 2714544, DE-A 3000610, DE-A 3832396; for the preparation of aromatic polyester carbonates, see, for example, DE-A 3007934).

[0044] Aromatic polycarbonates are prepared, for example, by the interfacial method through the reaction of diphenols with carbonyl halides (preferably phosgene) and / or aromatic dicarboxylic acid dihalides (preferably benzene dicarboxylic acid dihalides), where a chain terminator (such as a monophenol) is optionally used and a trifunctional or higher-functional branching agent (such as a triphenol or a tetraphenol) is optionally used. It can also be prepared by the melt polycondensation method through the reaction of diphenols with, for example, diphenyl carbonate.

[0045] The diphenols used for the preparation of aromatic polycarbonates and / or aromatic polyester carbonates are preferably diphenols of formula (1)

[0046]

[0047] where

[0048] A is a single bond, C1 to C5 alkylene, C2 to C5 alkylidene, C5 to C6 cycloalkylidene, -O-, -SO-, -CO-, -S-, -SO2-, C6 to C6 alkylene which may be fused with another aromatic ring which may contain heteroatoms. 12 -arylene,

[0049] or a group of formula (2) or (3)

[0050]

[0051] B is in each case C1 to C 12 - alkyl, preferably methyl, halogen, preferably chlorine and / or bromine,

[0052] x is in each case independently of one another 0, 1 or 2,

[0053] p is 1 or 0, and

[0054] R 5 and R 6 For each X 1 are selected individually and independently of one another to be hydrogen or C1 to C6-alkyl, preferably hydrogen, methyl or ethyl,

[0055] X 1 is carbon, and

[0056] m is an integer from 4 to 7, preferably 4 or 5, provided that at least one atom X 1 Upper, R 5 and R 6 At the same time it is an alkyl group.

[0057] Preferred diphenols are hydroquinone, resorcinol, dihydroxybiphenols, bis(hydroxyphenyl)-C1-C5-alkane, bis(hydroxyphenyl)-C5-C6-cycloalkane, bis(hydroxyphenyl)ether, bis(hydroxyphenyl)sulfoxide, bis(hydroxyphenyl)ketone, bis(hydroxyphenyl)sulfone and α,α-bis(hydroxyphenyl)diisopropylbenzene, and their ring-brominated and / or ring-chlorinated derivatives.

[0058] Particularly preferred diphenols are 4,4'-dihydroxybiphenyl, bisphenol A, 2,4-bis(4-hydroxyphenyl)-2-methylbutane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl sulfone, and their dibromo and tetrabromo or chlorinated derivatives, for example 2,2-bis(3-chloro-4-hydroxyphenyl)propane, 2,2-bis(3,5-dichloro-4-hydroxyphenyl)propane or 2,2-bis(3,5-dibromo-4-hydroxyphenyl)propane. Particularly preferred is 2,2-bis(4-hydroxyphenyl)propane (bisphenol A). The diphenols can be used alone or in the form of any desired mixtures. The diphenols are known from the literature or can be obtained by methods known from the literature.

[0059] Suitable chain terminators for the preparation of thermoplastic aromatic polycarbonates are, for example, phenol, p-chlorophenol, p-tert-butylphenol or 2,4,6-tribromophenol, and also long-chain alkylphenols, for example 4-[2-(2,4,4-trimethylpentyl)]phenol, 4-(1,3-tetramethylbutyl)phenol according to DE-A 2842005, or mono- or dialkylphenols having a total of 8 to 20 carbon atoms in the alkyl substituent, for example 3,5-di-tert-butylphenol, p-isooctylphenol, p-tert-octylphenol, p-dodecylphenol and 2-(3,5-dimethylheptyl)phenol and 4-(3,5-dimethylheptyl)phenol. The chain terminators are generally used in an amount of 0.5 to 10 mol %, based on the molar sum of the diphenols used in each case.

[0060] The average molecular weight (weight average M) of the thermoplastic aromatic polycarbonate w ) is preferably 20,000 to 40,000 g / mol, further preferably 22,000 to 32,000 g / mol, particularly preferably 24,000 to 30,000 g / mol, measured by GPC (gel permeation chromatography), the GPC being calibrated to bisphenol A polycarbonate standards, using dichloromethane as eluent, calibrated with linear polycarbonates (formed from bisphenol A and phosgene) of known molar mass distribution from PSS Polymer Standards Service GmbH, Germany, and calibrated by method 2301-0257502-09D (German version 2009) from Currenta GmbH & Co. OHG, Leverkusen. The eluent is dichloromethane. Column combination of crosslinked styrene-divinylbenzene resin. Diameter of the analytical column: 7.5 mm; length: 300 mm. Column material particle size: 3 μm to 20 μm. Solution concentration: 0.2% by weight. Flow rate: 1.0 ml / min, solution temperature: 30° C. Use UV and / or RI detection.

[0061] The preferred ranges lead to a particularly advantageous balance of mechanical and rheological properties of the composition according to the invention.

[0062] Thermoplastic aromatic polycarbonates can be branched in a known manner, more preferably by adding 0.05 to 2.0 mol % of trifunctional or more than trifunctional compounds, for example compounds with three or more phenolic groups, based on the total amount of diphenols used. Preference is given to using linear polycarbonates, more preferably polycarbonates based on bisphenol A.

[0063] Both homopolycarbonates and copolycarbonates are suitable. For the preparation of the copolycarbonates according to the invention of component A, it is also possible to use 1 to 25% by weight, preferably 2.5 to 25% by weight, of polydiorganosiloxanes with hydroxyaryloxy end groups, based on the total amount of diphenols used. These are known (US 3419634) and can be prepared by methods known from the literature. Also suitable are copolycarbonates containing polydiorganosiloxanes; the preparation of copolycarbonates containing polydiorganosiloxanes is described, for example, in DE-A 3334782.

[0064] Aromatic dicarboxylic acid dihalides for preparing aromatic polyester carbonates are preferably dichlorides of isophthalic acid, terephthalic acid, diphenyl ether-4,4'-dicarboxylic acid and naphthalene-2,6-dicarboxylic acid.

[0065] Particular preference is given to mixtures of isophthalic acid diacid chloride and terephthalic acid diacid chloride in a ratio of 1:20 to 20:1.

[0066] In the preparation of the polyester carbonates, carbonyl halides, preferably phosgene, are additionally used as difunctional acid derivatives.

[0067] Chain terminators which come into consideration for the preparation of aromatic polyester carbonates include, in addition to the monophenols already mentioned, their chlorocarbonates and optionally C1- to C2-substituted phenols. 22 -alkyl or halogen atom-substituted aromatic monocarboxylic acid chlorides, and aliphatic C2- to C 22 -monocarboxylic acid chlorides.

[0068] The amount of chain terminators is in each case from 0.1 to 10 mol %, based on the moles of diphenol for phenolic chain terminators and on the moles of dicarboxylic acid dichloride for monocarboxylic acid chloride chain terminators.

[0069] In the preparation of the aromatic polyester carbonates it is also possible to use one or more aromatic hydroxycarboxylic acids.

[0070] The aromatic polyester carbonates may be either linear or branched in a known manner (see in this respect DE-A 2940024 and DE-A 3007934), with preference being given to linear polyester carbonates.

[0071] The branching agents used may be, for example, trifunctional or polyfunctional carboxylic acid chlorides, for example trimesoyl chloride, cyanuric chloride, 3,3′,4,4′-benzophenonetetracarboxylic acid chloride, 1,4,5,8-naphthalenetetracarboxylic acid chloride or pyromellitic acid chloride, used in an amount of 0.01 to 1.0 mol % (based on the dicarboxylic acid dichloride used), or trifunctional or polyfunctional phenols, for example phloroglucinol, 4,6-dimethyl-2,4,6-tri(4-hydroxyphenyl)hept-2-ene, 4,6-dimethyl-2,4,6-tri(4-hydroxyphenyl)heptane, 1,3,5-tri(4-hydroxyphenyl)benzene, 1, .... 4-hydroxyphenyl)ethane, tris(4-hydroxyphenyl)phenylmethane, 2,2-bis[4,4-bis(4-hydroxyphenyl)cyclohexyl]propane, 2,4-bis(4-hydroxyphenylisopropyl)phenol, tetrakis(4-hydroxyphenyl)methane, 2,6-bis(2-hydroxy-5-methylbenzyl)-4-methylphenol, 2-(4-hydroxyphenyl)-2-(2,4-dihydroxyphenyl)propane, tetrakis(4-[4-hydroxyphenylisopropyl]phenoxy)methane, 1,4-bis[4,4'-dihydroxytriphenyl)methyl]benzene, the amount used is 0.01 to 1.0 mol% (based on the diphenol used). Phenolic branching agents can be added in advance together with diphenols; acid chloride branching agents can be added together with diacyl chlorides.

[0072] The proportion of carbonate structural units in the thermoplastic aromatic polyester carbonate can be changed arbitrarily. Preferably, the proportion of carbonate groups is based on the sum of ester groups and carbonate groups, and is at most 100 mol%, especially at most 80 mol%, and particularly preferably at most 50 mol%. Both the ester part and the carbonate part of the aromatic polyester carbonate can be present in the polycondensate in the form of blocks or in a randomly distributed form.

[0073] Thermoplastic aromatic polycarbonates and polyester carbonates can be used alone or in any desired mixtures.

[0074] Used as component A are linear polycarbonates which are further preferably based exclusively on bisphenol A.

[0075] Component B

[0076] The composition comprises, as component B, a polyester based on at least one aromatic or at least one cycloaliphatic dicarboxylic acid or mixtures thereof and cyclohexanedimethanol and optionally at least one further aliphatic diol. It is also possible to use mixtures of a plurality of such polyesters.

[0077] "Based on" here means that the polyester is prepared, for example, by polymerization of the dicarboxylic acids or their esters with the diols. The polyesters thus comprise structural units derived from aromatic or cycloaliphatic dicarboxylic acids and cyclohexanedimethanol and optionally further aliphatic diols.

[0078] Suitable aromatic or cycloaliphatic dicarboxylic acids are, for example, terephthalic acid, phthalic acid, isophthalic acid, naphthalene-2,6-dicarboxylic acid, 4,4′-biphenyldicarboxylic acid, 2,5-furandicarboxylic acid and cyclohexanedicarboxylic acid.

[0079] It is also possible to use mixtures of different dicarboxylic acids; for example, mixtures of terephthalic acid and up to 25 mol % of other dicarboxylic acids can be used.

[0080] The polyester preferably comprises only structural units derived from terephthalic acid and isophthalic acid as dicarboxylic acids, most preferably only structural units derived from terephthalic acid.

[0081] In the preparation of the polyesters, it is possible to start either from terephthalic acid and the other acids mentioned or from the alkyl esters or anhydrides of the corresponding acids.

[0082] As other aliphatic diols other than cyclohexanedimethanol, for example, ethylene glycol, butane-1,3-diol, butane-1,4-diol, propane-1,2-diol, propane-1,3-diol, pentane-1,5-diol, hexane-1,6-diol, isosorbide and tetramethylcyclobutanediol can be used. Ethylene glycol is preferred.

[0083] In a further preferred embodiment, isosorbide and ethylene glycol are used in addition to cyclohexanedimethanol; the polyester thus consists of three diol components in addition to the acid component.

[0084] Particularly preferably, component B is a polyester based on terephthalic acid and a mixture of cyclohexanedimethanol and ethylene glycol. In this context, it is further preferred that the molar ratio of cyclohexanedimethanol to ethylene glycol is from 40:60 to 80:20.

[0085] The preparation of polyesters according to component B is known. It can be achieved by esterification in the presence of a catalyst (for example a zinc compound) followed by polycondensation. A vacuum can be applied here and the reaction can be carried out at a temperature of, for example, 150° C. to 300° C. Other catalysts containing titanium, germanium, tin, aluminum or antimony as well as mixtures of different catalysts can be used in the polycondensation.

[0086] The reaction can be carried out continuously or discontinuously. The starting materials can be metered in separately or can also be premixed.

[0087] The polyesters according to component B have a weight-average molecular weight M preferably of 10 to 100 kg / mol. w , measured, for example, by gel permeation chromatography in 1,1,1,3,3,3-hexafluoro-2-propanol at a concentration of 1 g / l, using polymethyl methacrylate as standard.

[0088] In addition, the melt volume flow rate (MVR) of the polyester is preferably 20-80 cm3 / 10 minutes, preferably 30 to 70 cm 3 / 10 minutes, measured in each case in accordance with ISO 1133 (2012) at 270° C. and a load of 5 kg.

[0089] The preparation of polyesters according to component B is described, for example, in "Modern Polyesters: Chemistry and Technology of Polyesters and Copolyesters", (ed. J. Scheirs and T. E. Long, John Wiley & Sons, Ltd 2003) and the prior art cited therein. A suitable commercially available polyester is, for example, Skygreen TM JN100 (SK Chemicals Co., Ltd, South Korea). Another suitable commercially available polyester is, for example, ECOZEN TM T120 (SK Chemicals Co., Ltd, South Korea).

[0090] Component C

[0091] Phosphorus-containing flame retardants used as component C in the composition of the invention are preferably selected from monomeric and oligomeric phosphoric and phosphonic esters and phosphazenes, it being possible to use mixtures of various compounds selected from one or more of these groups as flame retardants.

[0092] Preferred monomeric and oligomeric phosphates and phosphonates are phosphorus compounds of the general formula (4)

[0093]

[0094] in

[0095] R 1 , R 2 , R 3 and R 4 each independently of one another is optionally halogenated C1 to C8-alkyl, C5 to C6-cycloalkyl, C6 to C8-alkyl, which is in each case optionally substituted by alkyl, preferably C1 to C4-alkyl, and / or halogen, preferably chlorine or bromine. 20 -Aryl or C7 to C 12 -aralkyl,

[0096] n is independently 0 or 1,

[0097] q is 0 to 30, and

[0098] X is a monocyclic or polycyclic aromatic group having 6 to 30 carbon atoms, or a straight-chain or branched aliphatic group having 2 to 30 carbon atoms, which may be OH-substituted and contains up to 8 ether bonds.

[0099] Preferably, R 1 , R 2 , R 3 and R 4 are independently C1 to C4-alkyl, phenyl, naphthyl or phenyl-C1 to C4-alkyl. 1 , R 2 , R 3 and R 4 In turn, it may be substituted by halogen and / or alkyl, preferably chlorine, bromine and / or C1 to C4-alkyl. Particularly preferred aryl groups are tolyl, phenyl, xylyl, propylphenyl or butylphenyl, and the corresponding brominated and chlorinated derivatives thereof.

[0100] X in formula (4) is preferably a monocyclic or polycyclic aromatic group having 6 to 30 carbon atoms. The latter is preferably derived from a diphenol.

[0101] n in formula (4) can be independently 0 or 1, preferably n is 1.

[0102] q represents a value of 0 to 30. When mixtures of a plurality of components of the formula (4) are used, mixtures having preferably a number average q value of 0.3 to 10, particularly preferably 0.5 to 10, in particular 1.05 to 1.4, most preferably 1.05 to 1.2 can be used.

[0103] X particularly preferably represents

[0104]

[0105] or a chlorinated or brominated derivative thereof; in particular, X is derived from resorcinol, hydroquinone, bisphenol A or diphenylphenol. Particularly preferably, X is derived from bisphenol A.

[0106] As component C according to the invention it is possible to use monophosphates (q=0), oligophosphates (q=1-30) or mixtures of monophosphates and oligophosphates.

[0107] The monophosphorus compound of the formula (1) is especially tributyl phosphate, tris(2-chloroethyl) phosphate, tris(2,3-dibromopropyl) phosphate, tris(2-ethylhexyl) phosphate, triphenyl phosphate, tricresyl phosphate, diphenylcresyl phosphate, diphenyloctyl phosphate, diphenyl-2-ethylcresyl phosphate, tris(isopropylphenyl) phosphate, halogen-substituted aryl phosphates, dimethyl methylphosphonate, diphenyl methylphosphonate, diethyl phenylphosphonate, triphenylphosphine oxide or tricresylphosphine oxide.

[0108] Particularly preferred phosphorus compounds according to component C are oligomeric phosphoric acid esters of the formula (5) based on bisphenol A.

[0109]

[0110] The phosphorus compounds according to the formula (4) are known (see, for example, EP-A 363608, EP-A 640655) or can be prepared in an analogous manner by known methods (eg, Ullmanns der technischen Chemie, Vol. 18, p. 301 ff., 1979; Houben-Weyl, Methoden der organischen Chemie, Vol. 12 / 1, p. 43; Beilstein, Vol. 6, p. 177).

[0111] The average q value can be determined by determining the composition (molecular weight distribution) of the phosphate mixture using a suitable method (gas chromatography (GC), high pressure liquid chromatography (HPLC), gel permeation chromatography (GPC)) and calculating the average value of q therefrom.

[0112] Phosphazenes are compounds of formula (6) and (7)

[0113]

[0114] in

[0115] R is in each case identical or different and is amino, in each case C1 to C8-alkyl, which is optionally halogenated, preferably halogenated by fluorine, or C1 to C8-alkoxy, in each case C5 to C6-cycloalkyl, which is optionally substituted by alkyl, preferably C1 to C4-alkyl, and / or halogen, preferably chlorine and / or bromine, 20 - aryl, preferably phenyl or naphthyl, C6 to C 20 -aryloxy, preferably phenoxy, naphthoxy, or C7- to C 12 - aralkyl, preferably phenyl-C1-C4-alkyl,

[0116] k is 0 or a number from 1 to 15, preferably a number from 1 to 10.

[0117] Propoxyphosphazenes, phenoxyphosphazenes, methylphenoxyphosphazenes, aminophosphazenes and fluoroalkylphosphazenes are described by way of example. Phenoxyphosphazenes are preferred. Phosphazenes can be used alone or in mixtures. The R groups can always be identical, or two or more groups in formula (6) and (7) can be different. Phosphazenes and their preparation are described, for example, in EP-A 728811, DE-A 1961668 and WO97 / 40092.

[0118] Component D

[0119] The composition may optionally contain one or more representatives selected from polymer additives and polymer blending partners as component D. The polymer additives or polymer blending partners are preferably selected from anti-drip agents, flame retardant synergists, smoke suppressants, lubricants and mold release agents, nucleating agents, antistatic agents, conductive additives, stabilizers, flow promoters, fillers and reinforcing agents, phase compatibilizers, impact modifiers, other polymer components different from components A and B (e.g., functional blending partners), and dyes and pigments.

[0120] Examples of impact modifiers are: graft polymers having a core-shell structure and a graft base comprising polybutadiene rubber, such as ABS and MBS, graft polymers having a graft base comprising acrylate rubber or silicone rubber or having a silicone acrylate rubber graft base, such as Metablen from Mitsubishi Rayon Co., Ltd. TM Type: Olefin-acrylate copolymer, such as DuPont's Elvaloy TM Type or Dow's Paraloid TM type.

[0121] In a preferred embodiment, at least one polymer additive selected from lubricants and mold release agents and stabilizers is used as component D.

[0122] In a preferred embodiment, at least one representative from the group consisting of sterically hindered phenols, organic phosphites, phosphorous acid and organic or inorganic Bronsted acids is used as stabilizer.

[0123] In a preferred embodiment, fatty acid esters, particularly preferably fatty acid esters of pentaerythritol or glycerol, are used as lubricants and mold release agents.

[0124] In another preferred embodiment, component D comprises at least one graft polymer having a core-shell structure and / or a rubber-free vinyl (co)polymer, further preferably in an amount of 1 to 10% by weight in total, based on the composition comprising components A, B, C and D.

[0125] Particularly preferably, a graft polymer having a core-shell structure and a graft base comprising polybutadiene rubber is used.

[0126] Particularly preferably, styrene-acrylonitrile copolymers are used as rubber-free vinyl (co)polymers.

[0127] Of course, the amount and type of component D must be selected so that flame retardancy and CTI are not significantly compromised.

[0128] Production of molding compound from the composition

[0129] Thermoplastic molding compositions can be produced from compositions comprising components A, B and C according to the invention and optionally component D. Thermoplastic molding compositions can be produced, for example, by mixing the individual constituents of the composition in a known manner and melt compounding and melt extruding in conventional apparatuses such as internal kneaders, extruders and twin-screw extruders at temperatures preferably from 200° C. to 320° C., particularly preferably from 240° C. to 300° C., very particularly preferably from 260° C. to 290° C.

[0130] In the context of this application, this process is generally referred to as compounding.

[0131] Thus, a "molding material" is understood to be the product obtained when the ingredients of the composition are melt-compounded and melt-extruded.

[0132] The individual components of the composition can be mixed in a known manner either sequentially or simultaneously, specifically either at about 20° C. (room temperature) or at higher temperatures. This means, for example, that some components can be metered in via the main feed opening of the extruder, while the remaining components can be introduced later during the compounding process via a side extruder.

[0133] Moulding materials can be used to produce mouldings. These can be produced, for example, by injection moulding, extrusion and blow moulding processes. Another form of processing is the production of mouldings from previously produced sheets or films by deep drawing. Moulding materials are particularly suitable for processing in extrusion, blow moulding and deep drawing processes.

[0134] It is also possible to meter the components of the composition directly into the conveying extruder of the injection molding machine, produce the molding material in the conveying extruder, and process it directly to the molding by correspondingly discharging the molding material into the injection molding mold (compounding or reactive compounding injection molding).

[0135] Therefore, another subject of the present invention relates to the use of the composition or molding compound according to the invention for the production of a molding, and a molding obtainable from the composition or molding compound according to the invention or comprising such a molding compound. According to the invention, the molding can also be an insulating layer in an electronic component (e.g. a transistor). In particular, the molding is the above-mentioned component, which is further preferably an electrical / electronic component.

[0136] The component is preferably a part of a (high) voltage switch, a (high) voltage inverter, a relay, an electronic connector, an electrical connector, a circuit breaker, a photovoltaic device, an electric motor, a radiator, a USB plug, an electric vehicle charger or charging plug, an electrical junction box, a smart meter housing, a miniature circuit breaker or a busbar. Likewise, a component can be a whole element, not just a part thereof.

[0137] For example, the component according to the invention can be produced by overmolding a metal conductor strip in injection molding. Here, the metal conductor strip is fixed in a preassembled form in the cavity of the injection molding mold. After the mold is closed, the conductor strip is flooded with the polymer melt under high pressure, whereby it forms a composite in the cooled state. After solidification and demoulding, the finished component is ready for use.

[0138] Another alternative is integrated plastic metal injection molding (IKMS). Here, the finished component is produced in two steps. In the first step, the plastic component with the conductor track that is then filled is produced. The finished plastic component is then placed in a second cavity and filled with solder, which forms the conductor track in the solidified state.

[0139] Another alternative is to subsequently connect the injection-molded component to the conductor strip, i.e. to produce the plastic component during injection molding and to assemble it with the conductor in a further step. Here, the injection-molded components can be connected during the assembly process by further input of energy. There are various ways to achieve this; for example, the metal conductor can be heated strongly so that it can be pressed into the plastic component. However, it is also possible to connect the conductor directly to the plastic component by laser welding.

[0140] Further embodiments of the present invention are listed below.

[0141] 1. A composition comprising

[0142] A) 60 to 93% by weight of at least one aromatic polycarbonate, polyester carbonate or a mixture thereof,

[0143] B) 2 to 20% by weight of polyesters based on at least one aromatic or at least one cycloaliphatic dicarboxylic acid or mixtures thereof and cyclohexanedimethanol and optionally other aliphatic diols,

[0144] C) 1 to 10% by weight of at least one phosphorus-containing flame retardant.

[0145] 2. The composition according to embodiment 1, characterized in that component B is an amorphous polyester.

[0146] 3. The composition according to embodiment 1 or 2, characterized in that the ratio of the weight proportion of component B in the composition to the weight proportion of phosphorus in the composition is less than 40, preferably greater than 5 to less than 40.

[0147] 4. The composition according to any one of the preceding embodiments, characterized in that component B is a polyester based on terephthalic acid and cyclohexanedimethanol and ethylene glycol.

[0148] 5. The composition according to embodiment 4, characterized in that the molar ratio of cyclohexanedimethanol to ethylene glycol is 40:60 to 80:20.

[0149] 6. The composition according to any one of the preceding embodiments, characterized in that component B is based on a mixture of cyclohexanedimethanol, ethylene glycol and isosorbide as diol component.

[0150] 7. The composition according to any one of the preceding embodiments, characterized in that component C is selected from monomeric and oligomeric phosphoric and phosphonic esters, phosphazenes and mixtures of these compounds.

[0151] 8. A composition according to any one of the preceding embodiments, characterized in that the compound used as component C is a compound of the general formula (4)

[0152]

[0153] in

[0154] R 1 , R 2 , R 3 and R 4 each independently of one another is optionally halogenated C1 to C8-alkyl, C5 to C6-cycloalkyl, C6 to C8-alkyl, which is in each case optionally substituted by alkyl, preferably C1 to C4-alkyl, and / or halogen, preferably chlorine or bromine. 20 -Aryl or C7 to C 12 -aralkyl,

[0155] n is independently 0 or 1,

[0156] q is 0 to 30, and

[0157] X is a monocyclic or polycyclic aromatic group having 6 to 30 carbon atoms, or a straight-chain or branched aliphatic group having 2 to 30 carbon atoms, which may be OH-substituted and contains up to 8 ether bonds.

[0158] 9. A composition according to any one of the preceding embodiments, comprising

[0159] 65 to 90 wt. % of component A

[0160] 3 to 18% by weight of component B

[0161] 2 to 9% by weight of component C.

[0162] 10. A composition according to any one of the preceding embodiments, comprising

[0163] 70 to 90 wt. % of component A

[0164] 4 to 16 wt. % of component B

[0165] 3 to 9% by weight of component C.

[0166] 11. The composition according to any of the preceding embodiments, further comprising 0.1 to 20% by weight of at least one polymer additive as component D, the polymer additive being selected from anti-drip agents, flame retardant synergists, smoke suppressants, lubricants and release agents, nucleating agents, antistatic agents, conductivity additives, stabilizers, flow promoters, fillers and reinforcing agents, phase compatibilizers, impact modifiers, other polymer components different from components A and B, and dyes and pigments.

[0167] 12. A composition according to embodiment 11, wherein the composition comprises as component D at least one graft polymer having a core-shell structure and / or a rubber-free vinyl (co)polymer in an amount of 1 to 10% by weight in total.

[0168] 13. The composition according to embodiment 11 or 12, wherein the graft polymer having a core-shell structure has a core comprising polybutadiene rubber.

[0169] 14. The composition according to any one of the preceding embodiments, consisting of components A to D.

[0170] Use of 15.2 to 20% by weight of polyesters based on aromatic or cycloaliphatic dicarboxylic acids or mixtures thereof and cyclohexanedimethanol and optionally other aliphatic diols and 1 to 10% by weight of at least one phosphorus-containing flame retardant for improving the CTI and flame retardancy according to UL 94V of polycarbonate compositions.

[0171] 16. The use according to embodiment 15, wherein a CTI of 600 V determined according to a rapid test method based on IEC 60112:2009 and a UL 94 V0 rating at a specimen thickness of 1.5 mm is achieved for a polycarbonate composition comprising 60 to 93 wt.% polycarbonate.

[0172] 17. Use according to embodiment 16, wherein the polycarbonate composition comprises 65 to 90% by weight of polycarbonate and wherein 3 to 18% by weight of polyesters based on aromatic or cycloaliphatic dicarboxylic acids or mixtures thereof and cyclohexanedimethanol and optionally other aliphatic diols and 2 to 9% by weight of at least one phosphorus-containing flame retardant are used.

[0173] 18. Use according to embodiment 16, wherein the polycarbonate composition comprises 70 to 90% by weight of polycarbonate and wherein 4 to 16% by weight of polyesters based on aromatic or cycloaliphatic dicarboxylic acids or mixtures thereof and cyclohexanedimethanol and optionally other aliphatic diols and 3 to 9% by weight of at least one phosphorus-containing flame retardant are used.

[0174] 19. Parts,

[0175] It includes

[0176] A first electrical conductor L1 and a second electrical conductor L2, having a first distance d1 and a second distance d2 between them,

[0177] which are connected by a thermoplastic material M in direct contact with the first and second electrical conductors,

[0178] wherein the distance d1 is the shortest distance between the first and second electrical conductors along the surface of the thermoplastic material M, and

[0179] wherein the distance d2 is the shortest distance between the first and second electrical conductors through air,

[0180] wherein d2 is chosen to prevent arcing through air at the respective operating voltage U of the component,

[0181] wherein d1 has the following values at the operating voltages U listed below:

[0182] d1 (0V ≤ U ≤ 250V): 1.3 mm to <2.5 mm

[0183] d1 (250V < U ≤ 500V) = 2.5 mm to <5.0 mm

[0184] d1 (500V < U ≤ 1000V) = 5.0 mm to <10.0 mm

[0185] and wherein the thermoplastic material M comprises the following components

[0186] A) 60 to 93 wt% of at least one aromatic polycarbonate, polycarbonate polyester or a mixture thereof,

[0187] B) 2 to 20 wt% of a polyester based on an aromatic or alicyclic dicarboxylic acid or a mixture thereof and cyclohexanedimethanol and optionally other aliphatic diols,

[0188] C) 1 to 10 wt% of at least one phosphorus-containing flame retardant.

[0189] 20. The component according to embodiment 19, wherein the component has an IP6K9K protection rating according to ISO 20653:2013, and wherein d1 has the following values at the operating voltages U listed below:

[0190] d1 (0V ≤ U ≤ 250V): 1.3 mm to <2.5 mm

[0191] d1 (250V < U ≤ 500V) = 2.5 mm to <5.0 mm

[0192] d1 (500V < U ≤ 1000V) = 5.0 mm to <10.0 mm.

[0193] 21. The component according to embodiment 20, wherein d1 has the following values at the operating voltages U listed below:

[0194] d1 (0V ≤ U ≤ 250V): 1.3 to <1.8 mm

[0195] d1 (250V < U ≤ 500V) = 2.5 to <3.6 mm

[0196] d1 (500V < U ≤ 1000V) = 5.0 to <7.1 mm

[0197] 22. The component according to any one of embodiments 19 to 21, wherein d2 is at least 1.2 mm.

[0198] 23. The component according to any one of embodiments 19 to 22, wherein d2 is 1.2 to 10.0 mm.

[0199] 24. The component according to any one of embodiments 19 to 23, wherein the thermoplastic material M comprises

[0200] 65 to 90 wt% of component A

[0201] 3 to 18 wt% of component B

[0202] 2 to 9 wt% of component C.

[0203] 25. The component according to any one of embodiments 19 to 24, wherein the thermoplastic material M comprises

[0204] 70 to 90 wt% of component A

[0205] 4 to 16 wt% of component B

[0206] 3 to 9 wt% of component C.

[0207] 26. The component according to any one of embodiments 19 to 25, wherein it is an electrical / electronic component.

[0208] 27. The component according to any one of embodiments 19 to 26, wherein it is part of a (high) voltage switch, (high) voltage inverter, relay, electronic connector, electrical connector, circuit breaker, photovoltaic device, motor, radiator, USB plug, electric vehicle charger or charging plug, electrical junction box, smart meter housing, miniature circuit breaker or busbar. Examples

[0209] Component A-1:

[0210] Linear polycarbonate based on bisphenol A, with a weight-average molecular weight M W26000 g / mol (determined by GPC in dichloromethane with reference to bisphenol A-based polycarbonate).

[0211] Component A-2:

[0212] Linear polycarbonate based on bisphenol A, with a weight average molecular weight M W 24,000 g / mol (determined by GPC in dichloromethane with reference to bisphenol A-based polycarbonate).

[0213] Component B

[0214] Skygreen TM JN100 (SK Chemicals Co., Ltd, South Korea): a copolyester based on terephthalic acid, cyclohexanedimethanol, ethylene glycol and diethylene glycol in a molar ratio of 44.4:30.7:23.7:1.1, with a weight average molecular weight of M W The melt volume flow rate (MVR) is 51 cm 3 / [10 min], measured according to ISO 1133 (2012 edition) at a temperature of 270° C. and a load of 5 kg.

[0215] Component C

[0216] Bisphenol A-based oligophosphate according to the following structure (Chemtura Manufacturing UK Limited)

[0217]

[0218] Component D-1

[0219] Pentaerythritol tetrastearate as a release agent, Cognis Oleochemicals GmbH, Germany

[0220] Component D-2

[0221] Irgafos diphosphite TM P-EPQ, 1,1-biphenyl-4,4'-diylbisphosphonite tetrakis(2,4-di-tert-butylphenyl) ester, BASF (Germany)

[0222] Component D-3

[0223] Irganox TM 1076, 3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionic acid octadecyl ester, BASF (Germany)

[0224] Component D-4

[0225] Cycolac TM INP449: A polytetrafluoroethylene (PTFE) formulation from SabiC consisting of 50 wt% PTFE contained in a SAN copolymer matrix.

[0226] Component D-5

[0227] Phosphorous acid, H3PO3, Sigma-Aldrich Chemie GmbH, Germany

[0228] Production and testing of molding compounds made from the composition

[0229] The components were mixed in a ZSK-26Mc18 twin-screw extruder from Coperion, with a material temperature of 250-280° C. The molded articles were produced in an Arburg 270E injection molding machine at a material temperature of 270° C. and a mold temperature of 70° C.

[0230] IZOD impact toughness was determined according to ISO 180-U (2019 edition) at room temperature using a test bar with dimensions of 80 mm x 10 mm x 4 mm.

[0231] The Vicat softening temperature was measured in accordance with DIN ISO 306 (method B, load 50 N, heating rate 120 K / h, 2013 edition) on one-sided injection-molded test bars with the dimensions 80 x 10 x 4 mm.

[0232] The flame retardancy was evaluated according to UL94V on bars with dimensions of 127 x 12.7 x 1.5 mm.

[0233] The comparative tracking index of the compositions described herein was tested according to a rapid test method based on IEC60112:2009. For this purpose, a 0.1% concentration of an ammonium chloride test solution (resistance of 395 ohms*cm) was applied dropwise on the surface of a specimen of 60 mm x 40 mm x 4 mm in size between two adjacent electrodes 4 mm apart, with a time interval of 30 s. A test voltage was applied between the electrodes, which varied during the test. The first specimen was tested at a starting voltage of 300 V or 350 V. A maximum of 50 drops were applied per voltage (one drop every 30 s), as long as no leakage current of >0.5 A or burning of the sample occurred within 2 s. After 50 drops, the voltage was increased by 50 V and a new specimen was tested at this higher voltage according to the above procedure. This process continued until 600 V was reached or a leakage current or burning occurred. If one of the above effects has occurred with less than 50 drops, the voltage was reduced by 25 V and a new specimen was tested at a lower voltage. The voltage is reduced until the 50-drop test is passed without leakage current or burning. This procedure is therefore used to determine the maximum possible voltage until the composition can withstand 50 drops of the test solution without leakage current. Finally, for confirmation, four further specimens are tested at the determined maximum voltage, with 50 drops each. In the examples, this confirmation value is shown as CTI. The 100-drop value was not determined, so it is a "rapid test method based on the standard".

[0234] Table 1:

[0235] Compositions of the invention and their properties

[0236]

[0237] kb means "no break

[0238] The data in Table 1 show that the test specimens made from the composition of the present invention have high CTI, very good flame retardancy, and high heat distortion resistance and impact toughness.

[0239] Table 2:

[0240] Non-inventive compositions and properties thereof

[0241]

[0242] kb means "no break

[0243] The data in Table 2 show that the samples made of non-compositions of the present invention do not achieve the desired performance. If the proportion of component B is too high, as shown in V5 and V6, even if the amount of component C is increased, it is impossible to achieve the desired flame retardancy. In this case (V6), the heat deformation resistance is further reduced. If the proportion of component C is further increased, although the flame retardancy can be improved again (V9), the heat deformation resistance is very low. In addition, the comparative tracking index (CTI) is no longer sufficient. Examples V7 and V8, in which the proportion of component C is also too high, also show a low comparative tracking index. In addition, all embodiments in which the proportion of component C is too high show insufficient impact toughness, i.e., fracture is observed in each case (V7, V8 and V9).

Claims

1. A composition comprising A) 60 to 93% by weight of at least one aromatic polycarbonate, polyester carbonate or a mixture thereof, B) 2 to 20% by weight of a polyester based on at least one aromatic or at least one cycloaliphatic dicarboxylic acid or a mixture thereof and cyclohexanedimethanol and optionally at least one further aliphatic diol, C) 1 to 10% by weight of at least one phosphorus-containing flame retardant.

2. The composition according to claim 1, characterized in that Component B is an amorphous polyester.

3. The composition according to claim 1 or 2, characterized in that The ratio of the weight proportion of component B in the composition to the weight proportion of phosphorus in the composition is less than 40, preferably greater than 5 and less than 40.

4. A composition according to any one of the preceding claims, characterized in that Component B is a polyester based on terephthalic acid and cyclohexanedimethanol and ethylene glycol.

5. The composition according to claim 4, characterized in that The molar ratio of cyclohexanedimethanol to ethylene glycol is 40:60 to 80:

20.

6. A composition according to any one of the preceding claims, characterized in that Component B is based on a mixture of cyclohexanedimethanol, ethylene glycol and isosorbide as diol component.

7. A composition according to any one of the preceding claims, characterized in that Component C is selected from monomeric and oligomeric phosphoric and phosphonic esters, phosphazenes and mixtures of these compounds.

8. The composition according to any one of the preceding claims, characterized in that The compound used as component C is the compound of the general formula (4) in R 1 , R 2 , R 3 and R 4 each independently of one another is optionally halogenated C1 to C8-alkyl, C5 to C6-cycloalkyl, C6 to C8-alkyl, which is in each case optionally substituted by alkyl, preferably C1 to C4-alkyl, and / or halogen, preferably chlorine or bromine. 20 -Aryl or C7 to C 12 -aralkyl, n is independently 0 or 1, q is 0 to 30, and X is a monocyclic or polycyclic aromatic group having 6 to 30 carbon atoms, or a straight-chain or branched aliphatic group having 2 to 30 carbon atoms, which may be OH-substituted and contains up to 8 ether bonds.

9. A composition according to any one of the preceding claims, comprising 65 to 90 wt. % of component A 3 to 18% by weight of component B 2 to 9% by weight of component C.

10. The composition according to any of the preceding claims, further comprising as component D 0.1 to 20% by weight of at least one polymer additive selected from anti-drip agents, flame retardant synergists, smoke suppressants, lubricants and mold release agents, nucleating agents, antistatic agents, conductivity additives, stabilizers, flow promoters, fillers and reinforcing agents, phase compatibilizers, impact modifiers, other polymer components different from components A and B, and dyes and pigments.

11. The composition according to claim 10, wherein the composition comprises as component D at least one graft polymer having a core-shell structure and / or a rubber-free vinyl (co)polymer in an amount of 1 to 10% by weight in total. Use of 12.2 to 20% by weight of polyesters based on aromatic or cycloaliphatic dicarboxylic acids or mixtures thereof and cyclohexanedimethanol and optionally other aliphatic diols and 1 to 10% by weight of at least one phosphorus-containing flame retardant for improving the CTI determined according to the rapid test method based on IEC 60112:2009 and the flame retardancy according to UL 94V of polycarbonate compositions.

13. The use according to claim 12, wherein a polycarbonate composition comprising 60 to 93 wt. % polycarbonate has a CTI of 600 V determined according to a rapid test method based on IEC 60112:2009 and a UL 94 V0 rating at a test specimen thickness of 1.5 mm.

14. A component comprising a first electrical conductor L1 and a second electrical conductor L2 having a first distance d1 and a second distance d2 from each other, They are connected by a thermoplastic material M which is in direct contact with the first and second electrical conductors, wherein the distance d1 is the shortest distance between the first electrical conductor and the second electrical conductor along the surface of the thermoplastic material M, and Wherein the distance d2 is the shortest distance through air between the first electrical conductor and the second electrical conductor, where d2 is selected so as to prevent arcing through air at the respective operating voltage U of the components, Where d1 has the following values ​​at the operating voltage U listed below: d1(0V≤U≤250V):1.3mm to <2.5mm d1(250V <u≤500v)=2.5mm至<5.0mmd1(500V <u≤1000v)=5.0mm至<10.0mmAnd wherein the thermoplastic material M comprises the following components A) 60 to 93% by weight of at least one aromatic polycarbonate, polyester carbonate or a mixture thereof, B) 2 to 20% by weight of polyesters based on aromatic or cycloaliphatic dicarboxylic acids or mixtures thereof and cyclohexanedimethanol and optionally other aliphatic diols, C) 1 to 10% by weight of at least one phosphorus-containing flame retardant.

15. The component according to claim 14, wherein the component has IP6K9K protection class according to ISO 20653:2013, and wherein d1 has the following values ​​at the operating voltage U listed below: d1(0V≤U≤250V):1.3mm to <2.5mm d1(250V <u≤500v)=2.5mm至<5.0mm d1(500V< / u≤500v)=2.5mm至<5.0mm

Citation Information

Patent Citations

  • wave transit device

    DE1961668A1

  • Continuous condensn of polyarylesters - suitable for extrusion or casting into films

    DE2232877A1

  • process for the production of aromatic copolyesters

    DE2703376A1

  • bisphenol a terephthalate carbonate

    DE2714544A1

  • polycarbonates WITH ALKYLPHENYL TERMINALS, THEIR PRODUCTION AND USE

    DE2842005A1