Coating type cutting tool

Through the multi-layer structure (Ti,Al)N coating, the problem of insufficient stress concentration and wear resistance at high cutting speeds of existing cutting tools is solved, and a longer service life and higher wear resistance are achieved. Suitable for drilling operations of various steel types.

CN119013435APending Publication Date: 2024-11-22WALTER AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380035511.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-29
Filing Date
2023-04-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The coating of existing metal machining cutting tools is prone to high stress concentration when subjected to high cutting speed and harsh operation, resulting in shortening of service life and insufficient wear resistance of backhand surfaces, making it difficult to adapt to drilling of various steel types. operate.

Method used

Using a multi-layer structure (Ti,Al)N coating, the first layer has high fracture toughness and low residual compression stress, the second layer forms a residual stress gradient between the first and third layers, and the third layer is nitrogen The chemical layer ensures the single-phase cubic structure and excellent adhesion of the coating through specific deposition processes and conditions.

Benefits of technology

It extends the service life of the cutting tool, improves the resistance to backcut surface wear, is suitable for drilling operations of various steel types, and improves the wear resistance of the overall carbide drill bit of the tool.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention relates to a coated cutting tool comprising a substrate and a coating comprising a first layer, a second layer and a third layer, where i) the first layer is a (Ti, Al) N layer adhered to the substrate, the first layer having an atomic ratio Al / (Ti + Al) of a.0.3 to 0.65, b. A fracture toughness in the range of 3.5 to 6 MPa [square root of] m, c. A substantially uniform residual stress [sigma] 1 in the range of + 100 to-1000 MPa, c. Ii) the second layer is a (Ti, Al) N layer adhered to the first layer, the second layer having an atomic ratio Al / (Ti + Al) of a.0.3 to 0.85, b. A residual stress sigma2 in a range from about sigma1 at an interface with the first layer to sigma3 at an interface with the third layer, and c. A residual stress sigma2 in a range from about sigma1 at an interface with the third layer to about sigma3 at an interface with the third layer. Wherein [sigma] 2 gradually increases from an interface with the first layer to an interface with the third layer adhered to the second layer, and wherein a residual stress [sigma] 2 at the interface with the third layer is substantially the same as a residual stress in the third layer, iii) the third layer consists of a nitride of one or more elements of group 4, 5 or 6 of the Periodic Table of Elements, or of Al and / or Si with a nitride of one or more elements of group 4, 5 or 6 of the Periodic Table of Elements, the third layer having a substantially uniform residual stress [sigma] 3, [sigma] 3lt; and the pressure is-1200 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a coated cutting tool, which comprises a substrate and a coating comprising a first layer, a second layer and a third layer. Background Art

[0002] There is a continuing desire to extend the service life of cutting tools for metal machining to withstand higher cutting speeds and / or other increasingly demanding cutting operations. Typically, cutting tools for metal machining comprise a hard substrate material such as cemented carbide coated with a thin hard, wear-resistant coating, such as a titanium aluminum nitride (Ti, Al) N coating deposited by a PVD process. A single-phase cubic crystal structure is typically desired, but there is a threshold value for aluminum content to provide such a single-phase cubic structure rather than a mixed structure comprising cubic and hexagonal structures, which threshold value may vary to some extent with, for example, deposition conditions. Furthermore, it is well known that thicker coatings can extend service life up to a certain limit where, for example, undesirable high stress concentrations occur in the coating-to-substrate interface.

[0003] The object of the present invention is to provide a coated cutting tool having a (Ti, Al)N coating which exhibits a single-phase cubic structure with high fracture toughness and low residual compressive stress while imparting improved adhesion of the coating to the substrate.

[0004] Another object of the present invention is to provide a coated cutting tool having excellent flank wear resistance.Another object is to provide a general purpose tool such as a solid carbide drill suitable for any machining operation including drilling various steel grades. Summary of the invention

[0005] The present invention relates to a coated cutting tool, the cutting tool comprising a substrate and a coating comprising a first layer, a second layer and a third layer, wherein

[0006] i) the first layer is a (Ti, Al)N layer adhered to the substrate, the first layer having

[0007] a. an atomic ratio Al / (Ti+Al) of 0.3 to 0.65, preferably 0.4 to 0.65, more preferably 0.5 to 0.65,

[0008] b. a fracture toughness in the range of 3.5 to 6 MPa√m, preferably 4 to 5 MPa√m,

[0009] c. a substantially uniform residual stress σ1 in the range of +100 to -1000 MPa, preferably -300 to -700 MPa,

[0010] ii) a second layer is a (Ti, Al)N layer adhered to the first layer, the second layer having

[0011] a. an atomic ratio Al / (Ti+Al) of 0.3 to 0.85, preferably 0.4 to 0.85,

[0012] b. a residual stress σ2 in the range of about σ1 at the interface with the first layer to σ3 at the interface with the third layer, wherein σ2 gradually increases from the interface with the first layer to the interface with the third layer adhered to the second layer, wherein the residual stress σ2 at the interface with the third layer is substantially the same as the residual stress in the third layer,

[0013] iii) The third layer is composed of nitrides of one or more elements in Group 4, 5 or 6 of the periodic table, or of nitrides of Al and / or Si and one or more elements in Group 4, 5 or 6 of the periodic table, and the third layer has a substantially uniform residual stress σ3, σ3<-1200 MPa, preferably σ3<-1400 MPa, and more preferably -5000 MPa<σ3<-1500 MPa.

[0014] According to one embodiment, substantially uniform residual stress means a maximum deviation of 15%, or preferably a maximum deviation of 5%, from the mean value of the residual stress.

[0015] The term "gradually" is also meant to include the following situation: the increase may be stepwise, but not necessarily a continuous increase. However, "gradually" preferably refers to a continuous and regular increase, such as a continuous linear increase.

[0016] According to one embodiment, the second layer is a cubic (Ti, Al)N layer.

[0017] According to one embodiment, the third layer may be a single layer or a multilayer, and is composed of a nitride containing at least one of Al, Zr, Ti, Nb and Cr, or is composed of a nitride of Al and / or Si and at least one of Zr, Ti, Nb and Cr. The third layer may be suitably composed of (Ti, Al) N, (Cr, Al) N, (Ti, Si) N, CrN, TiN or NbN.

[0018] According to one embodiment, the third layer is a cubic (Ti, Al)N layer or a (Ti, Si)N layer having an atomic ratio Al / (Ti+Al) of 0.67 to 0.85 or an atomic ratio Si / (Ti+Si) of 0.05 to 0.2.

[0019] According to one embodiment, the atomic ratio Al / (Ti+Al) of the second layer gradually increases from the interface with the first layer to the interface with the third layer, for example, from 0.5 to 0.8, or from 0.55 to 0.75.

[0020] The gradual increase in the Al content in the second layer can be achieved in several ways. For example, the increase in Al content can be achieved by selecting the type and amount of targets containing specific amounts of Al and Ti during the deposition process. In addition, the Al and Ti content of the deposited coating can be changed by changing the deposition conditions such as bias voltage and arc current.

[0021] According to one embodiment, at least one of the first, second and third layers is a multilayer consisting of two or more alternating (Ti, Al)N sublayer types differing in their composition and having an overall atomic ratio as specified herein.

[0022] According to one embodiment, at least one of the first, second and third (Ti, Al)N layers is a multilayer composed of two or more alternating (Ti, Al)N sublayer types that differ in their composition, wherein at least one (Ti, Al)N sublayer type has an atomic ratio Al / (Ti+Al) of 0.50 to 0.67, preferably 0.55 to 0.67, and most preferably 0.60 to 0.67, and at least one (Ti, Al)N sublayer type has an atomic ratio Al / (Ti+Al) of 0.70 to 0.90, preferably 0.75 to 0.85.

[0023] The type of (Ti, Al)N sublayer in the multilayer is suitably a nanolayer, which may have an average thickness of 1 to 100 nm, preferably 1.5 to 50 nm, most preferably 2 to 20 nm.

[0024] According to one embodiment, the first layer, the second layer and the third layer are single layers.

[0025] According to one embodiment, the third layer is a (Ti, Al)N layer having an atomic ratio Al / (Ti+Al) in the range of 0.70 to 0.85.

[0026] According to one embodiment, the atomic ratio Al / (Al+Ti) of the second layer is from 0.7 to 0.85.

[0027] According to one embodiment, the average grain size of the first layer is in the range of 50 to 500 nm, preferably 50 to 200 nm and most preferably 70 to 150 nm.

[0028] According to an embodiment, the thickness of the first layer is in the range of 1 μm to 20 μm, for example 2 μm to 10 μm, such as 3 μm to 8 μm.

[0029] According to one embodiment, the thickness of the coating is 3 to 25 μm, preferably 5 to 15 μm, most preferably 7 to 12 μm.

[0030] According to one embodiment, the first layer shows a distribution of 311 misorientation angles. The 311 misorientation angle is the difference between the normal vector of the first layer surface and the normal vector closest to the first layer surface. <311> Preferably, the cumulative frequency distribution of the 311 misorientation angles is such that ≥40% of the misorientation angles are less than 12.5°.

[0031] The term 311 misorientation angle refers to the smallest angle between the normal vector of the (Ti, Al)N layer and the normal vector of the layer closest to the (Ti, Al)N layer. <311> The angle between directions.

[0032] According to one embodiment, the cumulative frequency distribution of the 311 misorientation angles is such that more than 50%, such as more than 55%, of the misorientation angles are less than 12.5°.

[0033] According to one embodiment, the cumulative frequency distribution of the 311 misorientation angles is such that ≤ 95%, such as less than 85% or less than 75%, of the misorientation angles are less than 12.5°.

[0034] According to one embodiment, the cumulative frequency distribution of the 311 misorientation angles is such that 40% to 85%, such as 50% to 75%, of the misorientation angles are less than 12.5°.

[0035] According to one embodiment, the cumulative frequency distribution of the 311 misorientation angles is such that 5% to 40%, such as 8% to 25%, or such as 10% to 15%, of the misorientation angles are less than 5°.

[0036] The distribution of 311 misorientation angles can be determined by electron backscatter analysis (EBSD). However, the columnar grain width generally increases with increasing thickness of the (Ti, Al) N layer, especially for the first few microns of the (Ti, Al) N layer, and if the grain width is too small, EBSD analysis may not be applicable. Therefore, in the case of (Ti, Al) N layers with a thickness of less than 2 µm, if the grain size is considered too small for EBSD analysis, it is preferred to determine the distribution of 311 misorientation angles in transmission electron microscopy (TEM) analysis. EBSD or TEM analysis is suitable for a distance of 0.7 mm from the cutting edge.

[0037] According to one embodiment, the third layer is the outermost layer.

[0038] According to one embodiment, the first layer (Ti, Al)N has a Vickers hardness of ≧2400 HV (15 mN load), preferably 2500 to 2800 HV (15 mN load).

[0039] According to one embodiment, the plane strain modulus of the first layer (Ti, Al) N is ≥ 450 GPa, preferably ≥ 500 GPa, for example 450 to 550 or 450 to 500 GPa. The plane strain modulus of the third (Ti, Al) N layer is preferably 450 to 530 GPa, more preferably 480 to 510 GPa.

[0040] The substrate of the coated cutting tool can be any one commonly used in the field of cutting tools for metal machining. The substrate can be appropriately selected from cemented carbide, cermet, cubic boron nitride (cBN), ceramic, polycrystalline diamond (PCD) and high speed steel (HSS). In a preferred embodiment, the substrate is cemented carbide.

[0041] The coated cutting tool of the present invention obtained by the method further described herein has a first layer with lower residual stress. This is obtained by depositing the first layer on the substrate under selected process conditions including high temperature. The process also imparts increased fracture toughness to the first layer. The process also involves depositing a second layer, which is deposited while the temperature decreases linearly, as further explained in the working example. This also leads to the appearance of a residual stress gradient in the second layer. The third layer is deposited at the lowest temperature for the second layer, so that a single-phase cubic structure of a (Ti, Al)N composition with a high aluminum content can be deposited as the outermost layer. In order to improve the surface roughness and reduce the surface adhesion of the workpiece material, wet sandblasting and drag finishing can be performed. The manufactured coated cutting tool is preferably a blade for drilling, such as a solid carbide drill, a blade for turning or an end mill, or other indexable blades. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 A schematic diagram of an embodiment of a cutting tool as a milling insert is shown.

[0043] Figure 2 A schematic diagram of the coated cutting tool and the temperatures used during the deposition of the three layers are shown. DETAILED DESCRIPTION

[0044] Figure 1 A schematic diagram of an embodiment of a cutting tool (1) is shown having a rake face (2), a flank face (3) and a cutting edge (4). The cutting tool (1) is a milling insert in this embodiment. Figure 2 A schematic cross-sectional view of one embodiment of a coated cutting tool of the present invention having a substrate body (5) and a first coating (6), a second coating (7) and a third coating (8) is shown.

[0045] method

[0046] Electron Backscatter Diffraction (EBSD):

[0047] The cumulative frequency distribution of the 311 misorientation angle is calculated as follows: For each spot measurement of the entire EBSD scan (an incremental surface area representing the entire surface area analyzed), the crystal direction perpendicular to the surface plane of the (Ti,Al)N layer is derived from the measured absolute crystal orientation (i.e., orientation data in Euler angles).

[0048] Then, the crystal orientation is calculated to be closest to <311> The vector angle between the surface normal and the surface normal is the closest. <311> type direction (among all twelve crystal-equivalent possibilities). This angle is defined as the 311 misorientation angle. Because each measurement point constitutes an equal portion of the analyzed area, the relative frequency distribution of these angular misorientation values ​​characterizes the overall degree of 311 surface texture.

[0049] Electron Diffraction in Transmission Electron Microscopy (TEM):

[0050] The sample is suitably analyzed in cross section, i.e. the incident electron beam is parallel to the film plane. To exclude amorphization during sample preparation, different methods can be used: i) classical preparation, including mechanical cutting, bonding, grinding and ion polishing; and ii) using FIB to cut the sample and perform peeling for final polishing. The position analyzed is for example close to the substrate, about 200 nm from the substrate.

[0051] Then obtain the SAED data of the sample. According to the SAED data, the diffraction intensity profile along the 311 ring can be obtained, and the 311 ring is centered at the angular position corresponding to the coating normal. Then normalized integration is performed at the 311 diffraction spot and the -3-1-1 diffraction spot respectively, until the 45-degree misorientation angle. Then the two integrals are merged into an intensity distribution curve. The intensity distribution data derived from the 311 diffraction spot and the -3-1-1 diffraction spot are used to increase the number of data points, thereby reducing the signal-to-noise ratio as much as possible.

[0052] The intensity at a specific misorientation angle is proportional to the sample volume where the misorientation occurs. Therefore, the intensity distribution curve is equivalent to the distribution of 311 misorientation angles. Accordingly, the cumulative intensity curve obtained from the intensity distribution curve is equivalent to the cumulative frequency distribution of 311 misorientation angles.

[0053] Vickers Hardness:

[0054] The Vickers hardness was measured using a Picodentor HM500 nanoindentation method (load-depth diagram) from Helmut Fischer GmbH, Sindelfingen, Germany. For the measurement and calculation, the Oliver and Pharr evaluation algorithm was used, in which a diamond test body conforming to the Vickers standard was pressed into the layer and the force-path curve was recorded during the measurement. The maximum load used was 15 mN (HV 0.0015), and the time periods of load increase and load reduction were 20 seconds each. Based on this curve, the hardness was calculated.

[0055] Plane strain modulus:

[0056] The elastic properties of the coated samples are measured by the so-called plane strain modulus E ps The modulus is obtained by nanoindentation using the method of Oliver and Pharr. The nanoindentation data are obtained by the indentation described above for Vickers hardness.

[0057] Grain size:

[0058] The average grain size is determined from SEM images by the stereological line intersection method: a grid of lines is superimposed on the micrograph of interest and the intersections of the lines with the grain boundary network are marked. The distance statistics between adjacent intersections reflect the size of the three-dimensional grains (e.g. HE Exner, Quantitative Description of Microstructures by Image Analysis, in: Mater. Sci. Technol., Wiley-VCH Verlag GmbH & Co. KGaA, Weinheim, Germany, 2006 (including section 15.3.5 “Size and spacing” - ).

[0059] To account for the morphological features of PVD hard coatings (primarily elongated columnar grain shape), the spacing between grain boundaries was evaluated only on lines parallel to the film plane. Therefore, the data reflect the grain width parallel to the coating plane.

[0060] The corresponding SEM micrographs were taken from the flank faces of triply rotated test inserts made of cemented carbide (the substrate surface repeatedly faced the arc source during deposition). They were taken 100 µm from the substrate edge. The grain width was determined at a defined coating height of 2 µm. At least 380 spacing measurements were collected.

[0061] Residual stress:

[0062] Residual stress measurements were performed on a diffractometer from Seifert / GE (PTS 3003) according to the sin²ψ method. CuKα radiation with a polycapillary lens for the generation of a parallel beam was used in the analysis (high voltage 40 kV, current 40 mA). The incident beam was defined by a 2.0 mm pinhole. For the diffracted beam path, an energy dispersive detector (Meteor0D) was applied. An Euler holder was used to tilt the sample at an angle ψ (ψ = angle between the specimen surface normal and the diffraction vector). Residual stresses in the sample were measured using {111}-cubic-TiAlN reflections. 15 ψ angles were considered in the interval -60° < ψ < 60° (sin²ψ equidistant) to determine the residual stress values ​​in the coating. Assuming a rotationally symmetrical distribution of the residual stresses, only one φ direction was used. For the evaluation of the stresses in TiAlN, the X-ray elastic constant -s1=0.491 TPa was applied. -1 and 0.5s2 = 2.780 TPa -1 Peak fitting was done by using Rachinger correction (correction for Kα2) and pseudo-Voigt function for peak fitting.

[0063] In order to measure the residual stress of a layer of a coating having other deposited layers above it, the coating material is removed above the layer to be measured. Care must be taken to select and apply a material removal method that does not significantly change the residual stress within the remaining nitride multilayer material. A suitable method for removing the deposited coating material may be polishing, however, a gentle and slow polishing using a fine-grain polishing agent should be applied. As is known in the art, strong polishing using a coarse-grain polishing agent will increase the residual stress. Other suitable methods for removing the deposited coating material are ion etching and laser ablation.

[0064] thickness:

[0065] The layer thickness was determined by calotte grinding with a 30 mm diameter steel ball grinding a dome-shaped recess and further measuring the diameter of the ring, from which the layer thickness was calculated. The layer thickness of the rake face (RF) of the cutting tool was measured at 2000 µm from the corner, and the layer thickness of the flank face (FF) was measured in the middle of the flank face.

[0066] Fracture toughness:

[0067] In order to quantify the fracture toughness of the studied coatings, the micro-pillar splitting technique developed by Sebastiani et al. [1, 2, and 4] was used. In this test method, a sharp indenter tip is centered on the top surface of a micrometer-sized pillar in the sample material. As the pillar is loaded by the indenter, the force increases until the pillar fails, i.e. splits. The critical splitting force 𝑃 can then be calculated from the formula 𝑐 The critical stress intensity factor of crack generation from the indenter contact, i.e., the splitting fracture toughness 𝐾𝑐, is obtained:

[0068] K c =(E / H)P 𝑐 / R 3 / 2 (1)

[0069] where 𝛾 represents the proportionality factor related to the elastic-plastic properties of the tested material (the ratio of Young's modulus E to hardness H), and R represents the radius of the column. The above formula is based on the analytical model of a semi-elliptical surface crack and is verified by bonding zone finite element modeling (CZ-FEM) [2].

[0070] Pillars were micromachined from the target coating by focused ion beam (FIB) milling. A single-shot milling strategy using a pattern of concentric rings with continuously decreasing diameters was used to minimize the taper of the pillars. Therefore, the FIB probe current was gradually reduced from 15 nA (initial roughing) to a final polishing current of 300 pA. All pillars tested were characterized by a diameter of 7 μm and an aspect ratio of ∼1.3 (the pillar splitting technique requires a height-to-diameter ratio >1 [2]). Prior to any FIB milling, the surface of the sample to be structured was carefully polished using a colloidal silica suspension (Struers OPS 0.04 μm) with a nominal grain size of 40 nm. This step served to remove any roughness present on the surface of the deposited coating. No more than 100 nm of the top coating was removed by this procedure. After this surface preparation, the micropillars were uniformly placed approximately 120 μm from the cutting edge, close to the “nose radius” of the supporting substrate. The column load was applied on a Fischer Picodenter HM500 nanoindentation system (Helmut Fischer GmbH, Sindelfingen, Germany) using a three-sided pyramidal cube-corner diamond indenter (nominal surface angle of 35.26°). The experiments were performed in a load-controlled manner using a constant load rate of 1 mN / s. For each coating and sample state, at least 12 tests were performed to account for the inherent scatter of the fracture experiments (20 tests in most cases). The accuracy of the sample stage and tip positioning was experimentally verified to be within 10% of the column radius used and not to distort the measurement results [3]. To calculate the fracture toughness according to equation (1), the coating-specific 𝛾 factor was derived from the data published by Ghidelli et al. in reference [4]. The measurements can be performed by preparing a cross section of the coated tool or by carefully removing the top layer by mechanical polishing or focused ion beam machining.

[0071] [1] M. Sebastiani, KE Johanns, EG Herbert, F. Carassiti, GMPharr, A novel Pillar indentation splitting test for measuring fracturetoughness of thin ceramic coatings, Philos. Mag. 95 (2015) 1928–1944.https: / / doi.org / 10.1080 / 14786435.2014.913110.

[0072] [2] M. Sebastiani, K.E. Johanns, E.G. Herbert, G.M. Pharr,Measurement of fracture toughness by nanoindentation methods: Recent advancesand future challenges, Curr. Opin. Solid State Mater. Sci. 19 (2015) 324–333.https: / / doi.org / 10.1016 / j.cossms.2015.04.003.

[0073] [3] C.M. Lauener, L. Petho, M. Chen, Y. Xiao, J. Michler, J.M.Wheeler, Fracture of Silicon: Influence of rate, positioning accuracy, FIBmachining, and elevated temperatures on toughness measured by pillarindentation splitting, Mater. Des. 142 (2018) 340–349. https: / / doi.org / 10.1016 / j.matdes.2018.01.015.

[0074] [4] M. Ghidelli, M. Sebastiani, K.E. Johanns, G.M. Pharr, Effects ofindenter angle on micro‐scale fracture toughness measurement by pillarsplitting, J. Am. Ceram. Soc. 100 (2017) 5731–5738. https: / / doi.org / 10.1111 / jace.15093.

[0075] Example 1

[0076] Before depositing the coating, the WC-Co material was pre-treated by plasma etching (center beam etching) to remove about 1 µm, thereby eliminating organic residues and relieving surface damage and residual stress caused by previous grinding of the substrate. The etching was carried out at a temperature of 600 ° C, and the other process conditions were as follows:

[0077] I: 140A

[0078] U bias : 170 V

[0079] p Ar :0.21 Pa

[0080] t etch : 65 minutes

[0081] Arc-deposited (Ti, Al)N three-layer coatings were prepared by sequentially depositing a first base layer, a second intermediate layer, and a third top layer on a cemented carbide substrate. The first and second layers consisted of Ti deposited on a WC-Co type substrate. 0.40 Al 0.60 The substrate composition was 6 wt % Co and the remainder WC. Deposition was performed using cathodic arc deposition in a Balzers Innova Arc-PVD system (Oerlikon Balzers Coating AG, Balzers, Liechtenstein) with the following process parameters:

[0082] The first layer (base layer) of (Ti, Al) N:

[0083] Target: Ti 0.40 Al 0.60

[0084] Target size: round 150 mm

[0085] Arc current: 4×200 A

[0086] Pressure: 5 Pa

[0087] Temperature: 600℃

[0088] Total pressure: 5 Pa (N2)

[0089] Argon pressure: 0 Pa (0 sccm Ar)

[0090] Bias potential: -40 V

[0091] 2x and 3x rotation

[0092] Light source configuration APO, mag 14

[0093] The deposited layer thickness was approximately 3.1 µm.

[0094] The second layer (middle layer) of (Ti, Al) N:

[0095] Target: Ti 0.40 Al 0.60

[0096] Target size: round 150 mm

[0097] Arc current: 2×200 A

[0098] Pressure: 5 Pa (N2)

[0099] Temperature: 600 to 300°C

[0100] Total pressure: 5 Pa (N2 pressure)

[0101] Argon pressure: 0 Pa (0 Ar sccm)

[0102] Bias potential: -40 V

[0103] Light source configuration APO, mag 14

[0104] During the coating step, the temperature was linearly decreased from 600° C. to 300° C. The second layer was grown to a thickness of 1.5 µm.

[0105] The third layer (top layer) of (Ti, Al) N:

[0106] Target: Ti 0.27 Al 0.73

[0107] Target size: round 150 mm

[0108] Arc current: 2×200 A

[0109] Temperature: 300℃

[0110] Total pressure: 2 Pa

[0111] Argon flow rate: 300 sccm

[0112] Bias potential: -80 V

[0113] Light source configuration APO, mag 14

[0114] The deposited layer thickness was 1.4 µm. This resulted in a coating with a total thickness of 6 µm.

[0115] Residual stress of the first layer: -600 MPa

[0116] Fracture toughness of the first layer: 4.1 MPa√m

[0117] Hardness of the first layer: 2600 HV

[0118] Plane strain modulus of the first layer: 520 GPa

[0119] Electron backscatter diffraction (EBSD) analysis was performed on the first layer (base layer) of (Ti, Al) N. The cumulative frequency distribution of the 311 misorientation angle was calculated as described in the "Methods" section. The first layer (base layer) of (Ti, Al) N showed a cumulative frequency distribution of the 311 misorientation angle, such that about 62% of the 311 misorientation angles were less than 12.5°, and about 13% of the 311 misorientation angles were less than 5°.

[0120] The third layer (top layer) of (Ti, Al) N shows a 111-texture. It is estimated that the cumulative frequency distribution of the 111 misorientation angles of the third layer (top layer) of (Ti, Al) N is such that >50% of the 111 misorientation angles are less than 10°.

[0121] Example 2 (Comparative Example)

[0122] A base layer was prepared as a comparison according to the preparation method of the first layer (base layer) of Example 1, except that the thickness of the base layer was prepared to be 5.9 μm so that the coating thickness was comparable to the total coating thickness of Example 1.

[0123] Example 3

[0124] Drilling tests were conducted on various workpiece materials on a DMG MORI DMU65 MonoBlock vertical 3-axis machine tool as follows. In this Example 3, steel was machined using a coated cutting tool prepared using the coatings prepared according to Examples 1 and 2. The number of holes for critical flank wear for the test tools is listed in Table 1 below:

[0125] Workpiece material: Steel C45, 1.1191 (705 N / mm 2 )

[0126] Cutting speed, v c : 200 m / min

[0127] Feed / rev: 0.28 mm / rev

[0128] Drilling depth: 30 mm

[0129] Hole type: through hole

[0130] KSS: emulsion, 7%; 40 bar

[0131]

[0132] As can be seen from Table 1, the three-layer tool with the coating according to Example 1 (invention) has an extended tool life compared to the single-layer coating of Example 2 (reference).

[0133] Example 4

[0134] In Example 4, a simulation test was conducted on 42CrMo4 steel.

[0135] Workpiece material: 42CrMo4, (EN-JL1040; 215HB)

[0136] Cutting speed, V c :105 m / min

[0137] Feed / rev: 0.2 mm / rev

[0138] Drilling depth: 30 mm

[0139] Hole type: through hole

[0140] KSS: emulsion, 6%; 40 bar

[0141]

[0142] In Table 2, the invention has a significantly higher wear resistance in terms of critical flank wear compared to the same reference.

Claims

1. A coated cutting tool, comprising a substrate and a coating comprising a first layer, a second layer and a third layer, wherein i) the first layer is a (Ti, Al)N layer adhered to the substrate, the first layer having a. Atomic ratio Al / (Ti+Al) of 0.3 to 0.65, b. Fracture toughness in the range of 3.5 MPa√m to 6 MPa√m, c. Substantially uniform residual stress σ in the range of +100 MPa to -1000 MPa 1 , ii) the second layer is a (Ti, Al)N layer adhered to the first layer, the second layer having a. Atomic ratio Al / (Ti+Al) of 0.3 to 0.85, b. about σ at the interface with the first layer 1 σ at the interface with the third layer 3 Residual stress in the range of 2 , where σ 2 The residual stress σ at the interface with the third layer gradually increases from the interface with the first layer to the interface with the third layer adhered to the second layer. 2 is substantially the same as the residual stress in the third layer, iii) the third layer is composed of nitrides of one or more elements in Group 4, 5 or 6 of the periodic table, or of nitrides of Al and / or Si and one or more elements in Group 4, 5 or 6 of the periodic table, and the third layer has a substantially uniform residual stress σ 3 , σ 3 <-1200 MPa.

2. The coated cutting tool according to claim 1, wherein the third layer is a cubic (Ti, Al)N layer or a (Ti, Si)N layer having an atomic ratio Al / (Ti+Al) of 0.67 to 0.85 or an atomic ratio Si / (Ti+Si) of 0.05 to 0.

2. 3 . The coated cutting tool according to claim 1 , wherein the fracture toughness of the first layer is in the range of 4 MPa√m to 5 MPa√m. 4 . The coated cutting tool according to claim 1 , wherein the atomic ratio Al / (Ti+Al) of the second layer gradually increases from the interface with the first layer toward the interface with the third layer.

5. The coated cutting tool according to any one of claims 1 to 4, wherein at least one of the first layer, the second layer and the third layer is a multilayer consisting of two or more alternating (Ti, Al)N sublayer types that differ in their composition, wherein the total atomic ratio is as defined in claim 1.

6. The coated cutting tool according to any one of claims 1 to 5, wherein the cumulative frequency distribution of the 311 misorientation angles of the first layer is such that ≥40% of the 311 misorientation angles are less than 12.5°.

7. The coated cutting tool according to any one of claims 1 to 6, wherein the first layer, the second layer and the third layer are single layers.

8. The coated cutting tool according to any one of claims 1 to 7, wherein the third layer is a (Ti, Al)N layer having an atomic ratio Al / (Ti+Al) in the range of 0.70 to 0.

85.

9. The coated cutting tool according to any one of claims 1 to 8, wherein the residual stress of the first layer is in the range of -300 MPa to -700 MPa.

10. The coated cutting tool according to any one of claims 1 to 9, wherein the tool is a solid carbide drill, an end mill or an indexable insert.

11. The coated cutting tool according to any one of claims 1 to 10, wherein the atomic ratio Al / (Al+Ti) of the second layer is 0.7 to 0.

85.

12. The coated cutting tool according to any one of claims 1 to 11, wherein an average grain size of the first layer is in the range of 50 nm to 500 nm.

13. The coated cutting tool according to any one of claims 1 to 12, wherein the thickness of the first layer is in the range of 1 μm to 20 μm.

14. The coated cutting tool according to any one of claims 1 to 13, wherein the thickness of the coating is in the range of 3 μm to 25 μm.