Method for customizing magnetic permeability of soft magnet and soft magnet obtained thereby
Through laser melting and ablation technology, the deposit of austenite phase stabilization donor materials on the surface of soft magnetic materials has been solved, and the cost and time problems of magnetic customization of soft magnetic materials in the prior art have been solved, thus achieving efficient improvement of magnetic properties and simplification of production processes. .
Patent Information
- Application Number
- CN202380033439.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-01-30
- Filing Date
- 2023-01-31
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art has limitations in the magnetic properties of customized soft magnetic materials, especially in increasing magnetic permeability and reducing production time and costs, and conventional processes rely on labor-intensive masking and demasking processes. .
Using laser melting and laser ablation technology to selectively deposit and alloy the austenite phase to stabilize donor materials on the surface of soft magnetic materials, eliminating the need for complex masks and chemical treatments, and achieving fast and low-cost magnetic customization .
It realizes efficient magnetic customization of soft magnetic material surfaces, reduces production steps and time, improves permeability contrast ratio, and reduces costs, and is suitable for motors and other magnetic applications.
Smart Images

Figure CN119013743A_ABST
Abstract
Description
[0001] Priority data
[0002] This international patent application claims priority to U.S. Provisional Patent Application No. 63 / 329,535 filed on April 11, 2022 and U.S. Patent Application No. 18 / 102,905 filed on January 30, 2023, each of which is hereby incorporated by reference herein. Field of the Invention
[0003] The present invention generally relates to methods for tailoring magnetic properties in soft magnetic bodies and magnetic structures obtained thereby. Background of the Invention
[0005] A magnet is a material or object that produces a magnetic field. The magnetic field creates a force that acts on other magnets or ferromagnetic materials such as iron, steel, nickel or cobalt. A permanent magnet is an object made of a material that has been magnetized and creates its own persistent magnetic field. Applications of permanent magnets include, but are not limited to, electric vehicle motors, electric takeoff assist motors and sensors, magnetic separators and magnetic detectors.
[0006] Some ferromagnetic materials are soft magnetic materials ("soft magnets") such as annealed iron. Soft magnets can be magnetized, but do not tend to remain magnetized. On the other hand, hard magnetic materials ("hard magnets") are typically difficult to demagnetize. Hard magnets have a high magnetic coercivity, while soft magnets have a relatively low magnetic coercivity. Applications of soft magnets include transformer cores, motors, generators, inductors, and electromagnets.
[0007] Most modern electric machines employ magnetically permeable soft ferromagnetic materials (such as steel or magnets) whose geometry is used to guide the magnetic field and provide an effective medium for energy transfer. Common magnetic materials used for this purpose are stacked layers of non-oriented electrical steel sheets. The functional soft magnetic material used for electric machines is typically ferrosilicon (FeSi) alloys.
[0008] In order to improve the magnetic properties, soft magnetic materials can be alloyed with other materials and heat treated to optimize the microstructure. This process introduces defects, grain boundaries and impurities that hinder the movement of magnetic domain walls and significantly impair the magnetic properties. Conventional processes use computer-aided design of machine cores to develop special precision tools for cutting and punching dies, which are used for the purpose of die forming and stamping. The FeSi sheets are then cold rolled to the thickness required for the stack and cut to the required size. These sheets are coated with insulating materials that resist eddy current flow. Stamping and punching are then performed to form the sheets into the desired geometry. The sheets are then stacked on an alignment fixture by pin connection or welding. Post-machining and heat treatment of the stack may be required to prevent deterioration caused by stress generated by stamping, welding and interlocking. In conventional processes, several stacks are stamped, stacked, measured, machined and finished in each process. Therefore, labor time and production time may be very long.
[0009] New or improved methods, structures and systems are desired to tailor magnetic properties in soft magnetic materials. Current masking and bulk nitriding work is limited to low saturation alloys. Prior art methods require masking and demasking of the surface of a heat resistant varnish. Masking and demasking are labor intensive and not rapidly repeatable.
[0010] A scalable, low-cost process is desired to selectively alloy the magnetic surface of a rotor, a key component of an electromagnetic system such as a motor, generator, or alternator.In general, methods for tailoring the behavior of soft magnetic materials are needed. Summary of the invention
[0011] The present invention addresses the foregoing needs in the art, as will now be summarized and then further described in detail below.
[0012] Some variations provide a method of customizing a surface of a soft magnetic material, the method comprising:
[0013] (a) providing a selected ferromagnetic receptor material;
[0014] (b) providing a selected austenite phase stabilizing donor material;
[0015] (c) depositing a selected austenite phase stabilizing donor material onto one or more first surface regions of a ferromagnetic receptor material;
[0016] (d) not depositing the selected austenite phase stabilizing donor material on the one or more second surface regions of the ferromagnetic receptor material;
[0017] (e) laser melting a selected austenite phase stabilizing donor material into the one or more first surface regions to form molten austenite phase stabilizing donor material; and
[0018] (f) solidifying the molten austenite phase stabilized donor material to form a solid austenite phase stabilized donor material located within the one or more first surface regions, thereby selectively alloying the ferromagnetic acceptor material within the one or more first surface regions,
[0019] wherein the one or more first surface regions are characterized by a first average magnetic permeability after the selective alloying in step (f),
[0020] wherein the one or more second surface regions are characterized by a second average magnetic permeability, and
[0021] The first average magnetic permeability is higher than the second average magnetic permeability.
[0022] In some embodiments, the method does not employ a mask. In some embodiments, the method does not employ a chemical treatment.
[0023] In some methods, in step (c), the austenite phase stabilizing donor material is deposited in the form of powder particles.Alternatively or additionally, in step (c), the austenite phase stabilizing donor material may be deposited in the form of a film, foil or mesh.
[0024] In some methods, the selected ferromagnetic acceptor material is selected from the group consisting of FeSi, FeNi, FeCo, NiCo, FeSiAl, and combinations thereof.
[0025] In some methods, the selected austenite phase stabilizing donor material is selected from the group consisting of Ni, Mn, Co, Cr, Si, Mo, Nb, Ti, Mg, Cu, Al, N, C, B, and combinations thereof.
[0026] In step (c), for example, the selected austenite phase stabilizing donor material can be deposited on the one or more first surface regions using slurry coating, laser cladding, electron beam cladding, electroplating, electroless plating, wire arc deposition, chemical vapor deposition, physical vapor deposition, thermal spraying, plasma spraying, or a combination thereof.
[0027] After step (f), the one or more first surface regions may have an average thickness of, for example, from about 1 micron to about 3000 microns. In certain embodiments, the average thickness is from about 100 microns to about 500 microns.
[0028] In some methods, the first average magnetic permeability is at least 90% higher than the second average magnetic permeability. In certain embodiments, the first average magnetic permeability is at least 99% higher than the second average magnetic permeability (such as at least 99.9% or at least 99.99%).
[0029] For example, soft magnetic materials may be present in rotors in electric motors.
[0030] Other variations provide a method of customizing a surface of a soft magnetic material, the method comprising:
[0031] (a) providing a selected ferromagnetic receptor material;
[0032] (b) providing a selected austenite phase stabilizing donor material;
[0033] (c) depositing a selected austenite phase stabilizing donor material onto one or more first surface regions of a ferromagnetic receptor material;
[0034] (d) not depositing the selected austenite phase stabilizing donor material on the one or more second surface regions of the ferromagnetic receptor material; and
[0035] (e) laser ablating a selected austenite phase-stabilized donor material into the one or more first surface regions to force the selected austenite phase-stabilized donor material to penetrate into the one or more first surface regions to selectively alloy the ferromagnetic receptor material in the one or more first surface regions,
[0036] wherein the one or more first surface regions are characterized by a first average magnetic permeability,
[0037] wherein the one or more second surface regions are characterized by a second average magnetic permeability, and
[0038] The first average magnetic permeability is higher than the second average magnetic permeability.
[0039] In some embodiments employing laser ablation, the method does not employ masks, chemical treatments, or either of these.
[0040] In some methods, in step (c), the selected austenite phase stabilizing donor material is deposited in the form of powder particles.
[0041] The selected ferromagnetic acceptor material may be selected from the group consisting of FeSi, FeNi, FeCo, NiCo, FeSiAl, and combinations thereof.
[0042] The selected austenite phase stabilizing donor material may be selected from the group consisting of Ni, Mn, Co, Cr, Si, Mo, Nb, Ti, Mg, Cu, Al, N, C, B, and combinations thereof.
[0043] In some embodiments employing laser ablation, in step (c), for example, the selected austenite phase stabilizing donor material may be deposited on the one or more first surface regions using electrodeposition, chemical vapor deposition, physical vapor deposition, thermal spraying, plasma spraying, or a combination thereof.
[0044] In some methods, the one or more first surface regions have an average thickness of from about 1 micron to about 3000 microns.
[0045] The first average magnetic permeability is at least 90% greater than the second average magnetic permeability.
[0046] Soft magnetic materials may be present in rotors in electric motors.
[0047] Some variations provide a soft magnet having surface-tailored magnetic permeability, wherein the soft magnet comprises:
[0048] (i) a first region comprising a first core region and a first surface region, wherein the first core region comprises a ferromagnetic material, and wherein the first surface region comprises an austenite phase stabilizing donor material; and
[0049] (ii) a second region comprising a second core region, wherein the second core region comprises a ferromagnetic material, and wherein the second region does not comprise an austenite phase stabilizing donor material;
[0050] wherein the first surface region has an average thickness from about 1 micron to about 3000 microns,
[0051] wherein the first region is characterized by a first average magnetic permeability,
[0052] wherein the second region is characterized by a second average magnetic permeability, and
[0053] The first average magnetic permeability is higher than the second average magnetic permeability.
[0054] Certain embodiments provide a soft magnet having surface-tailored magnetic permeability, wherein the soft magnet comprises:
[0055] (i) a first region comprising a first core region and a first surface region, wherein the first core region comprises a ferromagnetic material, and wherein the first surface region comprises a first concentration of an austenite phase stabilizing donor material; and
[0056] (ii) a second region comprising a second core region and a second surface region, wherein the second core region comprises a ferromagnetic material, wherein the second surface region comprises a second concentration of an austenite-stabilizing donor material, and wherein the second concentration of the austenite-stabilizing donor material is lower than the first concentration of the austenite-stabilizing donor material;
[0057] wherein the first surface region has an average thickness from about 1 micron to about 3000 microns,
[0058] wherein the first region is characterized by a first average magnetic permeability,
[0059] wherein the second region is characterized by a second average magnetic permeability, and
[0060] The first average magnetic permeability is higher than the second average magnetic permeability.
[0061] In some soft magnets, the ferromagnetic material is selected from the group consisting of FeSi, FeNi, FeCo, NiCo, FeSiAl, and combinations thereof.
[0062] In some soft magnets, the austenite phase stabilizing donor material is selected from the group consisting of Ni, Mn, Co, Cr, Si, Mo, Nb, Ti, Mg, Cu, Al, N, C, B and combinations thereof.
[0063] In some soft magnetic bodies, the first surface region has an average thickness of from about 100 microns to about 500 microns.
[0064] In the first region of the soft magnetic body, for example, the thickness of the first surface region may be about 0.1% to about 50% of the thickness of the first core region.
[0065] In some soft magnets, the first average magnetic permeability is at least 90% higher than the second average magnetic permeability. In some soft magnets, the first average magnetic permeability is at least one order of magnitude higher than the second average magnetic permeability. In different embodiments, the first average magnetic permeability is at least two, three, or four orders of magnitude higher than the second average magnetic permeability (four orders of magnitude is a 10,000:1 contrast ratio).
[0066] The soft magnetic body may contain multiple instances of the first region and / or the second region.
[0067] For example, soft magnets may be present in the rotor in an electric motor. BRIEF DESCRIPTION OF THE DRAWINGS
[0068] Figure 1 Schematic diagram of a method for customizing the surface of a soft magnetic material.
[0069] Figure 2is an exemplary flow chart outlining a method for selectively alloying a ferromagnetic receptor material in one or more first surface regions using laser melting and solidification of an austenite phase stabilized donor material.
[0070] Figure 3 is an exemplary flow chart outlining a method for selectively alloying a ferromagnetic receptor material in one or more first surface regions using laser ablation to force infiltration of an austenite phase-stabilized donor material into the first surface region or regions.
[0071] Figure 4 is a schematic diagram showing two electromagnets, one of which serves as a north (N) magnetic pole and the other of which serves as a south (S) magnetic pole.
[0072] Figure 5 is similar to Figure 4 Schematic diagram showing the north (N) and south (S) magnetic poles.
[0073] Figure 6 is a schematic illustration of a soft magnet with surface tailored magnetic permeability.
[0074] Figure 7 is a micrograph of the FeSi sheet with Ni selective regions formed by melting and resolidification of Ni foil in Example 1 (scale bar = 1000 microns).
[0075] Fig. 8A is a scanning electron microscope (SEM) micrograph of a cross section of a Ni foil welded to a FeSi sheet in Example 1 (scale bar = 200 microns).
[0076] Figure 8B is an Energy Dispersive X-ray Spectroscopy (EDS) graph showing the different compositions present in Example 1.
[0077] Fig. 9 is a micrograph of the FeSi sheet having the Cu selective region (weld zone) formed by melting and resolidification of the Cu foil in Example 2 (white scale bar = 20 micrometers).
[0078] Fig.10 is a micrograph of a FeSi sheet having Ni selective regions formed by melting and resolidification of Ni powder in Example 3 (scale bar = 1000 microns). DETAILED DESCRIPTION
[0079] The methods, structures, systems, and compositions of the present invention will now be described in detail with reference to various non-limiting examples.
[0080] This description will enable those skilled in the art to make and use the invention, and describes several embodiments, modifications, variations, alternatives and uses of the invention. These and other embodiments, features and advantages of the invention will become more apparent to those skilled in the art when reference is made to the following detailed description of the invention in conjunction with the accompanying drawings.
[0081] As used in this specification and the appended claims, the singular forms "a / an" and "the" include plural referents unless the context clearly dictates otherwise. Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.
[0082] Unless otherwise indicated, all numerical values expressing conditions, concentrations, dimensions, and the like used in the specification and claims should be understood as being modified in all instances by the term "about". Accordingly, unless indicated to the contrary, the numerical parameters set forth in the following specification and the appended claims are approximations that may vary at least as a function of the particular analytical technique.
[0083] The term "comprising," which is synonymous with "including," "containing," or "characterized by," is inclusive or open-ended and does not exclude additional, unrecited elements or method steps. "Comprising" is a specialized term used in claim language that means the specified claim elements are essential, but other claim elements may be added and still constitute a concept within the scope of the claim.
[0084] As used herein, the phrase "consisting of excludes any element, step, or ingredient not specified in the claim. When the phrase "consisting of" (or variations thereof) appears in a clause in the body of a claim, rather than immediately following the preamble, the phrase is limited only to the elements set forth in that clause; other elements are not excluded from the claim as a whole. As used herein, the phrase "consisting essentially of limits the scope of a claim to the specified elements or method steps, plus those that do not materially affect the basis and novel feature or features of the claimed subject matter.
[0085] With respect to the terms "comprising", "consisting of", and "consisting essentially of", where one of these three terms is used herein, the presently disclosed and claimed subject matter may include the use of any of the other two terms, except when used with Markush groups. Thus, in some embodiments not otherwise expressly recited, any instance of "comprising" may be replaced by "consisting of" or, alternatively, "consisting essentially of".
[0086] Some variations of the invention provide a rapid, scalable and low-cost process for making soft magnets selectively alloyed on the surface of the magnet. The technique allows the surface of an object to be programmed with selected areas of different magnetic permeabilities. Areas with high magnetic permeability and areas with low magnetic permeability can be selectively produced in three dimensions, allowing specific control over the magnetic properties and energy density of the soft magnet.
[0087] Soft magnetic materials are those that are easily magnetized and demagnetized. "Soft magnets" (or "temporary magnets") typically have an intrinsic magnetic coercivity of less than 1000 A / m.
[0088] Compared to the prior art, the present invention reduces the number of steps for customizing the surface of a magnetic object. The present invention eliminates the need for any masking and chemical treatment for removing the mask. Instead of masking and removing the mask, selective laser melting and / or laser ablation is used to quickly and efficiently incorporate the austenite phase stabilizing material into the surface of the ferromagnetic material in a targeted manner. The present invention not only eliminates the need for complex masks or chemical treatments, but also reduces processing time and costs.
[0089] The inventors have discovered that selective alloying can be greatly simplified by surface alloying and laser processing (laser melting and / or laser ablation). The simplicity results in a precise, fast and reliably repeatable process.
[0090] Commercial applications of the present invention include, but are not limited to, programmable soft magnetic motors, electric vehicle (EV) permanent magnet motors, and electric takeoff assist motors and sensors. An exemplary embodiment customizes the surface of a rotor for use in an electric vehicle. The surface is customized by selectively alloying the surface of the rotor so that different zones or regions of the rotor surface are programmed to have different magnetic permeabilities.
[0091] refer to Figure 1 It is possible to understand variations of the present invention, and this figure is a schematic diagram of a method for customizing the surface of a soft magnetic material. Figure 1In the embodiment of the present invention, a bulk alloy is selected. The bulk alloy forms a ferromagnetic receptor material having a target receptor metal surface. An alloying element (austenite phase stabilizing donor material) such as Ni or Mn is deposited on the surface. Figure 1 In the embodiment, the donor material is deposited as a layer of spherical particles, which is for illustration purposes only; for example, the donor material can be a powder, foil or layer, vapor deposited material, sprayed material, or electroplated material. A laser is used to incorporate the donor material into the surface of the ferromagnetic receptor material via laser melting and / or laser ablation. Figure 1 As shown, the result is an alloyed surface of thickness t, which can be controlled by adjusting the laser power. The austenite phase stabilizes the donor material to tailor the surface of the soft magnet and thus its magnetic permeability. Figure 1 In FIG. 1 , for purposes of this illustration, only selected first surface areas are depicted, while second surface areas that are not intended for deposition are not depicted.
[0092] and Figure 1 Some related embodiments employ laser ablation rather than laser melting. When laser ablation is used, an austenite phase stabilized donor material (e.g., Ni) is still applied to the surface of a ferromagnetic acceptor material (e.g., FeSi or FeCo). Instead of using a laser as a heat source to melt the donor material, a laser of sufficient power is used to force the donor material into the surface of the acceptor material. The donor is not necessarily melted, but rather pushed into the surface of the acceptor. Figure 1 Certain related embodiments employ a combination of laser melting and laser ablation.
[0093] Whether laser melting or laser ablation is employed, the donor material or the acceptor material may or may not be lost, for example, by evaporation, sublimation, random diffusion, etc. In some methods, all elements of the acceptor material and the donor material remain in a solid or liquid phase, below their normal boiling points.
[0094] Some variations provide a method of customizing a surface of a soft magnetic material, the method comprising:
[0095] (a) providing a selected ferromagnetic receptor material;
[0096] (b) providing a selected austenite phase stabilizing donor material;
[0097] (c) depositing a selected austenite phase stabilizing donor material onto one or more first surface regions of a ferromagnetic receptor material;
[0098] (d) not depositing the selected austenite phase stabilizing donor material on the one or more second surface regions of the ferromagnetic receptor material;
[0099] (e) laser melting a selected austenite phase stabilizing donor material into the one or more first surface regions to form molten austenite phase stabilizing donor material; and
[0100] (f) solidifying the molten austenite phase stabilized donor material to form a solid austenite phase stabilized donor material located within the one or more first surface regions, thereby selectively alloying the ferromagnetic acceptor material within the one or more first surface regions,
[0101] wherein the one or more first surface regions are characterized by a first average magnetic permeability after the selective alloying in step (f),
[0102] wherein the one or more second surface regions are characterized by a second average magnetic permeability, and
[0103] The first average magnetic permeability is higher than the second average magnetic permeability.
[0104] Figure 2 is an exemplary flow chart outlining a method for selectively alloying a ferromagnetic receptor material in one or more first surface regions using laser melting and solidification of an austenite phase stabilized donor material. Because the austenite phase stabilized donor material is melted and then resolidified, Figure 2 The method can be considered as a type of laser-based additive manufacturing.
[0105] In some methods, in step (c), the austenite phase stabilizing donor material is deposited in the form of powder particles.Alternatively or additionally, in step (c), the austenite phase stabilizing donor material may be deposited in the form of a film, foil or mesh.
[0106] In a preferred embodiment, the method does not employ a mask. In a preferred embodiment, the method does not employ a chemical treatment.
[0107] In some methods, the selected ferromagnetic acceptor material is selected from the group consisting of FeSi, FeNi, FeCo, NiCo, FeSiAl, and combinations thereof. For any of these ferromagnetic acceptor materials, various stoichiometries are possible. The elements that make up the ferromagnetic acceptor material can be combined together to form molecules (compounds), can be together in solid solution as a single phase alloy, or can exist in a multiphase alloy. Other ferromagnetic acceptor materials are possible, such as (but not limited to) iron oxide, iron-zinc alloys, and manganese-zinc alloys.
[0108] It should be understood that FeSi refers to Fe x Si y Compounds or alloys in which x and y can take different values to form compounds or alloys of iron and silicon. When x = 1 and y = 1, the compound is iron monosilicide Fe1 Si 1 When x = 2 and y = 1, the compound is Fe2Si 2 Si. When x = 1 and y = 2, the compound is iron disilicide FeSi 2 , and so on. In some embodiments, FeSi is a ferrosilicon alloy of iron and silicon, for example, wherein the silicon content is about 1%-20% by weight.
[0109] It should be understood that FeNi refers to Fe x Ni y Compounds or alloys, where x and y can take different values to form compounds or alloys of iron and nickel. For example, FeNi can be selected from Fe 1 Ni 1 , Fe 2 Ni、Fe 3 Ni、FeNi 2 In some embodiments, FeNi is a nickel-iron alloy of iron and nickel, for example, wherein the nickel content is about 2%-80% by weight.
[0110] It should be understood that FeCo refers to Fe x Co y Compounds or alloys, where x and y can take different values to form compounds or alloys of iron and cobalt. For example, FeCo can be selected from Fe 1 Co 1 , Fe 2 Co、Fe 3 Compounds of Co or combinations thereof. In some embodiments, FeCo is a cobalt-iron alloy of iron and cobalt, for example wherein the cobalt content is about 10%-90% by weight.
[0111] It should be understood that NiCo refers to Ni x Co y Compounds or alloys, wherein x and y can take different values to form compounds or alloys of nickel and cobalt. For example, NiCo can be selected from Ni1Co1, Ni 2 Co、NiCo 2 In some embodiments, NiCo is a nickel-cobalt alloy having a nickel content of about 1% to about 99% by weight and a cobalt content of about 99% to about 1% by weight.
[0112] It should be understood that FeSiAl refers to Fe x Si y Al zCompounds or alloys, wherein x, y and z can take different values to form compounds or alloys of iron, silicon and aluminum. In some embodiments, FeSiAl is a ferrosilicon-aluminum alloy, for example, wherein the silicon content is about 1% to about 20% by weight, the aluminum content is about 0.1% to about 5% by weight, and the remainder is iron.
[0113] In some methods, the selected austenite phase stabilizing donor material is selected from the group consisting of Ni, Mn, Co, Cr, Si, Mo, Nb, Ti, Mg, Cu, Al, N, C, B and combinations thereof. The "combination" in this paragraph means that a plurality of elements can be used alone as austenite phase stabilizing donor materials, such as titanium (Ti) and boron (B); or a plurality of elements are combined into a compound or alloy to be used as an austenite phase stabilizing donor material, such as titanium boride (TiB 2 ); or a combination of these two types.
[0114] In step (c), for example, the selected austenite phase stabilizing donor material may be deposited on the one or more first surface regions using slurry coating, laser cladding, electron beam cladding, electroplating, electroless plating, wire arc deposition, chemical vapor deposition, physical vapor deposition, thermal spraying, plasma spraying, or a combination thereof. In certain embodiments, the selected austenite phase stabilizing donor material is deposited on the first surface regions by laying down a powder, sheet, film, or slab on the one or more first surface regions without laying down on the second surface regions.
[0115] In step (d), the selected austenite phase stabilized donor material is not deposited on one or more second surface regions of the ferromagnetic receptor material. The design of the final soft magnetic body will determine the number, size and distribution of the second surface regions compared to the first surface regions (where the austenite phase stabilized donor material is deposited). Depending on the deposition technique, a person skilled in the art of materials science will understand how to selectively deposit the donor material in the first surface region but not in the second surface region.
[0116] For example, in the case of laser cladding or electron beam cladding, precise cladding in the target area (first surface area) is possible. The cladding is of an austenite phase stabilized donor material, which is not necessarily a solid austenite phase stabilized donor material formed later in step (f). In certain embodiments employing laser cladding in step (c), the laser cladding in step (c) and the laser melting in step (e) are time-coordinated or overlapped, such that during step (c), there is laser melting of the donor material into the first surface area. This can be: sequential, where laser cladding occurs first and then laser melting; or simultaneous, where laser cladding occurs simultaneously with laser melting; or a combination thereof.
[0117] In the case of wire arc deposition, the wire diameter, wire layout, anode-cathode configuration, and electrical power can be optimized to precisely deposit the austenite phase stabilized donor material.
[0118] In the case of chemical vapor deposition, physical vapor deposition, thermal spraying, and plasma spraying, the deposited or sprayed austenite-stabilized donor material can be selectively directed to the target second surface region without the use of a mask in various ways. For example, in selective vapor deposition, high selectivity of deposition of the austenite-stabilized donor material in the first surface region (relative to the second surface region) can be obtained by the different chemical behavior of the reactants with the underlying substrate (in this case, the ferromagnetic receptor material).
[0119] In the case of electroplating or electroless plating, selective plating can be utilized. In some embodiments of selective plating, a brush holds a plating solution. By using a low voltage, a brush immersed in a plating solution allows for localized plating. Selective plating can be used to apply a uniform distribution of plating material on a localized (selective) area corresponding to a first surface area. Unlike full electroplating techniques that require immersion in an electrolyte bath, selective plating uses an electrolyte plating solution and an anode connected to a wire to target a specific area.
[0120] In the case where an austenite-stabilized donor material is deposited in a first surface region by laying down a powder, sheet, or another type of object, there are a variety of ways to perform such deposition in a spatially selective manner. The powder may be selectively laid down in a first region and not in a second region, being careful not to disturb the volume of the powder. This technique is particularly feasible for low concentrations of austenite-stabilized donor material, as electrostatic interactions between the powder and the surface may be sufficient to hold the powder in the intended location. At higher concentrations of austenite-stabilized donor material, a powder binder may be used to combine the powder with a ferromagnetic receptor material. Sheets or films of predetermined size may be selectively laid down in a first region and not in a second region. Likewise, if necessary, a binder may be used to combine the sheet / film with the ferromagnetic receptor material.
[0121] Another variation can utilize a patterned object (e.g., a grid or concentric circle pattern) laid down on the ferromagnetic receptor material, wherein the pattern is a selective pattern of or associated with the first surface area and the second surface area. Note that this is very different from a mask. When a mask is used, the mask physically blocks the laser path to the underlying substrate. In contrast, in these embodiments using a patterned object, the pattern forms areas where material will be deposited, rather than areas where material will be blocked / masked. These embodiments essentially combine steps (c) and (d), in the sense that laying down the patterned object deposits the donor material on one or more first surface areas and simultaneously does not deposit the donor material on one or more second surface areas.
[0122] During step (e) of the variation employing laser melting (rather than laser ablation), there is infiltration of the donor material in molten form. Additional infiltration within the first surface region may occur, typically by diffusion, during and after solidification of the molten donor material into the solid austenite phase stabilized donor material. Because the diffusivity of the donor material is expected to be much higher in the liquid phase than in the solid phase, most of the infiltration will generally occur prior to solidification.
[0123] In some embodiments, the ferromagnetic receptor material does not melt, but remains solid during steps (c), (d), (e), and (f). In other embodiments, the laser energy reaches the ferromagnetic receptor material and a portion (not all) of the receptor material melts. Some ferromagnetic receptor material may be laser melted due to direct exposure to laser photons, such as in gaps between donor material particles or sheets. Alternatively, some ferromagnetic receptor material may be laser melted due to indirect heat transfer from the donor material (after it is melted by the laser energy). It will be appreciated that whether any portion of the ferromagnetic receptor material melts will be determined by its properties (at least its melting point) and the heat and mass transfer within the system, which in turn is affected by the laser power, laser time, amount and thickness of the donor layer, material thermal diffusivity, etc.
[0124] In certain embodiments, a precursor of a selected austenite-stabilizing donor material may be deposited on one or more first surface regions of the ferromagnetic receptor material. The precursor comprises the selected austenite-stabilizing donor material and other elements that are driven off during or after step (e). As an example, when the selected austenite-stabilizing donor material is nitrogen (N), the precursor may be ammonia NH 3 Ammonia can be deposited via vapor deposition, so that NH 3 molecules adsorbed on the surface. During laser melting, NH 3 can be decomposed into: surface-adsorbed N, which remains in the first surface region (and can permeate within the first surface region); and gas-phase H2 , which is released into the atmosphere and does not remain in the first surface region. The local temperature caused by the laser interaction is expected to be high enough for such a decomposition reaction, which can also be catalyzed by the surface of the ferromagnetic acceptor material.
[0125] In step (f), there is a solid austenite phase stabilizing donor material (e.g., see Fig. 8A and Figure 8B ). Ideally, there is complete selectivity such that first surface regions have a uniform concentration of austenite-stabilized donor material permeating those regions, while second surface regions are completely free of any austenite-stabilized donor material. In practice, complete selectivity may be difficult to achieve. Depending on the application of the soft magnetic material and the desired magnetic properties, some tolerances are generally acceptable. In particular, some austenite-stabilized donor material may be located on or in one or more defective second surface regions; likewise, there may be defective first surface regions that do not have austenite-stabilized donor material on or in such defective regions. The selectivity of austenite-stabilized donor material can be quantified as the percentage of austenite-stabilized donor material located on or in the first surface region relative to all austenite-stabilized donor material located on or in all surface regions of the ferromagnetic receptor material. For example, if the austenite-stabilized donor material is located entirely on or in the first surface region, and no donor material is located on or in the second surface region, then the selectivity of the austenite-stabilized donor material is 100%. If the austenite-stabilizing donor material is erroneously located on or in the second surface region, and no donor material is correctly located on or in the first surface region, the selectivity of the austenite-stabilizing donor material is 0%. If the donor material is randomly distributed over all surface regions, and assuming that the total volume of the first and second surface regions is equal, the selectivity of the austenite-stabilizing donor material is 50%. Preferably, the selectivity of the austenite-stabilizing donor material is at least 80%, more preferably at least 90%, most preferably at least 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 99.5%, 99.9%, 99.95%, 99.99% or 100%, including all intermediate ranges.
[0126] In certain alternative embodiments, 100% selectivity is not desired. Rather, in these alternative embodiments, the first surface region has a first concentration of the austenite-stabilizing donor material and the second surface region has a second concentration of the austenite-stabilizing donor material, wherein the second concentration is lower than the first concentration but greater than zero.
[0127] After step (f), the one or more first surface regions may have an average thickness, for example, from about 1 micron to about 3000 microns. In certain embodiments, the average thickness is from about 100 microns to about 500 microns. In various embodiments, the average thickness is about, at least about, or at most about 1, 2, 5, 10, 25, 50, 75, 100, 150, 200, 250, 300, 400, 500, 600, 750, 1000, 1500, 2000, 2500, or 3000 microns, including any intermediate ranges. The average thickness of the first surface region is defined as the depth (in units of length) containing an average of 99 wt % austenite phase stabilized donor material. This definition is used to ignore stray or impure donor elements and is used to take into account embodiments in which the donor material is primarily located on top of the ferromagnetic acceptor material, embodiments in which the donor material is completely infiltrated within the ferromagnetic acceptor material, and embodiments in which the donor material is both present on top of the ferromagnetic acceptor material and infiltrated therein. For illustration, in Fig. 8A In , it is estimated that 99 wt % of the Ni (donor material) is in a layer with a thickness of about 175 μm. Fig. 8A In the embodiment of FIG. 5 , the donor nickel is present both on top of and infiltrated within the ferromagnetic acceptor material FeSi.
[0128] In some embodiments, the solid austenite phase stabilized donor material is located within one or more first surface regions, rather than being a coating disposed only on top of the ferromagnetic acceptor material. A portion of the donor material may be located on top of the first surface region. Preferably, at least a portion of the donor material permeates within the first surface region, such that the donor material is blended (homogeneously or non-homogeneously) with the ferromagnetic acceptor material. This is particularly useful in Figure 8B , where Ni (brighter dots) has clearly infiltrated into the FeSi ferromagnetic acceptor material and is therefore located therein. It is believed that the infiltration of the austenite phase stabilized donor material into the volume of the ferromagnetic acceptor material is beneficial to the magnetic properties. The donor material infiltration is produced by laser melting or laser ablation as disclosed herein.
[0129] Note that as the ferromagnetic acceptor material in molten form moves toward the surface, some amount of penetration of the donor material into the ferromagnetic acceptor material may occur, causing mixing with the donor element. In the reference frame of the donor element, the donor element penetrates into the ferromagnetic acceptor material.
[0130] In some methods, the first average permeability is at least 90% higher than the second average permeability. In certain embodiments, the first average permeability is at least 99% higher than the second average permeability. In different embodiments, the first average permeability is at least 50%, 60%, 70%, 80%, 90%, 99%, 100%, 150%, 200%, 300%, 400%, 500%, 600%, 700%, 800%, 900% or 1000% higher than the second average permeability. The ratio of the first average permeability to the second average permeability is the permeability contrast ratio between the first surface area and the second surface area. For example, when the first average permeability is 1000% higher than the second average permeability, there is a permeability contrast ratio of 10:1 (or an order of magnitude). In various embodiments, the permeability contrast ratio is about or at least about 10: 1, 50: 1, 100: 1, 500: 1, 1000: 1, 2000: 1, 5000: 1, 10000: 1, 20000: 1, or 50000: 1. In various embodiments, the first average permeability is at least two, three, or four orders of magnitude greater than the second average permeability (four orders of magnitude is 10000: 1 contrast, which is preferred in some embodiments).
[0131] In some methods using laser melting, for example, soft magnetic materials are used in rotors in electric motors. The contrast ratio between the magnetic permeability of the first surface region and the magnetic permeability of the second surface region is very useful for rotors, especially for rotors used in electric motors (e.g., electric motors for electric vehicles).
[0132] Other variations provide a method of customizing a surface of a soft magnetic material, the method comprising:
[0133] (a) providing a selected ferromagnetic receptor material;
[0134] (b) providing a selected austenite phase stabilizing donor material;
[0135] (c) depositing a selected austenite phase stabilizing donor material onto one or more first surface regions of a ferromagnetic receptor material;
[0136] (d) not depositing the selected austenite phase stabilizing donor material on the one or more second surface regions of the ferromagnetic receptor material; and
[0137] (e) laser ablating a selected austenite phase-stabilized donor material into the one or more first surface regions to force the selected austenite phase-stabilized donor material to penetrate into the one or more first surface regions to selectively alloy the ferromagnetic receptor material in the one or more first surface regions,
[0138] wherein the one or more first surface regions are characterized by a first average magnetic permeability,
[0139] wherein the one or more second surface regions are characterized by a second average magnetic permeability, and
[0140] The first average magnetic permeability is higher than the second average magnetic permeability.
[0141] Figure 3 is an exemplary flow chart outlining a method for selectively alloying a ferromagnetic receptor material in one or more first surface regions using laser ablation to force infiltration of an austenite phase-stabilized donor material into the first surface region or regions.
[0142] In this specification, "laser ablating" and "laser ablation" are defined as the use of a laser to physically force a first material (in this context, the donor material) into a second material (in this context, the acceptor material). In some embodiments, laser ablation utilizes momentum transfer from the donor material impacting a selected surface of the acceptor material. Through laser ablation, donor atoms can be pushed into the pores or spaces between acceptor material molecules, trapped in the lattice of acceptor material molecules, embedded within acceptor material molecules, dissolved in the same phase as the acceptor material molecules, suspended in another phase different from the acceptor material phase, or a combination thereof. In these embodiments, there may be no loss of acceptor material.
[0143] In other embodiments using laser ablation, there may be erosion of a small portion of the first surface area, thereby ejecting or radiating ferromagnetic receptor material, such as via spalling. This removal of receptor material can provide space for donor material to be pushed in. However, ejection of ferromagnetic receptor material is generally undesirable because receptor material is lost (reduced mass efficiency) and may become accumulated elsewhere as impurities.
[0144] In certain embodiments, laser ablation utilizes a pulsed laser or a high-intensity continuous wave laser beam. Relatively long laser pulses (e.g., nanosecond pulses) may overheat and thermally damage the acceptor material or the donor material, while ultrashort laser pulses (e.g., femtoseconds) cause minimal material damage during processing due to ultrashort light-matter interactions. Excimer lasers with deep ultraviolet light (e.g., wavelengths of approximately 100 nm) can be used for laser ablation.
[0145] A combination of a laser melting mechanism and a laser ablation mechanism may be employed in certain methods of customizing the surface of a soft magnetic material (selectively at one or more first surface regions). When both laser melting and laser ablation are employed, at least a portion of the austenite phase stabilized donor material is melted via a laser. The molten donor material solidifies on or in the one or more first surface regions. At least a portion of the austenite phase stabilized donor material is physically pushed into a ferromagnetic receptor material using the same laser or possibly different lasers. The donor material may be forced into the same first surface region on which / wherein the solidified donor material (from laser melting) resides. Alternatively or additionally, the donor material may be forced into different subsets of the first surface region. In certain embodiments, the donor material is melted and then pushed into the receptor material in the form of molten molecules, which may be solid or molten. In certain embodiments, the first portion of the donor material melts and solidifies on or in some first surface regions, while the second portion of the donor material does not melt but is ablated into the same first surface region and / or other first surface regions.
[0146] When laser melting is combined with laser ablation, it is still preferred not to deposit donor material on or in the second surface area. In principle, a third surface area can be selected and donor material can be deposited on or in the third surface area using laser melting or laser ablation, while donor material can be deposited on or in the first surface area using laser ablation or laser melting, respectively, always avoiding any deposition on or in the second surface area. These embodiments can be employed, for example, where the tailored magnetic properties are different for laser melting than for laser ablation, or when different donor materials are desired in different selected areas.
[0147] In some methods employing laser ablation, in step (c), the austenite phase stabilizing donor material is deposited in the form of powder particles.Alternatively or additionally, in step (c), the austenite phase stabilizing donor material may be deposited in the form of a film, foil or mesh.
[0148] In a preferred embodiment using laser ablation, the method does not use a mask. In a preferred embodiment using laser ablation, the method does not use a chemical treatment.
[0149] In some methods employing laser ablation, the selected ferromagnetic acceptor material is selected from the group consisting of FeSi, FeNi, FeCo, NiCo, FeSiAl, and combinations thereof. For any of these ferromagnetic acceptor materials, various stoichiometries are possible. The elements constituting the ferromagnetic acceptor material may be combined together to form molecules (compounds), may be together in solid solution as a single phase alloy, or may be present in a multiphase alloy.
[0150] As described above for laser melting, when laser ablation is used, it is understood that FeSi refers to Fe x Si y Compounds or alloys in which x and y can take different values to form compounds or alloys of iron and silicon. When x = 1 and y = 1, the compound is iron monosilicide Fe 1 Si 1 When x = 2 and y = 1, the compound is Fe2Si 2 Si. When x = 1 and y = 2, the compound is iron disilicide FeSi 2 , and so on. In some embodiments, FeSi is a ferrosilicon alloy of iron and silicon, for example, wherein the silicon content is about 1%-20% by weight.
[0151] It should be understood that FeNi refers to Fe x Ni y Compounds or alloys, where x and y can take different values to form compounds or alloys of iron and nickel. For example, FeNi can be selected from Fe 1 Ni 1 , Fe 2 Ni、Fe 3 Ni、FeNi 2 In some embodiments, FeNi is a nickel-iron alloy of iron and nickel, for example, wherein the nickel content is about 2%-80% by weight.
[0152] It should be understood that FeCo refers to Fe x Co y Compounds or alloys, where x and y can take different values to form compounds or alloys of iron and cobalt. For example, FeCo can be selected from Fe 1 Co 1 , Fe 2 Co、Fe 3 Compounds of Co or combinations thereof. In some embodiments, FeCo is a cobalt-iron alloy of iron and cobalt, for example wherein the cobalt content is about 10%-90% by weight.
[0153] It should be understood that NiCo refers to Ni x Co y Compounds or alloys, wherein x and y can take different values to form compounds or alloys of nickel and cobalt. For example, NiCo can be selected from Ni1Co1, Ni 2 Co、NiCo 2 In some embodiments, NiCo is a nickel-cobalt alloy having a nickel content of about 1% to about 99% by weight and a cobalt content of about 99% to about 1% by weight.
[0154] It should be understood that FeSiAl refers to Fex Si y Al z Compounds or alloys, wherein x, y and z can take different values to form compounds or alloys of iron, silicon and aluminum. In some embodiments, FeSiAl is a ferrosilicon-aluminum alloy, for example, wherein the silicon content is about 1% to about 20% by weight, the aluminum content is about 0.1% to about 10% by weight, and the remainder is iron.
[0155] In some methods using laser ablation, the selected austenite phase stabilization donor material is selected from the group consisting of Ni, Mn, Co, Cr, Si, Mo, Nb, Ti, Mg, Cu, Al, N, C, B and combinations thereof. The "combination" in this paragraph means that a plurality of elements can be used alone as austenite phase stabilization donor materials, such as nickel (Ni) and boron (B); or a plurality of elements are combined into compounds or alloys to be used as austenite phase stabilization donor materials, such as nickel boride (Ni 2 B); or a combination of these two types.
[0156] When laser ablation is used, in step (c), for example, the selected austenite phase stabilizing donor material may be deposited on the one or more first surface regions using slurry coating, laser cladding, electron beam cladding, electroplating, electroless plating, wire arc deposition, chemical vapor deposition, physical vapor deposition, thermal spraying, plasma spraying, or a combination thereof. In certain embodiments, the selected austenite phase stabilizing donor material is deposited on the first surface regions by laying down a powder, sheet, film, or slab on the one or more first surface regions without laying down on the second surface regions.
[0157] When laser ablation is used, in step (d), the selected austenite phase stabilized donor material is not deposited on one or more second surface regions of the ferromagnetic receptor material. The design of the final soft magnetic body will determine the number, size, and distribution of the second surface regions compared to the first surface regions (where the austenite phase stabilized donor material is deposited). Depending on the deposition technique, a person skilled in the art of materials science will understand how to selectively deposit the donor material in the first surface region but not in the second surface region. The next seven paragraphs further describe different means of depositing the donor material in embodiments using laser ablation.
[0158] In the case of laser cladding or electron beam cladding, precise cladding in the target area (first surface area) is possible. The cladding is of an austenite phase stabilized donor material, which is not necessarily a solid austenite phase stabilized donor material formed later in step (f). In certain embodiments employing laser cladding in step (c), the laser cladding in step (c) and the laser ablation in step (e) are time-coordinated or overlapped, such that during step (c), there is physical penetration (forced) of the donor material into the first surface area. This can be: sequential, where laser cladding occurs first and then laser ablation; or simultaneous, where laser cladding occurs simultaneously with laser ablation; or a combination thereof.
[0159] In the case of wire arc deposition, the wire diameter, wire layout, anode-cathode configuration, and electrical power can be optimized to precisely deposit the austenite phase stabilized donor material.
[0160] In the case of chemical vapor deposition, physical vapor deposition, thermal spraying, and plasma spraying, the deposited or sprayed austenite-stabilized donor material can be selectively directed to the target second surface region without the use of a mask in various ways. For example, in selective vapor deposition, high selectivity of deposition of the austenite-stabilized donor material in the first surface region (relative to the second surface region) can be obtained by the different chemical behavior of the reactants with the underlying substrate (in this case, the ferromagnetic receptor material).
[0161] In the case of electroplating or electroless plating, selective plating can be utilized. In some embodiments of selective plating, a brush holds a plating solution. By using a low voltage, a brush immersed in a plating solution allows for localized plating. Selective plating can be used to apply a uniform distribution of plating material on a localized (selective) area corresponding to a first surface area. Unlike full electroplating techniques that require immersion in an electrolyte bath, selective plating uses an electrolyte plating solution and an anode connected to a wire to target a specific area.
[0162] In the case where an austenite-stabilized donor material is deposited in a first surface region by laying down a powder, sheet, or another type of object, there are a variety of ways to perform such deposition in a spatially selective manner. The powder may be selectively laid down in a first region and not in a second region, being careful not to disturb the volume of the powder. This technique is particularly feasible for low concentrations of austenite-stabilized donor material, as electrostatic interactions between the powder and the surface may be sufficient to hold the powder in the intended location. At higher concentrations of austenite-stabilized donor material, a powder binder may be used to combine the powder with a ferromagnetic receptor material. Sheets or films of predetermined size may be selectively laid down in a first region and not in a second region. Likewise, if necessary, a binder may be used to combine the sheet / film with the ferromagnetic receptor material.
[0163] Another variation can utilize a patterned object (e.g., a grid or concentric circle pattern) laid down on the ferromagnetic receptor material, wherein the pattern is a selective pattern of or associated with the first surface area and the second surface area. Note that this is very different from a mask. When a mask is used, the mask physically blocks the laser path to the underlying substrate. In contrast, in these embodiments using a patterned object, the pattern forms areas where material will be deposited, rather than areas where material will be blocked / masked. These embodiments essentially combine steps (c) and (d), in the sense that laying down the patterned object deposits the donor material on one or more first surface areas and simultaneously does not deposit the donor material on one or more second surface areas.
[0164] During step (e) of the variation employing laser ablation, there is infiltration of the donor material in solid form by forced convection, without being limited by theory. Additional infiltration within the first surface region may occur, such as by diffusion. Because convection of the donor material is expected to be faster than diffusion, typically, when laser ablation is used, most of the donor material infiltration is due to convection caused by the laser ablation.
[0165] In some embodiments employing laser ablation, the ferromagnetic receptor material does not melt, but rather remains solid during steps (c), (d), and (e). In other embodiments, the laser energy reaches the ferromagnetic receptor material, and a portion (not all) of the receptor material melts. Some of the ferromagnetic receptor material may be laser melted due to direct exposure to laser photons, such as in gaps between donor material particles or sheets. Alternatively, some of the ferromagnetic receptor material may be laser melted due to indirect heat transfer from the donor material, rather than from its initial energy from the laser. It will be appreciated that whether any portion of the ferromagnetic receptor material melts will be determined by its properties (at least its melting point) and the heat and mass transfer within the system, which in turn is affected by the laser power, laser time, amount and thickness of the donor layer, thermal diffusivity of the material, etc. Partial melting of the ferromagnetic receptor material may be advantageous because the physical pushing (momentum transfer) of the donor elements can be enhanced when the receptor material is molten rather than solid.
[0166] In certain embodiments employing laser ablation, a precursor of a selected austenite phase stabilizing donor material may be deposited on one or more first surface regions of the ferromagnetic receptor material. The precursor comprises the selected austenite phase stabilizing donor material and other elements driven off during step (e). As an example, when the selected austenite phase stabilizing donor material is boron (B), the precursor may be diborane B 2 H 6 Diborane can be deposited via vapor deposition, making B 2 H6 During laser ablation, or optionally as an additional processing step before laser ablation, B 2 H 6 can be decomposed into: surface-adsorbed B, which can be forced to penetrate into the first surface region; and gas-phase H 2 , which is released into the atmosphere and is not retained in the first surface region. The local temperature caused by laser ablation is expected to be high enough for such a decomposition reaction, which can also be catalyzed by the surface of the ferromagnetic receptor material.
[0167] After step (e) in the method using laser ablation, there is solid austenite phase-stabilized donor material located in (infiltrated into) the one or more first surface regions. Ideally, there is complete selectivity, so that the first surface regions have a uniform concentration of austenite phase-stabilized donor material infiltrated into these regions, while the second surface regions are completely free of any austenite phase-stabilized donor material. In practice, it may be difficult to achieve complete selectivity. Depending on the application of the soft magnetic material and the required magnetic properties, some tolerances are generally acceptable. In particular, some austenite phase-stabilized donor material may be located on or in one or more defective second surface regions; similarly, there may be defective first surface regions that do not have austenite phase-stabilized donor material. The selectivity of austenite phase-stabilized donor material can be quantified as the percentage of austenite phase-stabilized donor material located in the first surface region relative to all austenite phase-stabilized donor material located on or in all surface regions of the ferromagnetic receptor material. For example, if the austenite phase stabilized donor material is completely located in the first surface region and no donor material is located on or in the second surface region, the selectivity of the austenite phase stabilized donor material is 100%. If the austenite phase stabilized donor material is erroneously located on or in the second surface region and no donor material is correctly located in the first surface region, the selectivity of the austenite phase stabilized donor material is 0%. If the donor material is randomly distributed over all surface regions and assuming that the total volume of the first surface region and the second surface region are equal, the selectivity of the austenite phase stabilized donor material is 50%. Preferably, in embodiments employing laser ablation, the selectivity of the austenite phase stabilized donor material is at least 75%, more preferably at least 85%, most preferably at least 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99% or 100%, including all intermediate ranges.
[0168] After step (e) in the method using laser ablation, the one or more first surface regions can have, for example, an average thickness from about 1 micron to about 3000 microns. In certain embodiments, the average thickness is from about 100 microns to about 500 microns. In various embodiments, the average thickness is about, at least about, or at most about 1, 2, 5, 10, 25, 50, 75, 100, 150, 200, 250, 300, 400, 500, 600, 750, 1000, 1500, 2000, 2500, or 3000 microns, including any intermediate ranges. The average thickness of the first surface region is defined as the depth (unit of length) containing an average of 99 wt% austenite phase stabilized donor material. This definition is used to ignore stray or impurity donor elements and to take into account different penetration depths of donor materials.
[0169] In embodiments employing laser ablation, the solid austenite phase stabilized donor material is preferably located within one or more first surface regions, rather than being merely a coating disposed on top of the ferromagnetic receptor material. A portion of the donor material may be located on top of the first surface region. For example, a few atoms of the donor material may not have sufficient momentum to penetrate further than the surface. Due to force-derived penetration, the donor material blends (homogeneously or non-homogeneously) with the ferromagnetic receptor material. It is believed that penetration of the austenite phase stabilized donor material into the volume of the ferromagnetic receptor material is beneficial to the magnetic properties.
[0170] In some methods employing laser ablation, the first average permeability is at least 90% higher than the second average permeability. In certain embodiments, the first average permeability is at least 99% higher than the second average permeability. In various embodiments employing laser ablation, the first average permeability is at least 50%, 60%, 70%, 80%, 90%, 99%, 100%, 150%, 200%, 300%, 400%, or 500% higher than the second average permeability. When the first average permeability is 500% higher than the second average permeability, there is a 5:1 permeability contrast ratio of the first surface area to the second surface area.
[0171] In some methods using laser ablation, for example, soft magnetic materials are used in rotors in electric motors.
[0172] In some methods employing laser melting or laser ablation, an electromagnetic field is applied during the fabrication of the soft magnetic material. During one or more steps, an electromagnetic field may be applied to the ferromagnetic receptor material.
[0173] Figure 4is a schematic diagram showing two electromagnets, one of which acts as the North (N) magnetic pole and the other acts as the South (S) magnetic pole. An electromagnet is a magnet in which a magnetic field is generated by an electric current. The electromagnet can be composed of a wire (e.g., a copper wire) wound into a coil. The current passing through the wire creates a magnetic field that is concentrated in a hole in the center of the coil. The electromagnet NS pair is separated from a receptor sheet (ferromagnetic receptor material), a donor layer (austenite phase stabilized donor material), and a laser configured for laser melting or laser ablation of the donor material. The ferromagnetic receptor material is a soft magnetic material that is being customized. In Figure 4 , for the purpose of this illustration, only the first surface area is depicted, while the second surface area is not depicted.
[0174] Figure 5 is similar to Figure 4 Schematic diagram showing a north (N) magnetic pole and a south (S) magnetic pole. The N and S poles are spaced so that when a current is applied to the electromagnet, a magnetic field is generated. Figure 5 In a simplified manner, it is depicted as a wavy magnetic field line. The NS pole spacing can vary from about 0.1 mm to about 1 m, such as from about 1 mm to about 100 mm. The strength of the magnetic field can vary so that the magnetic flux density is from about 0.01 T to about 10 T, such as from about 0.1 T to about 1 T. Figure 5 In the present invention, there is an acceptor sheet (ferromagnetic acceptor material), a donor layer (austenite phase stabilized donor material), and a laser configured for laser melting or laser ablation of the donor material. The ferromagnetic acceptor material is a soft magnetic material being tailored. Figure 5 In the embodiment of the invention, only the first surface region is depicted, and the second surface region is not depicted, for the purpose of this illustration. Preferably, the electromagnet and the ferromagnetic receptor material are configured so that when the electromagnet is turned on, there are electromagnetic field lines that pass through the donor material and through the first surface region being customized. The electromagnetic field lines may also pass through portions of the ferromagnetic receptor material that are not being customized, such as deeper into the first surface region, the second surface region, etc. The electromagnetic field lines may intersect with and pass through the laser.
[0175] In the method using laser melting and applying an electromagnetic field, the electromagnetic field may be applied during step (c), during step (d), during step (e), and / or during step (f). In the method using laser ablation and applying an electromagnetic field, the electromagnetic field may be applied during step (c), during step (d), and / or during step (e).
[0176] Electromagnetic fields can be beneficial during laser melting and solidification of an austenite phase-stabilizing donor material and, optionally, during laser melting and solidification of a portion of a ferromagnetic acceptor material. For example, electromagnetic fields can have advantages in terms of crystal structure. For more details, see the section entitled "Microstructure Evolution and Control During Laser-Based Additive Manufacturing with Optional Electromagnetic Fields" later in this specification. In addition, U.S. Patent Application Publication No. 20220044870A1, published on February 10, 2022, is hereby incorporated by reference herein.
[0177] Some variations provide a soft magnet having surface-tailored magnetic permeability, wherein the soft magnet comprises:
[0178] (i) a first region comprising a first core region and a first surface region, wherein the first core region comprises a ferromagnetic material, and wherein the first surface region comprises an austenite phase stabilizing donor material; and
[0179] (ii) a second region comprising a second core region, wherein the second core region comprises a ferromagnetic material, and wherein the second region does not comprise an austenite phase stabilizing donor material;
[0180] wherein the first surface region has an average thickness from about 1 micron to about 3000 microns,
[0181] wherein the first region is characterized by a first average magnetic permeability,
[0182] wherein the second region is characterized by a second average magnetic permeability, and
[0183] The first average magnetic permeability is higher than the second average magnetic permeability.
[0184] Certain embodiments provide a soft magnet having surface-tailored magnetic permeability, wherein the soft magnet comprises:
[0185] (i) a first region comprising a first core region and a first surface region, wherein the first core region comprises a ferromagnetic material, and wherein the first surface region comprises a first concentration of an austenite phase stabilizing donor material; and
[0186] (ii) a second region comprising a second core region and a second surface region, wherein the second core region comprises a ferromagnetic material, wherein the second surface region comprises a second concentration of an austenite-stabilizing donor material, and wherein the second concentration of the austenite-stabilizing donor material is lower than the first concentration of the austenite-stabilizing donor material;
[0187] wherein the first surface region has an average thickness from about 1 micron to about 3000 microns,
[0188] wherein the first region is characterized by a first average magnetic permeability,
[0189] wherein the second region is characterized by a second average magnetic permeability, and
[0190] The first average magnetic permeability is higher than the second average magnetic permeability.
[0191] Some variations provide a soft magnetic body produced by a process comprising:
[0192] (a) providing a selected ferromagnetic receptor material;
[0193] (b) providing a selected austenite phase stabilizing donor material;
[0194] (c) depositing a selected austenite phase stabilizing donor material onto one or more first surface regions of a ferromagnetic receptor material;
[0195] (d) not depositing the selected austenite phase stabilizing donor material on the one or more second surface regions of the ferromagnetic receptor material;
[0196] (e) laser melting a selected austenite phase stabilizing donor material into the one or more first surface regions to form molten austenite phase stabilizing donor material; and
[0197] (f) solidifying the molten austenite phase stabilized donor material to form a solid austenite phase stabilized donor material located within the one or more first surface regions, thereby selectively alloying the ferromagnetic acceptor material within the one or more first surface regions,
[0198] This produces soft magnets with surface-tailored magnetic permeability.
[0199] wherein the one or more first surface regions are characterized by a first average magnetic permeability after the selective alloying in step (f),
[0200] wherein the one or more second surface regions are characterized by a second average magnetic permeability, and
[0201] The first average magnetic permeability is higher than the second average magnetic permeability.
[0202] Some variations provide a soft magnetic body produced by a process comprising:
[0203] (a) providing a selected ferromagnetic receptor material;
[0204] (b) providing a selected austenite phase stabilizing donor material;
[0205] (c) depositing a selected austenite phase stabilizing donor material onto one or more first surface regions of a ferromagnetic receptor material;
[0206] (d) not depositing the selected austenite phase stabilizing donor material on the one or more second surface regions of the ferromagnetic receptor material; and
[0207] (e) laser ablating a selected austenite phase-stabilized donor material into the one or more first surface regions to force the selected austenite phase-stabilized donor material to penetrate into the one or more first surface regions to selectively alloy the ferromagnetic receptor material in the one or more first surface regions,
[0208] This produces soft magnets with surface-tailored magnetic permeability.
[0209] wherein the one or more first surface regions are characterized by a first average magnetic permeability,
[0210] wherein the one or more second surface regions are characterized by a second average magnetic permeability, and
[0211] The first average magnetic permeability is higher than the second average magnetic permeability.
[0212] In some soft magnets, the ferromagnetic material is selected from the group consisting of FeSi, FeNi, FeCo, NiCo, FeSiAl and combinations thereof. For any of these ferromagnetic materials, various stoichiometries are possible. The elements constituting the ferromagnetic material may be combined together to form molecules (compounds), may be together in solid solution as a single-phase alloy, or may be present in a multiphase alloy.
[0213] It should be understood that FeSi refers to Fe x Si y Compounds or alloys in which x and y can take different values to form compounds or alloys of iron and silicon. When x = 1 and y = 1, the compound is iron monosilicide Fe 1 Si 1 When x = 2 and y = 1, the compound is Fe2Si 2 Si. When x = 1 and y = 2, the compound is iron disilicide FeSi 2, and so on. In some embodiments, FeSi is a ferrosilicon alloy of iron and silicon, for example, wherein the silicon content is about 1%-20% by weight.
[0214] It should be understood that FeNi refers to Fe x Ni y Compounds or alloys, where x and y can take different values to form compounds or alloys of iron and nickel. For example, FeNi can be selected from Fe 1 Ni 1 , Fe 2 Ni、Fe 3 Ni、FeNi 2 In some embodiments, FeNi is a nickel-iron alloy of iron and nickel, for example, wherein the nickel content is about 2%-80% by weight.
[0215] It should be understood that FeCo refers to Fe x Co y Compounds or alloys, where x and y can take different values to form compounds or alloys of iron and cobalt. For example, FeCo can be selected from Fe 1 Co 1 , Fe 2 Co、Fe 3 Compounds of Co or combinations thereof. In some embodiments, FeCo is a cobalt-iron alloy of iron and cobalt, for example wherein the cobalt content is about 10%-90% by weight.
[0216] It should be understood that NiCo refers to Ni x Co y Compounds or alloys, wherein x and y can take different values to form compounds or alloys of nickel and cobalt. For example, NiCo can be selected from Ni1Co1, Ni 2 Co、NiCo 2 In some embodiments, NiCo is a nickel-cobalt alloy having a nickel content of about 1% to about 99% by weight and a cobalt content of about 99% to about 1% by weight.
[0217] It should be understood that FeSiAl refers to Fe x Si y Al z Compounds or alloys, wherein x, y and z can take different values to form compounds or alloys of iron, silicon and aluminum. In some embodiments, FeSiAl is a ferrosilicon-aluminum alloy, for example, wherein the silicon content is about 10% to about 40% by weight, the aluminum content is about 22% to about 55% by weight, and the remainder is iron.
[0218] In some soft magnets, the austenite phase stabilization donor material is selected from the group consisting of Ni, Mn, Co, Cr, Si, Mo, Nb, Ti, Mg, Cu, Al, N, C, B and combinations thereof. The "combination" in this paragraph means that a plurality of elements can be used alone as austenite phase stabilization donor materials, such as titanium (Ti) and nitrogen (N); or a plurality of elements are combined into compounds or alloys to be used as austenite phase stabilization donor materials, such as titanium nitride (TiN); or a combination of these two types.
[0219] The soft magnetic body may include multiple instances of the first region and / or the second region. Figure 6 ), there are multiple first areas and multiple second areas. The "first surface area" mentioned herein will be understood to also refer to multiple first surface areas, such as 2, 3, 4, 5, 6, 7, 8, 9, 10 or more individual first surface areas with customized magnetic properties. Similarly, the "second surface area" mentioned herein will be understood to also refer to multiple second surface areas, such as 2, 3, 4, 5, 6, 7, 8, 9, 10 or more individual second surface areas with customized magnetic properties. Vice versa; in certain embodiments where alloy deposition is customized for a specific area, the reference to the plural form of "first surface areas" will be understood to refer to a single first surface area. Finally, in certain embodiments where alloy deposition and magnetic customization are avoided in a specific local area, the reference to the plural form of "second surface areas" will be understood to refer to a single second surface area.
[0220] In some soft magnetic bodies, there is a solid austenite phase stabilizing donor material located on or in one or more first surface regions (see, e.g., Fig. 8A and Figure 8B). Ideally, there is complete selectivity, such that first surface regions have a uniform concentration of austenite-stabilizing donor material permeating these regions, while second surface regions are completely free of any austenite-stabilizing donor material. In practice, complete selectivity may be difficult to achieve. Depending on the application of the soft magnet and its required magnetic properties, some tolerances are generally acceptable. In particular, some austenite-stabilizing donor material may be located on or in one or more defective second surface regions; likewise, there may be defective first surface regions that do not have austenite-stabilizing donor material on or in such defective regions. The selectivity of austenite-stabilizing donor material can be quantified as the percentage of austenite-stabilizing donor material located on or in the first surface region relative to all austenite-stabilizing donor material located on or in all surface regions of the ferromagnetic material. For example, if the austenite-stabilizing donor material is located entirely on or in the first surface region, and no donor material is located on or in the second surface region, the selectivity of the austenite-stabilizing donor material is 100%. If the austenite phase stabilizing donor material is erroneously located on or in the second surface region, and no donor material is correctly located on or in the first surface region, the selectivity of the austenite phase stabilizing donor material is 0%. If the donor material is randomly distributed on all surface regions, and assuming that the total volume of the first surface region and the second surface region are equal, the selectivity of the austenite phase stabilizing donor material is 50%. Preferably, in the disclosed soft magnet, the selectivity of the austenite phase stabilizing donor material is at least 80%, more preferably at least 90%, most preferably at least 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 99.5%, 99.9%, 99.95%, 99.99% or 100%, including all intermediate ranges.
[0221] Note that a selectivity of 0% with respect to the first surface area is equivalent to a selectivity of 100% with respect to the second surface area. According to convention, in this patent application, first surface areas are those surface areas for which magnetic tailoring is to be performed.
[0222] In some alternative soft magnets, the first surface region has a first concentration of austenite phase stabilizing donor material, and the second surface region has a second concentration of austenite phase stabilizing donor material, wherein the second concentration is lower than the first concentration but higher than 0. In these embodiments, the selectivity (as defined in the previous paragraph) should be higher than 50%, but need not be close to 100%. In different embodiments of these alternative soft magnets, the selectivity of the austenite phase stabilizing donor material is at least 60%, preferably at least 70%, and more preferably at least 80%.
[0223] In some soft magnets, the one or more first surface regions may have an average thickness, for example, from about 1 micron to about 3000 microns. In certain embodiments, the average thickness is from about 100 microns to about 500 microns. In different soft magnets, the average thickness is about, at least about, or at most about 1, 2, 5, 10, 25, 50, 75, 100, 150, 200, 250, 300, 400, 500, 600, 750, 1000, 1500, 2000, 2500, or 3000 microns, including any intermediate ranges. The average thickness of the first surface region is defined as the depth (unit of length) containing an average of 99 wt% austenite phase stabilized donor material. This definition is used to ignore stray or impurity donor elements, and is used to take into account embodiments in which the donor material is primarily located on top of the ferromagnetic material, embodiments in which the donor material is completely infiltrated in the ferromagnetic material, and embodiments in which the donor material is both present on top of the ferromagnetic material and infiltrated therein. For illustration, in Fig. 8A In , it is estimated that 99 wt % of the Ni (donor material) is in a layer with a thickness of about 175 μm. Fig. 8A In the embodiment of FIG. 5 , the donor nickel is present both on top of the ferromagnetic material FeSi and infiltrated therein.
[0224] In some soft magnetic bodies, the austenite phase stabilizing donor material is located within one or more first surface regions, rather than being a coating disposed only on top of the ferromagnetic material. A portion of the donor material may be located on top of the first surface region. Preferably, at least a portion of the donor material permeates within the first surface region, such that the donor material is blended (homogeneously or non-homogeneously) with the ferromagnetic material. This is for example Figure 8B , where Ni (brighter dots) has clearly infiltrated into the FeSi ferromagnetic material and is therefore located therein. It is believed that the infiltration of the austenite phase stabilizing donor material into the bulk of the ferromagnetic material is beneficial for the magnetic properties.
[0225] In the first region of the soft magnetic body, for example, the thickness of the first surface region can be about 0.1% to about 50% of the thickness of the first core region. Typically, the thickness of the first surface region is about 0.5% to about 10% of the thickness of the first core region, unless there is deep penetration of the donor material due to, for example, high laser power. In various embodiments, the thickness of the first surface region accounts for about, at least about, or at most about 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 50% of the thickness of the first core region, including all intermediate ranges.
[0226] In some soft magnets, the first average magnetic permeability is at least 90% higher than the second average magnetic permeability. In some soft magnets, the first average magnetic permeability is at least 99% higher than the second average magnetic permeability. In different soft magnets, the first average magnetic permeability is at least 50%, 60%, 70%, 80%, 90%, 99%, 100%, 150%, 200%, 300%, 400%, 500%, 600%, 700%, 800%, 900% or 1000% higher than the second average magnetic permeability. When the first average magnetic permeability is 1000% higher than the second average magnetic permeability, there is a 10:1 magnetic permeability contrast ratio of the first surface area to the second surface area, which provides a beneficial soft magnet. The ratio of the first average magnetic permeability to the second average magnetic permeability is the "magnetic permeability contrast ratio" between the first surface area and the second surface area. In various embodiments, the permeability contrast ratio is about or at least about 10:1, 50:1, 100:1, 500:1, 1000:1, 2000:1, 5000:1, 10000:1, 20000:1, or 50000:1.
[0227] For example, soft magnets may be used in rotors in electric motors. A high contrast ratio between the magnetic permeability of the first surface region and the magnetic permeability of the second surface region is very useful for rotors, especially for use in electric motors, such as electric motors for electric vehicles.
[0228] Figure 6 is a schematic illustration of a soft magnet with surface-tailored magnetic permeability. Figure 6 In the soft magnetic material, there are multiple high permeability regions (with dotted shadows) and multiple low permeability regions (white). Figure 6 In some variations of, at different levels of permeability contrast ratio, the shaded areas have a first average permeability and the white areas have a second average permeability lower than the first average permeability. Figure 6 In other variations of the present invention, there are two distinct low permeability regions. One of the low permeability regions is air, indicated by white shading. The other low permeability region is formed by bridges and pillars connecting high permeability regions, which are indicated by dotted shading. In these variations, the bridges and pillars are depicted as solid lines connecting high permeability regions (in Figure 6 Different levels of permeability contrast ratio between bridges and pillars of high permeability regions are possible, such as 10000:1 or even higher.
[0229] Microstructure evolution and control during laser-based additive manufacturing using optional electromagnetic fields
[0230] Current manufacturing methods (e.g., pressing and sintering) are inherently limited in geometry by the shape of the mold (typically prismatic) and the loss of final net shape due to shrinkage during sintering. In contrast, laser-based additive manufacturing is able to manufacture complex three-dimensional geometries without the costs and material losses associated with subtractive manufacturing methods (such as machining to the final net shape).
[0231] Additive manufacturing provides control over crystal orientation. The final crystal orientation of the grains depends on several contributing thermodynamic driving forces. For example, one such factor is the direction of the maximum thermal gradient, where solidifying cubic crystals tend to orient themselves in a <100> Orientation-preferential growth. Thermal gradients can be controlled using laser scanning strategies, by localized heating in various spatially and / or temporally varying patterns. The formation of crystal texture can also be tailored during solidification and subsequent solid-state transformation by applying an external magnetic field, potentially producing more texture uniformity with specific localization and orientation.
[0232] In some embodiments, the magnetic properties are improved by controlling the crystal orientation (texture) of the grains in addition to the magnetization orientation in the microstructure. This control is particularly powerful when both the crystal texture and the magnetic orientation are tailored in a synergistic manner during additive manufacturing. To this end, the grains can be crystallographically oriented in the direction (or directions) that allows the highest remanent magnetization; at the same time, a magnetic field can be applied to orient the magnetization in that same direction. The result is a magnet with an optimal crystal orientation and magnetic orientation, and therefore a maximum energy product. Magnetic materials can also be optimized by 3D optimization of the crystal texture in areas susceptible to demagnetization. By employing additive manufacturing, local thermal, magnetic, and stress fields can be manipulated in the production of magnetic materials with selected crystal textures that are location-specific.
[0233] Additive manufacturing offers the opportunity to tailor the local structure voxel by voxel in a serial layered process. The processed voxel is the volume affected by the heat input from the direct energy source in a layer-based approach, which includes the melt pool as well as the surrounding heat-affected zone. The solidifying crystal texture can be controlled by the direction of heat extraction. In addition to the thermal field, a magnetic field can be applied during processing to control both the crystal texture and the magnetization orientation. The external magnetic field can be generated, for example, by means of an induction coil, multiple induction coils, a permanent magnet or an array of permanent magnets.
[0234] In the present description, additive manufacturing can be utilized in a variety of ways. In a soft magnetic body having surface-tailored magnetic permeability, the one or more first surface regions can be additively manufactured using laser melting and solidification of a donor material. Additionally, the entire soft magnetic body can be additively manufactured, including ferromagnetic materials. Although Figure 1The bulk alloy in is illustrated as having a simple rectangular geometry, which is for illustrative purposes only. By using additive manufacturing of the bulk alloy, arbitrary 3D shapes can be manufactured. Additive manufacturing (also known as 3D printing) of ferromagnetic receptor materials can be performed before depositing donor materials (alloying elements). Alternatively, additive manufacturing of ferromagnetic receptor materials can be performed simultaneously with depositing donor materials and before laser melting or laser ablation of the donor material. For example, donor material deposition can be integrated into the additive manufacturing of ferromagnetic receptor materials, or can be another step that is also interpreted as additive manufacturing. In certain embodiments, the manufacture of ferromagnetic receptor materials, selective deposition of donor materials on one or more first surface regions, laser melting / solidification and / or laser ablation are integrated into the additive manufacturing process. In this section, the discussion of microstructure and texture control can be applicable to any area of additively manufactured soft magnets.
[0235] Some embodiments enable control of solidification of additively manufactured or welded microstructures at the order of a single domain limit (e.g., about 1 μm to 5 μm) to maximize resistance to demagnetization in addition to controlling the orientation of the easy axis (or at least one easy axis when more than one is present). Certain embodiments take advantage of easy axis alignment in magnet regions of interest (e.g., surfaces or corners) to improve overall resistance to demagnetization in bulk magnets. Certain embodiments manipulate solidification by controlling electromagnetic fields to increase the total energy product of additively manufactured or welded magnets.
[0236] By manufacturing the magnet in an additive manner, where laser melting and solidification in each layer occurs voxel by voxel, the magnetic orientation of each voxel can be independently aligned. Independent voxel alignment can be achieved by applying a magnetic field during additive manufacturing, such as during the cooling process of each voxel (including solidification and solid state transition). If desired, the magnetic orientation of each voxel can be set independently of all other voxels.
[0237] In some embodiments, the magnetic orientation is arranged so as to produce a field with certain areas of concentrated magnetic flux. These embodiments are useful, for example, to resist demagnetization in certain areas, or to optimize the air gap flux in the case of a motor producing torque. Near sharp geometric features (e.g., edges), high flux densities may be encountered at non-optimal angles, resulting in nucleation of reverse domains, which leads to partial or complete demagnetization of the magnet. To resist such early demagnetization, the orientation of the magnetic alignment can be selected or adjusted to optimize the angle between the crystal orientation and the magnetic orientation of the susceptible area. Some embodiments take into account the Wigner-Seitz angle dependence of the magnetic coercivity. Advantages of some embodiments include the possibility of utilizing stronger external fields as well as higher temperatures.
[0238] Magnet material costs make up up to 70% of the total cost of an electric motor and are a limiting factor in the widespread adoption of electric vehicles. Magnet costs can be significantly improved by using additive manufacturing to produce near-net-shape products that incur minimal material waste during production.
[0239] In addition, by improving the demagnetization resistance of the magnetic architecture through tailored crystal textures, the mass and volume efficiency of the magnet can be increased, thereby reducing the amount of material required to match the performance efficiency of the motor or other magnet application. This benefit, combined with the ability to produce optimized magnet shapes to optimize field effectiveness, can also improve magnet motor efficiency in addition to reducing the overall cost of manufacturing.
[0240] Epitaxial dendrite solidification tends to grow in the direction of the maximum thermal gradient. However, in the presence of an externally applied magnetic field, the solidification direction may become misaligned with the maximum thermal gradient. Adjustment of the electromagnetic field direction affects the texture evolution and provides an additional lever other than the dendrite solidification direction.
[0241] A magnetically susceptible material is one that will be magnetized in an applied magnetic field. Magnetic susceptibility indicates whether a material is attracted into or repelled from a magnetic field. Paramagnetic materials align with the applied field and are attracted to areas of larger magnetic fields. Diamagnetic materials are anti-aligned and are pushed toward areas of lower magnetic fields. Above an applied field, the magnetization of a material increases its own magnetic field. The magnetizability of materials is caused by the atomic-scale magnetic properties of the particles from which they are made, typically determined by the magnetic moment of the electrons.
[0242] The "magnetic axis" is the straight line connecting the two poles of a magnetized body. The torque exerted on the magnet by a magnetic field in the direction of the magnetic axis is equal to zero. The "crystal texture" is the distribution of crystal orientations of a polycrystalline material. The "crystal orientation" is defined by the planar (Miller) indices of the lattice planes of the crystal.
[0243] In some embodiments, the magnetic field orientation is selected to control the crystal texture within the magnetic metal layer, but not necessarily the magnetic axis. In some embodiments, the magnetic field orientation is selected to control the magnetic axis within the magnetic metal layer, but not necessarily the crystal texture. In certain embodiments, the magnetic field orientation is selected to control both the crystal texture and the magnetic axis within the magnetic metal layer.
[0244] The energy source for additive manufacturing can be a laser beam, an electron beam, or both a laser beam and an electron beam. The energy source preferably applies a thermal gradient that melts a portion of the feedstock composition in the scanning direction, rather than bulk melting the entire feedstock composition. In some embodiments, additive manufacturing utilizes a technology selected from the group consisting of selective laser melting, electron beam melting, laser engineered net shaping, selective laser sintering, direct metal laser sintering, laser melting integrated with machining, laser powder injection, laser consolidation, direct metal deposition, directed energy deposition, plasma arc-based manufacturing, ultrasonic consolidation, arc melting, welding, and combinations thereof.
[0245] An additively manufactured object may comprise a plurality of voxels. A "voxel" is a three-dimensional (3D) pixel. A plurality of voxels form a single layer having a thickness defined by the voxel height. In some embodiments, a single voxel is defined by a characteristic voxel length scale selected from about 50 microns to about 1000 microns. In certain embodiments, the characteristic voxel length scale is selected from about 100 microns to about 500 microns. An exemplary voxel is on the order of 100 μm x 100 μm x 100 μm. Another exemplary voxel is on the order of 10 μm x 10 μm x 10 μm.
[0246] The geometry of the voxel can be a cube, but this is not necessary. For example, the voxel can be rectangular or can have an irregular shape. For any voxel geometry, there is a characteristic voxel length scale equivalent to the cube root of the average voxel volume. The characteristic voxel length scale can be about, at least about, or at most about 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 15, 20, 25, 30, 40, 50, 75, 100, 125, 150, 200, 250, 300, 350, 400, 450, 500, 600, 700, 800, 900 or 1000 microns, including all intermediate ranges (e.g., 100 to 500 microns). The characteristic voxel length scale is typically a function of the laser or electron beam intensity, beam diameter, scan speed, and the properties of the manufactured material (e.g., kinematic viscosity).
[0247] In some embodiments of additive manufacturing, there is solidification of a single voxel, and the magnetic field can be varied voxel by voxel if desired. Using a highly localized energy source, and possibly using different compositions during manufacturing, small voxels of structure with specific crystal orientations and magnetic properties can be produced independently of other voxels.
[0248] Depending on the intensity of the energy transferred, each voxel can be produced, for example, by melting and solidification of the starting material or by sintering or other heat treatment of the material region. During solidification, the voxel in molten form produces one or more solid grains having a single crystal structure. In some embodiments, the solidified voxel contains a single grain. In other embodiments, the solidified voxel contains a plurality of grains having some distribution of crystal orientation and magnetic orientation. Geometrically, a single voxel can have the same size as a single grain, or can be larger than the average grain size within the magnetic metal layer. In various embodiments, the average voxel contains about, at least about, or at most about 1, 1.5, 2, 2.5, 3, 4, 5, 6, 7, 8, 9, 10, 15, 20, 25, 50, 75 or 100 grains, including all intermediate ranges.
[0249] When a voxel contains multiple grains, each with its own crystal orientation and magnetic easy axis, the voxel will have a voxel average crystal orientation and a voxel average magnetic easy axis. In some embodiments, the voxels are configured so that all grains have the same or similar crystal orientation and / or magnetic easy axis. In other embodiments, the voxels are configured so that individual grains have different crystal orientations and / or magnetic easy axes.
[0250] The magnetic metal layer from additive manufacturing has a crystal texture resulting from individual grains, which in turn form voxels. There is a magnetic easy axis for each grain, an average magnetic easy axis for each voxel, and an average magnetic easy axis for the magnetic metal layer. There can be varying degrees of alignment between these graded magnetic easy axes.
[0251] In some embodiments, a voxel contains a plurality of grains having a narrow distribution of crystal orientations along the easy axis of the crystal, and co-aligned magnetic domains contained within each grain. This co-alignment produces a maximum total residual magnetic flux for the voxel. In a larger structure having a plurality of voxels, there may be a narrow distribution of crystal orientations along the easy axis, and co-aligned magnetic domains contained within each voxel. This co-alignment produces a maximum total residual magnetic flux for the structure.
[0252] The grain size can vary widely, such as from about 0.1 micron to about 1000 microns. In various embodiments, the average grain size (within a given voxel or throughout the structure) can be about, at least about, or at most about 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.5, 2, 2.5, 3, 3.5, 4, 5, 6, 7, 8, 9, 10, 15, 20, 25, 30, 35, 40, 45, 50, 75, 100, 125, 150, 200, 250, 300, 350, 400, 500, 600, 700, 800, 900, or 1000 microns.
[0253] Grain size can be measured by a variety of techniques, including, for example, dynamic light scattering, laser diffraction, or image analysis. Dynamic light scattering is a non-invasive established technique for measuring the size and size distribution of particles typically in the submicron region (and the latest technology is even 1 nanometer). Laser diffraction is a widely used particle size measurement technique for materials ranging in size from hundreds of nanometers to several millimeters. Exemplary dynamic light scattering instruments and laser diffraction instruments for measuring particle size can be obtained from Malvern Instruments Ltd., Worcestershire, UK. Image analysis can be performed directly on micrographs, scanning electron micrographs or other images to estimate grain size and distribution.
[0254] In some embodiments, the magnetic field orientation is selected to control voxel-specific magnetic axes within a plurality of individual voxels contained within the magnetic metal layer. In these or other embodiments, the magnetic field orientation is selected to control voxel-specific crystal textures within a plurality of individual voxels contained within the magnetic metal layer.
[0255] When multiple solid layers are generated by sequentially solidifying multiple melt layers in the build direction, the magnetic field orientation can be adjusted in the build direction. In other words, in addition to the variation of the magnetic field orientation within a layer (voxel-specific magnetic field orientation), the magnetic field orientation can be different from one layer to another.
[0256] The atomic structure of a crystal introduces a preferred direction of magnetization. This is called magnetocrystalline anisotropy. The "magnetic easy axis" is the direction inside the crystal along which a small applied magnetic field is sufficient to achieve saturation magnetization. There can be a single easy axis or multiple easy axes. The "magnetic hard axis" is the direction inside the crystal along which a large applied magnetic field is required to achieve saturation magnetization. The magnetic easy axis and the magnetic hard axis will exist regardless of whether a magnetic field is actually applied. The magnetic easy axis is different from the magnetic axis. The magnetic axis only exists when a magnetic field is actually applied, while the magnetic easy axis is a fixed property of a given crystalline material.
[0257] In some embodiments, the magnetic field orientation may be selected to control voxel-specific magnetic easy axes within a plurality of individual voxels contained within the magnetic metal layer.
[0258] In some embodiments, individual voxels are substantially magnetically aligned with each other with reference to the magnetic easy axis of each voxel within a given magnetic metal layer. "Substantially magnetically aligned" means that based on the calculation of all magnetic easy axes within the magnetic metal layer, there is a standard deviation of less than 25°, less than 20°, less than 10°, or less than 5°. In certain embodiments, all magnetic easy axes are substantially aligned so that the standard deviation is less than 2°, less than 1°, less than 0.5°, less than 0.1°, or about 0°. Remanence measurements can be used to determine the alignment of the magnetic easy axes. See McCurrie, "Determination of the degree of easy axis alignment in uniaxial permanent magnets from remanence measurements," Journal of Applied Physics 52, 7344 (1981), which is incorporated herein by reference.
[0259] In some embodiments, the magnetic field orientation is selected to control a voxel-specific magnetic axis and a voxel-specific magnetic easy axis within a plurality of individual voxels contained within the magnetic metal layer, wherein the voxel-specific magnetic axis is substantially aligned with the voxel-specific magnetic easy axis for at least a portion of the magnetic metal layer. In some embodiments, the voxel-specific magnetic axis is substantially aligned with the voxel-specific magnetic easy axis for all of the magnetic metal layer.
[0260] In other embodiments, the magnetic field orientation is selected to control a voxel-specific magnetic axis and a voxel-specific magnetic easy axis within a plurality of individual voxels contained within the magnetic metal layer, wherein, for at least a portion of the magnetic metal layer, the voxel-specific magnetic axis is configured at an angle to the voxel-specific magnetic easy axis.
[0261] In some methods, additive manufacturing conditions are controlled such that a thermal gradient helps create a crystalline texture within the magnetic metal layer.
[0262] In some embodiments, different feedstock compositions, each including one or more magnetic materials or magnetically susceptible materials, are exposed to an energy source. Crystal texture can be adjusted during additive manufacturing. Different feedstock compositions can be not only different species, but also different concentrations of the same species.
[0263] Different raw material compositions can produce graded compositions. For example, the concentration of magnetic rare earth elements can be adjusted throughout the magnetic structure. One example uses local doping of Dy, Nd or Yb in susceptible areas for demagnetization. Local doping can be achieved, for example, via a spray additive process.
[0264] Some embodiments specifically optimize crystal texture sites throughout the volume of a soft magnet. Compared to conventionally processed magnetic materials having a single easy axis orientation or a narrow distribution of easy axis orientations, the texture-controlled magnets disclosed herein can have an easy axis orientation that is tailored to resist the demagnetization field in high susceptibility regions of demagnetization. Such regions can exist where the demagnetization field is highly concentrated and / or the orientation changes rapidly relative to the magnetic field direction, such as at corners.
[0265] The interface between domains is susceptible to domain reversal (demagnetization) due to the relatively low nucleation barrier. The optimal easy axis orientation relative to the external magnetic field preferably increases the energy barrier for nucleation of reverse magnetic domains, thereby maintaining magnetization. For example, by matching a single magnetic domain with a single grain, the resistance to domain reversal within the grain is minimized, thereby increasing the energy barrier for nucleation of reverse domains.
[0266] In some embodiments, without limitation, the additive manufacturing feedstock is a powder functionalized with a plurality of nanoparticle surfaces. The nanoparticles can promote heterogeneous nucleation in the melt pool to induce equiaxed grain growth. In some embodiments, the nanoparticles are magnetic or susceptible to magnetic influences and become magnetically aligned during solidification to produce a crystal texture determined by an external magnetic field. Alternatively or additionally, the nanoparticles (whether or not they are magnetic or susceptible to magnetic influences) can induce the growth of a magnetic phase, which can then be magnetically aligned with the direction of the magnetic field.
[0267] In general, the base particles and / or surface modified particles can be selected from the group consisting of Al, Si, Fe, Cu, Ni, Mn, Mg, Cr, Zn, V, Ti, Bi, Ga, Pb, Zr, H, Li, Be, B, C, N, O, F, Na, P, S, Cl, K, Ca, Sc, Co, Zn, Ga, Ge, As, Se, Br, Rb, Sr, Y, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, In, Sn, Te, I, Cs, Ba, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg, Tl, Ce, Nd, and combinations thereof.
[0268] In general, the geometry of the raw material composition is not limited, and can be, for example, in the form of powder particles, silk material, rod, strip, plate, film, coil, sphere, cube, prism, cone, irregular shape or its combination. In certain embodiments, the raw material composition is in the form of powder, silk material or its combination (for example, silk material with powder on the surface). When the raw material composition is in the form of powder, the powder particles can have, for example, from about 1 micron to about 500 microns, such as from about 10 microns to about 100 microns of the average diameter. When the raw material composition is in the form of silk material, the silk material can have, for example, from about 10 microns to about 1000 microns, such as from about 50 microns to about 500 microns of the average diameter.
[0269] The energy source for additive manufacturing can be provided by a laser beam, an electron beam, alternating current, direct current, plasma energy, induction heating from an applied magnetic field, ultrasonic energy, other sources, or a combination thereof. Typically, the energy source is a laser beam.
[0270] Selective laser melting uses a laser (e.g., a Yb fiber laser) to provide melting energy. Selective laser melting is designed to melt metal powders and fuse them together using a high power density laser. The process is capable of completely melting metal materials into solid 3D parts. A combination of direct drive motors and mirrors can be used instead of fixed optical lenses. An inert atmosphere is usually used. The vacuum chamber can be completely purged between build cycles, resulting in lower oxygen concentrations and reduced gas leaks. Selective laser melting is a type of powder bed-based additive manufacturing.
[0271] Electron beam melting uses a heated bed of metal powder, which is then melted and shaped layer by layer in a vacuum using an electron beam energy source similar to that used in electron microscopes. The metal powder is welded together layer by layer under vacuum. Electron beam melting is another type of powder bed based additive manufacturing.
[0272] Laser Engineered Net Shaping is a powder injection technology that operates by injecting metal powder into a molten metal pool using a laser as the energy source.
[0273] Laser engineered net shaping can be used to manufacture metal parts directly from a solid model designed by computer aided design using metal powder injected into a molten pool created by a focused high power laser beam. Laser engineered net shaping is similar to selective laser sintering, but the metal powder is applied only where material is being added to the part at that time. Note that "net shaping" is meant to encompass "near net" manufacturing.
[0274] The direct metal laser sintering process works by melting fine metal powder in a powder bed layer by layer. The laser provides the necessary energy and the system operates in a protective atmosphere of typically nitrogen or argon.
[0275] Another method utilizes powder injection to provide the material to be deposited. Instead of a powder bed that reacts with the energy beam, powder is injected through a nozzle, which is then melted to deposit the material. The powder can be injected with an inert carrier gas or by gravity feed. A separate shielding gas can be used to protect the molten metal pool from oxidation.
[0276] Directed energy deposition uses focused energy (electron beam or laser beam) to melt the material by melting as it is deposited. Powder or wire feedstock can be used for this process. Powder feed systems (such as laser metal deposition and laser engineered net shaping) blow powder through a nozzle, where the powder is melted by the laser beam on the surface of the part. Laser-based wire feed systems (such as laser metal deposition-wire) feed wire through a nozzle, where the wire is melted by the laser in an open environment (gas around the laser) or in a sealed gas housing or chamber, under inert gas protection.
[0277] Powder bed based additive manufacturing is preferred due to its ability to produce near net shape products and smaller customizable voxel sizes (such as about 200 μm or less) compared to directed energy deposition (typically >500 μm).
[0278] Some embodiments utilize wire feedstock and an electron beam heat source to produce near-net-shape parts in a vacuum chamber. The electron beam gun deposits metal layer by layer through the wire feedstock until the part reaches the desired shape. The part is then optionally subjected to final heat treatment and machining. Wires may be preferred over powders for safety and cost reasons.
[0279] In some embodiments, the additively manufactured magnet or magnet region has a microstructure with a crystal texture that is oriented not only in the additive manufacturing build direction. For example, the solid layers can have different primary growth direction angles relative to each other.
[0280] Additive manufacturing is in principle not limited to the number of solid layers that can be manufactured. The number of individual solid layers can be at least 2 layers, such as at least 10 individual solid layers. The number of solid layers can be much greater than 10, such as about 100, 1000 or more. In the case of welding or single-layer manufacturing, a single layer can be present in the final structure.
[0281] The plurality of additively manufactured solid layers may be characterized, for example, by an average layer thickness of at least 10 microns, such as about 10, 20, 30, 40, 50, 75, 100, 150, or 200 microns.
[0282] Each solid layer can contain many voxels. In the special case of a substantially vertical construction (e.g., narrow column), each layer can be a single voxel. The average number of voxels in each layer can be, for example, about, at least about, or at most about 2, 3, 4, 5, 10, 20, 30, 40, 50, 100, 150, 200, 300, 400, 500, 600, 700, 800, 900, or 1000, including all intermediate ranges.
[0283] The magnetic metal layer may be characterized by a microstructure having equiaxed grains. For example, a soft magnetic first region (comprising a first core region having a ferromagnetic material and a first surface region having a donor material) may comprise equiaxed grains. The equiaxed grains may be grains of the donor material, grains of the ferromagnetic material, or grains comprising both the donor material and the ferromagnetic material.
[0284] A microstructure with "equiaxed grains" means that at least 90 vol% (volume percent), preferably at least 95 vol%, and more preferably at least 99 vol% of the metal alloy contains grains of approximately equal length, width, and height. In some embodiments, at least 99 vol% of the magnets contain grains characterized by a standard deviation of less than 25%, preferably less than 10%, and more preferably less than 5% on each of the average grain length, average grain width, and average grain height. Equiaxed grains can be produced when there are many nucleation sites generated by certain grain-refining nanoparticles contained in the microstructure.
[0285] The surface modified particles of some embodiments are grain-refined nanoparticles. The grain-refined nanoparticles are preferably present in a concentration of at least 0.01 vol% (such as at least 0.1 vol%, at least 1 vol%, or at least 5 vol%) of the raw material composition. In various embodiments, the grain-refined nanoparticles are present in a concentration of about, or at least about 0.1, 0.2, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 vol%.
[0286] In some embodiments, the grain-refined nanoparticles are lattice-matched within ±5% of an otherwise equivalent material containing base particles but not containing grain-refined nanoparticles. In certain embodiments, the grain-refined nanoparticles are lattice-matched within ±2% or ±0.5% of a material containing base particles but not containing grain-refined nanoparticles.
[0287] Nanoparticle is the particle of maximum size between about 1nm and about 5000nm.The preferred size of nanoparticle is about 2000nm or less, about 1500nm or less or about 1000nm or less.In certain embodiments, the size of nanoparticle is at least 50nm.In different embodiments, average nanoparticle size is about 2,5,10,25,50,100,200,300,400,500,1000,2000,3000,4000 or 5000 nanometers.Microparticle is the particle of maximum size between about 1 micron and 1000 microns.Nanoparticle or micron particle size can be based on the desired performance and the function selection of final magnet.
[0288] Nanoparticles or micron particles can be spherical or any shape with a maximum size typically not exceeding the above maximum size. Nanoparticles or micron particles can include a coating with one or more layers of different materials. A mixture of nanoparticles and micron particles can be used. In certain embodiments, the micron particles themselves are coated with nanoparticles, and the micron particles / nanoparticle composite materials are combined on the base particles as a coating or layer.
[0289] The number of nanoparticles per micron-particle can vary widely. The average number of individual nanoparticles disposed on a micron-particle (equivalently, the average number ratio of nanoparticles to powder micron-particles) can be, for example, about 10, about 10, or about 10. 2 , about 10 3 , about 10 4 , about 10 5 , or about 10 6 The distribution of nanoparticles on the surface of the feedstock particles can vary. In some embodiments, surface regions contain relatively high concentrations of nanoparticles, and the nanoparticles may be agglomerated on the surface of those regions.
[0290] In various embodiments, the nanoparticle surface coverage can also vary widely from about 1% to 100%. The nanoparticle surface coverage is the average area fraction of the assembled nanoparticles covering the raw material particles. For example, the nanoparticle surface coverage can be about, or at least about 1%, 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, or 100%. Due to the small size of the nanoparticles, benefits may be obtained with a surface area coverage of less than 1%.
[0291] In some embodiments, at least 1% of the surface area of the microparticles contains nanoparticles that are chemically and / or physically disposed on the surface of the microparticles. When a higher concentration of nanoparticles is desired in the final material, it is preferred that a higher surface area of the microparticles contains nanoparticles. In various embodiments, at least 1%, 2%, 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, or 95% of the total surface area of the microparticles contains nanoparticles that are chemically and / or physically disposed on the surface of the microparticles.
[0292] In some embodiments, the micron particles have an average micron particle size of from about 1 micron to about 1 centimeter. In various embodiments, the average micron particle size is about 5 microns, 10 microns, 50 microns, 100 microns, 200 microns, 500 microns, 1 millimeter, 5 millimeters, or 10 millimeters.
[0293] Nanoparticles or microparticles are typically of a different composition than the base particle.Nanoparticles or microparticles may include metals, hydrides, carbides, nitrides, borides, oxides, intermetallic compounds, or other materials that form one or more of the above materials when processed.
[0294] In some embodiments, the surface functionalization is in the form of a continuous coating or a discontinuous coating. A continuous coating covers at least 90% of the surface, such as about 95%, 99%, or 100% of the surface (recognizing that there may be defects, voids, or impurities at the surface). An intermittent coating is discontinuous and covers less than 90% (such as about 80%, 70%, 60%, 50%, 40%, 30%, 20%, 10%, 5%, 2%, 1%, or less) of the surface. An intermittent coating can be uniform (e.g., with some repeating pattern on the surface) or non-uniform (e.g., random).
[0295] Generally speaking, the functionalized coating can be continuous or discontinuous. The coating can have several characteristic features. In one embodiment, the coating can be smooth and conform to the surface below. In another embodiment, the coating can be nodular. Nodular growth is often a feature of the kinetic restrictions of nanoparticle assembly. For example, the coating can look like cauliflower or small irregular fractals growing from the surface. These features may be affected by the underlying material, coating method, reaction conditions, etc.
[0296] The coating may or may not be in the form of nanoparticles or microparticles. That is, the coating may be derived from nanoparticles or microparticles, and there may no longer be discrete nanoparticles or microparticles. Various coating techniques may be employed, such as, but not limited to, electroless deposition, immersion deposition, or solution coating. The coating thickness is preferably less than about 20% of the underlying particle diameter, such as less than 15%, 10%, 5%, 2%, or 1% of the underlying particle diameter.
[0297] In some embodiments, surface functionalization also includes direct chemical or physical modification of the surface of the powder material, such as to enhance the binding of nanoparticles or microparticles. Direct chemical modification of the surface of the powder material (such as adding molecules) can also be used to affect the solidification behavior of the powder material. A variety of surface modifications described herein can be used simultaneously.
[0298] The choice of composition will depend on the desired magnet properties and should be considered on a case-by-case basis. One skilled in the art of materials science or metallurgy will be able to select appropriate materials for the intended use based on the information provided in this disclosure.
[0299] Electrostatic forces, van der Waals forces, chemical bonds, physical bonds, and / or any other forces can be used to attach nanoparticles or microparticles. Chemical bonds are forces that hold atoms together in a molecule or compound. Electrostatic forces and van der Waals forces are examples of physical forces that can cause bonding. Physical bonding is bonding that occurs when molecular entities become entangled in space. Typically, chemical bonds are stronger than physical bonds. Chemical bonds can include ionic bonds, covalent bonds, or combinations thereof.
[0300] In some embodiments, the surface-modified particles have an average particle size of 10 microns or less, such as 1 micron or less.The surface-modified particles can be spherical, non-spherical (eg, pyramidal or cubic), or randomly shaped.
[0301] Preferably, the microstructure of the additively manufactured magnet is substantially crack-free. Avoiding cracks should be important for magnets. For example, samarium-cobalt magnets are brittle and prone to cracking and chipping. Crack-free SmCo-based soft magnets can be manufactured using the principles of the present disclosure.
[0302] A magnet microstructure that is "substantially crack-free" means that at least 99.9 vol% of the metal alloy does not contain linear or curved cracks greater than 0.1 microns in width and greater than 10 microns in length. In other words, to be considered a crack, the defect must be a void space with a width of at least 0.1 microns and a length of at least 10 microns. Regardless of the width, a void space with a length less than 10 microns but greater than 1 micron can be considered a porous void (see below). Void spaces with a length of at least 10 microns but a width less than 0.1 microns are molecular-level gaps that are not considered defects.
[0303] Typically, cracks contain open spaces that may be a vacuum or may contain gases such as air, CO 2 、N 2 The cracks may also contain solid material that is different from the primary material phase of the metal alloy. The undesired material disposed within the cracks may itself contain a higher porosity than the bulk material, may contain a different solid crystalline (or amorphous) phase, or may be an entirely different material resulting from, for example, impurities during manufacturing.
[0304] In addition to being substantially crack-free, the magnet microstructure may also be substantially free of porous defects. "Substantially free of porous defects" means that at least 99 vol% of the magnet contains no porous voids having an effective diameter of at least 1 micrometer.
[0305] Preferably, at least 80 vol%, more preferably at least 90 vol%, even more preferably at least 95 vol%, and most preferably at least 99 vol% of the magnet does not contain porous voids having an effective diameter of at least 1 micron. Porous voids with an effective diameter of less than 1 micron are typically not considered defects because they are generally difficult to detect by conventional non-destructive evaluation. Also preferably, at least 90 vol%, more preferably at least 95 vol%, even more preferably at least 99 vol%, and most preferably at least 99.9 vol% of the metal alloy does not contain larger porous voids having an effective diameter of at least 5 microns.
[0306] Typically, the porous void contains open space, which may be a vacuum or may contain a gas such as air, CO 2 、N 2 and / or Ar. In some embodiments, porous voids can be reduced or eliminated. For example, the additively manufactured metal part can be hot isostatically pressed to reduce residual porosity and optionally obtain a final additively manufactured magnet that is substantially free of porous defects in addition to being substantially free of cracks.
[0307] In additive manufacturing, post-production processes such as heat treatment, light machining, surface finishing, coloring, stamping or other finishing operations can be applied. In addition, several additively manufactured parts can be chemically or physically joined together to produce the final magnet.
[0308] In this detailed description, reference has been made to a number of embodiments and the accompanying drawings, in which specific exemplary embodiments of the invention are shown by way of illustration. These embodiments have been described in sufficient detail to enable those skilled in the art to practice the invention, and it should be understood that modifications may be made to the various disclosed embodiments by those skilled in the art.
[0309] When the above method and step indicate that some events occur in a certain order, those of ordinary skill in the art will recognize that the order of some steps can be modified, and such modification is carried out according to variations of the present invention. In addition, some steps can be carried out simultaneously by parallel processes when possible, or can be carried out successively.
[0310] All publications, patents, and patent applications cited in this specification are herein incorporated by reference in their entirety to the same extent as if each individual publication, patent, or patent application was specifically and individually set forth herein.
[0311] The above-described embodiments, variations, and accompanying drawings should provide an indication of the practicality and versatility of the present invention. Other embodiments that do not provide all of the features and advantages set forth herein may also be used without departing from the spirit and scope of the present invention. Such modifications and variations are considered to fall within the scope of the present invention as defined by the claims.
[0312] Examples
[0313] Example 1: FeSi magnet with laser melted Ni on the surface to selectively tailor the magnetic permeability.
[0314] This experiment utilized a laser welding chamber. Nickel (Ni) foil was laid on top of the FeSi sheet and wrapped around it. The FeSi sheet, reduced in size to a width of about 4.8 mm, was placed on a linear actuator. The sample was placed in the focal plane of the laser, which was a YAG (yttrium aluminum garnet) laser operating at 1064 nm. 3 Al 5 O 12 ) laser. The laser power was set to 1000 W and the spot size was 200 μm, resulting in 0.03 W / μm at the surface of the sample. 2 The laser was fired at a rate of 6 Hz, so that the sample was driven by a linear actuator below the laser, producing a line scan. This technique uses a dynamic laser beam to simulate automated processes, such as those found in 3D printers. The line scans are then overlapped to form an area scan. When the laser comes into contact with the Ni foil, the nickel melts into the surface of the FeSi sheet, effectively alloying the FeSi surface. Nickel is used as an austenite phase stabilizing material to selectively tailor the FeSi magnetic permeability.
[0315] This experiment can be performed in the presence and absence of an electromagnetic field. Two electromagnets are connected together with a wire to serve as the North (N) and South (S) magnetic poles. The NS pair of electromagnets are spaced about 6.4 mm apart with the aid of a flux concentrator to achieve a magnetic field strength that causes a flux density of about 0.6 T in the experiment with the electromagnetic field present.
[0316] Figure 7 is a micrograph of a FeSi sheet with Ni selective regions resulting from melting and resolidification of Ni foil in the absence of an electromagnetic field. Figure 7 The scale bar is 1000 μm. Fig. 8A is a scanning electron microscope (SEM) micrograph of a cross section of a Ni foil welded to a FeSi sheet in the absence of an electromagnetic field (SEM scale bar is 200 micrometers). Fig. 8A In the SEM images, slight color differences indicate differences in composition; the lighter areas correspond to Ni-rich areas, while the darker areas correspond to FeSi-rich areas, as demonstrated in the SEM images. Ni is clearly melted into the surface of the FeSi sheet. Figure 8Bis an energy dispersive X-ray spectroscopy (EDS) graph showing the different compositions present. The brighter spots indicate where Ni is detected, while the darker areas indicate where Fe is detected. In the top Ni-rich region, Ni accounts for about 65% (on an atomic basis) and Fe accounts for about 32% (on an atomic basis).
[0317] This experiment demonstrated that the surface of magnetic materials can be selectively alloyed, eliminating the need for complex masks.
[0318] Example 2: FeSi magnet with laser melted Cu on the surface to selectively tailor the magnetic permeability.
[0319] This experiment utilized a laser welding chamber. Copper (Cu) foil was laid on top of the FeSi sheet and wrapped around it. The FeSi sheet, which was reduced in size to a width of about 4.8 mm, was placed on a linear actuator. The sample was placed in the focal plane of the laser, which was a YAG (yttrium aluminum garnet) laser operating at 1064 nm. 3 Al 5 O 12 ) laser. The laser power was set to 1000 W and the spot size was 200 μm, resulting in 0.03 W / μm at the surface of the sample. 2 The laser was fired at a rate of 6 Hz, so that the sample was driven by a linear actuator below the laser, producing a line scan. This technique uses a dynamic laser beam to simulate automated processes, such as those found in 3D printers. The line scans are then overlapped to form an area scan. When the laser comes into contact with the Cu foil, the copper melts into the surface of the FeSi sheet, effectively alloying the FeSi surface. Copper is used as an austenite phase stabilizing material to selectively tailor the FeSi magnetic permeability. This experiment was conducted in the absence of an electromagnetic field.
[0320] Fig. 9 is a micrograph of a FeSi sheet with a Cu selective region (weld zone) formed by melting and resolidification of Cu foil. Fig. 9 The scale bar (white) is 20 μm.
[0321] This experiment demonstrated that the surface of magnetic materials can be selectively alloyed, eliminating the need for complex masks.
[0322] Example 3: FeSi magnet with laser melted Ni on the surface to selectively tailor the magnetic permeability.
[0323] Another experiment was conducted, which was similar to Example 1, but using nickel powder instead of nickel foil. Melting and resolidification were achieved using a metal 3-D printer without applying an external electromagnetic field. A FeSi sheet was placed in the 3D printing chamber, Ni powder was brushed on the FeSi surface, and a laser was scanned over the area to melt the Ni into the FeSi surface.
[0324] Fig.10 is a micrograph of a FeSi sheet with Ni selective regions formed by melting and resolidification of Ni powder. Fig.10 The scale bar is 1 mm (1000 μm).
[0325] This experiment demonstrated that the surface of magnetic materials can be selectively alloyed, eliminating the need for complex masks.
Claims
1. A method for customizing the surface of a soft magnetic material, the method comprising: (a) providing a selected ferromagnetic receptor material; (b) providing a selected austenite phase stabilizing donor material; (c) depositing the selected austenite phase stabilizing donor material onto one or more first surface regions of the ferromagnetic receptor material; (d) not depositing the selected austenite phase stabilizing donor material on one or more second surface regions of the ferromagnetic receptor material; (e) laser melting the selected austenite phase stabilizing donor material into the one or more first surface regions to form molten austenite phase stabilizing donor material; as well as (f) solidifying the molten austenite phase stabilized donor material to form a solid austenite phase stabilized donor material located within the one or more first surface regions, thereby selectively alloying the ferromagnetic receptor material within the one or more first surface regions, wherein the one or more first surface regions are characterized by a first average magnetic permeability, wherein the one or more second surface regions are characterized by a second average magnetic permeability, and Wherein, the first average magnetic permeability is higher than the second average magnetic permeability.
2. The method of claim 1, wherein: The method does not employ a mask.
3. The method of claim 1, wherein: The method does not employ chemical treatment.
4. The method of claim 1, wherein: In step (c), the selected austenite phase stabilizing donor material is deposited in the form of powder particles.
5. The method of claim 1, wherein: In step (c), the selected austenite phase stabilizing donor material is deposited in the form of a film, foil or web.
6. The method of claim 1, wherein: The selected ferromagnetic acceptor material is selected from the group consisting of FeSi, FeNi, FeCo, NiCo, FeSiAl and combinations thereof.
7. The method of claim 1, wherein: The selected austenite phase stabilizing donor material is selected from the group consisting of Ni, Mn, Co, Cr, Si, Mo, Nb, Ti, Mg, Cu, Al, N, C, B and combinations thereof.
8. The method of claim 1, wherein: In step (c), the selected austenite phase stabilizing donor material is deposited on the one or more first surface regions using slurry coating, laser cladding, electron beam cladding, electroplating, electroless plating, wire arc deposition, chemical vapor deposition, physical vapor deposition, thermal spraying, plasma spraying or a combination thereof.
9. The method of claim 1, wherein: After step (f), the one or more first surface regions have an average thickness of from about 1 micron to about 3000 microns.
10. The method of claim 9, wherein: The average thickness is from about 100 microns to about 500 microns.
11. The method of claim 1, wherein: The first average magnetic permeability is at least 90% greater than the second average magnetic permeability.
12. The method of claim 1, wherein: The first average magnetic permeability is at least 99% greater than the second average magnetic permeability.
13. A method for customizing the surface of a soft magnetic material, the method comprising: (a) providing a selected ferromagnetic receptor material; (b) providing a selected austenite phase stabilizing donor material; (c) depositing the selected austenite phase stabilizing donor material onto one or more first surface regions of the ferromagnetic receptor material; (d) not depositing the selected austenite phase stabilizing donor material on one or more second surface regions of the ferromagnetic receptor material; as well as (e) laser ablating the selected austenite phase-stabilizing donor material into the one or more first surface regions to force the selected austenite phase-stabilizing donor material to penetrate into the one or more first surface regions to selectively alloy the ferromagnetic receptor material in the one or more first surface regions, wherein the one or more first surface regions are characterized by a first average magnetic permeability, wherein the one or more second surface regions are characterized by a second average magnetic permeability, and Wherein, the first average magnetic permeability is higher than the second average magnetic permeability.
14. The method of claim 13, wherein: The method does not employ masks or chemical treatments.
15. The method of claim 13, wherein: In step (c), the selected austenite phase stabilizing donor material is deposited in the form of powder particles.
16. The method of claim 13, wherein: The selected ferromagnetic acceptor material is selected from the group consisting of FeSi, FeNi, FeCo, NiCo, FeSiAl and combinations thereof.
17. The method of claim 13, wherein: The selected austenite phase stabilizing donor material is selected from the group consisting of Ni, Mn, Co, Cr, Si, Mo, Nb, Ti, Mg, Cu, Al, N, C, B and combinations thereof.
18. The method of claim 13, wherein: In step (c), the selected austenite phase stabilizing donor material is deposited on the one or more first surface regions by electrodeposition, chemical vapor deposition, physical vapor deposition, thermal spraying, plasma spraying, or a combination thereof.
19. The method of claim 13, wherein: The one or more first surface regions have an average thickness of from about 1 micron to about 3000 microns.
20. The method of claim 13, wherein: The first average magnetic permeability is at least 90% greater than the second average magnetic permeability.
21. A soft magnet with surface-tailored magnetic permeability, wherein: The soft magnetic body comprises: (i) a first region comprising a first core region and a first surface region, wherein the first core region comprises a ferromagnetic material, and wherein the first surface region comprises an austenite phase stabilizing donor material; and (ii) a second region, the second region comprising a second core region, wherein the second core region comprises the ferromagnetic material, and wherein the second region does not comprise the austenite phase stabilizing donor material; wherein the first surface region has an average thickness from about 1 micron to about 3000 microns, and wherein the first region is characterized by a first average magnetic permeability, wherein the second region is characterized by a second average magnetic permeability, and wherein the first average magnetic permeability is higher than the second average magnetic permeability.
22. The soft magnetic body according to claim 21, wherein: The ferromagnetic material is selected from the group consisting of FeSi, FeNi, FeCo, NiCo, FeSiAl and combinations thereof.
23. The soft magnetic body according to claim 21, wherein: The austenite phase stabilizing donor material is selected from the group consisting of Ni, Mn, Co, Cr, Si, Mo, Nb, Ti, Mg, Cu, Al, N, C, B and combinations thereof.
24. The soft magnetic body according to claim 21, wherein The average thickness is from about 100 microns to about 500 microns.
25. The soft magnetic body according to claim 21, wherein In the first region, the thickness of the first surface region is about 0.1% to about 50% of the thickness of the first core region.
26. The soft magnetic body according to claim 21, wherein The first average magnetic permeability is at least 90% greater than the second average magnetic permeability.
27. The soft magnetic body according to claim 21, wherein: The first average magnetic permeability is at least one order of magnitude higher than the second average magnetic permeability.
28. The soft magnetic body according to claim 21, wherein The first average magnetic permeability is at least two orders of magnitude higher than the second average magnetic permeability.
29. The soft magnetic body according to claim 21, wherein The soft magnetic body includes a plurality of instances of the first region and / or the second region.
30. The soft magnetic body according to claim 21, wherein: The soft magnet is present in a rotor in an electric motor.
Citation Information
Patent Citations
Methods for tailoring the magnetic permeability of soft magnets, and soft magnets obtained therefrom
US20230321757A1
Magnetic materials and methods for their manufacture
CN106062899A
Magnet having regions of different magnetic properties and method for forming such a magnet
CN106796835A
Insulated ferromagnetic laminates and method of manufacturing
CN114006506A
Magnetic field generation device for generating a magnetic field with a defined field distribution
DE102017217698A1
Cited By
Preparation method of refractory alloy surface ultrahigh-temperature ceramic and refractory metal silicide composite coating
CN119506871A