Novel scouring pad and preparation method thereof
Through needle-punched non-woven fabric layer and heat treatment technology, combined with surface materials and particle application, the problems of traditional cleaning cloth are solved, insufficient detergent ability and lack of versatility, and the efficiency and environmental protection of the new cleaning cloth are achieved. performance.
Patent Information
- Application Number
- CN202411149000.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
AI Technical Summary
Traditional cleaning cloths are easy to be layered, have insufficient stain removal capabilities, lack of versatility and poor environmental protection during use, and cannot meet the needs of modern efficient and environmentally friendly cleaning products.
The needle-punched non-woven fabric layer consists of 50-70% low-melting fiber 4080 staple fiber and 30-50% polyester staple fiber. The fiber network is formed by heat treatment, and soda powder, citric acid, walnut powder or tangerine peel are applied to the surface. Materials such as powder are combined with the sandblasting process to apply emery or quartz sand particles to form a physical mesh structure to enhance decontamination.
It solves the problems of layering and slag detachment, improves the decontamination ability and versatility, is suitable for different cleaning needs, and shows higher wear resistance and environmental protection performance.
Smart Images

Figure CN119014772A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cleaning product manufacturing, in particular to a novel scouring pad and a preparation method thereof. Background Art
[0002] In the field of modern household and industrial cleaning, scouring pads are an indispensable cleaning tool. They are usually used to remove surface dirt, oil stains and stubborn dirt, and are widely used in a variety of applications such as home kitchens, bathrooms and factory workshops. As people's demand for efficient and environmentally friendly cleaning products continues to grow, the types and performance of scouring pads on the market continue to evolve. Traditional scouring pads are mainly made of polyester fibers, which are formed by needle punching and glue bonding. This production method shows significant defects in the use of the product.
[0003] When used for a long time or in contact with water, traditional scouring pads are prone to delamination and slag, which not only reduces the cleaning effect but also shortens the service life of the product. This problem mainly stems from the failure of the adhesive in humid conditions, resulting in a weakening of the bonding force between the fiber layers. In addition, due to production process limitations, traditional scouring pads are difficult to flexibly adjust in thickness and density, and cannot be customized according to different cleaning needs, which limits their applicability in different occasions.
[0004] In terms of stain removal ability, traditional scouring pads usually rely on mechanical friction to remove stains, which is especially ineffective when dealing with stubborn dirt, and often require additional chemical cleaning agents to improve the stain removal effect. This not only increases the cost of use, but may also cause health and environmental problems. For the treatment of stubborn oil stains, traditional scouring pads lack sufficient surface friction and the strength of the decontamination particles, resulting in low cleaning efficiency and requiring a lot of manpower to barely achieve the desired effect.
[0005] Although scouring pads have been widely used, these technical defects still limit their performance improvement and market application scope. The existing technology cannot effectively solve the problems of delamination, insufficient decontamination ability and lack of multifunctionality. Therefore, the market urgently needs a more efficient, durable and environmentally friendly cleaning solution to replace traditional scouring pads. In response to these challenges, the present invention provides a new scouring pad and a preparation method thereof. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention provides a new type of scouring pad and a preparation method thereof, which solves the problems of traditional scouring pads being easy to delaminate during use, having insufficient decontamination ability, lacking multifunctionality and poor environmental protection.
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions: A new type of scouring pad includes a needle-punched non-woven fabric layer, which is composed of 50-70% of low-melting fiber 4080 staple fibers and 30-50% of polyester staple fibers by weight.
[0008] Preferably, the needle-punched nonwoven fabric layer has a mass per unit area of 120-180 g / m2, a thickness of 1.5-3 mm before heat treatment, and a needle-punching density of 450-600 needles / cm 2 .
[0009] Preferably, the surface of the non-woven fabric layer has a microscopic concave-convex structure.
[0010] A method for preparing a novel scouring pad is prepared by using any of the novel scouring pad components described above, comprising the following steps:
[0011] S1, mixing 50-70% of low-melting fiber 4080 staple fiber and 30-50% of polyester staple fiber, and combing them into a fiber web;
[0012] S2, forming a preliminary non-woven fabric layer by a needle punching process;
[0013] S3, performing heat treatment to form a fiber network;
[0014] S4, applying material to the surface of the nonwoven fabric layer by spraying or dipping;
[0015] S5. Apply particles to the surface of the nonwoven fabric layer using a sandblasting process.
[0016] Preferably, the fiber network formed by the non-woven fabric layer after heat treatment in step S3 has a physically interlocking structure.
[0017] Preferably, in step S4, the material applied to the surface of the non-woven fabric layer is selected from one of baking soda, citric acid, walnut powder or tangerine peel powder.
[0018] Preferably, the surface application material is bonded to the non-woven fabric layer by mechanical locking between the fibers.
[0019] Preferably, the particles applied in step S5 include corundum or quartz sand.
[0020] Preferably, during the heat treatment of the needle-punched nonwoven fabric layer in step S3, the fiber shrinkage rate is controlled by adjusting the heat treatment temperature between 140-180° C. and the time between 30-120 seconds.
[0021] Preferably, the non-woven fabric finally prepared in step S5 is suitable for a variety of applications, including but not limited to household cleaning, industrial decontamination, kitchen oil stain cleaning and daily maintenance of sanitary facilities.
[0022] The present invention provides a novel scouring pad and a preparation method thereof. The invention has the following beneficial effects:
[0023] 1. The present invention adopts a glue-free needle punching and heat treatment process, and through physical interlocking and close integration of the fiber network, prevents the product from being delaminated and falling off during use, and solves the problem that traditional scouring pads are prone to being delaminated and falling off during use.
[0024] 2. The present invention can control the shrinkage rate of the fiber by adjusting the heat treatment temperature (140-180°C) and time (30-120 seconds), thereby producing products of different thicknesses and densities to meet different cleaning needs, solving the problem that the thickness and density of the scouring pad in the prior art are usually difficult to adjust, limiting the versatility of the product.
[0025] 3. The present invention applies materials such as baking soda, citric acid, walnut powder or tangerine peel powder on the surface of the non-woven fabric layer by spraying or dipping, and combines them with the fibers through mechanical locking, thereby enhancing the decontamination ability of the product and solving the problem that the decontamination effect of traditional scouring pads is limited and additional chemical cleaners are required to achieve an ideal cleaning effect.
[0026] 4. The present invention applies corundum or quartz sand particles on the surface of the non-woven fabric through the sandblasting process, thereby enhancing the detergency, especially performing well in removing stubborn stains and oil stains, solving the problem that the existing scouring pads are not effective in dealing with stubborn stains and require a lot of manpower to remove. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Flow chart of the method of the present invention. DETAILED DESCRIPTION
[0028] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Please refer to the attached Figure 1 The embodiment of the present invention provides a new type of scouring pad, including a needle-punched non-woven fabric layer, which is composed of 50-70% of low-melting fiber 4080 staple fibers and 30-50% of polyester staple fibers by weight.
[0030] The needle-punched nonwoven fabric layer has a unit area mass of 120-180g / m2, a thickness of 1.5-3mm before heat treatment, and a needle-punching density of 450-600 needles / cm 2 .
[0031] The surface of the non-woven fabric layer has a microscopic concave-convex structure.
[0032] A method for preparing a novel scouring pad is prepared by using any of the novel scouring pad components described above, comprising the following steps:
[0033] S1, mixing 50-70% of low-melting fiber 4080 staple fiber and 30-50% of polyester staple fiber, and combing them into a fiber web;
[0034] S2, forming a preliminary non-woven fabric layer by a needle punching process;
[0035] S3, performing heat treatment to form a fiber network;
[0036] S4, applying material to the surface of the nonwoven fabric layer by spraying or dipping;
[0037] S5. Apply particles to the surface of the nonwoven fabric layer using a sandblasting process.
[0038] The fiber network formed by the nonwoven fabric layer after heat treatment in step S3 has a physically interlocking structure.
[0039] In step S4, the material applied on the surface of the non-woven fabric layer is selected from one of baking soda, citric acid, walnut powder or tangerine peel powder.
[0040] The surface-applied material is bonded to the nonwoven layer by mechanical locking between the fibers.
[0041] The particles applied in step S5 include corundum or quartz sand.
[0042] In step S3, during the heat treatment of the needle-punched nonwoven fabric layer, the fiber shrinkage rate is controlled by adjusting the heat treatment temperature between 140-180° C. and the time between 30-120 seconds.
[0043] The nonwoven fabric finally prepared in step S5 is suitable for a variety of applications, including but not limited to household cleaning, industrial decontamination, kitchen oil stain cleaning, and daily maintenance of sanitary facilities.
[0044] Embodiment 1
[0045] Implementation steps:
[0046] Material selection and mixing:
[0047] 60% of low-melting fiber 4080 staple fiber and 40% of polyester staple fiber are selected and mixed according to weight percentage.
[0048] Fiber web formation:
[0049] The mixed fibers are combed into a uniform fiber web by a carding machine.
[0050] Needle punching:
[0051] The needle punching process was used, and the needle punching density was set to 500 needles / cm 2 , forming a preliminary non-woven fabric layer.
[0052] Heat Treatment:
[0053] Heat treatment was performed at 150°C for 60 seconds to form a compact fiber network.
[0054] Material application:
[0055] Soda powder material is applied to the surface of the non-woven fabric layer through a spraying process to enhance the decontamination ability.
[0056] Particle coating:
[0057] Sandblasting is a process that applies diamond grains to the surface to increase surface friction.
[0058] Summarize:
[0059] Example 1 demonstrates basic material selection and processing, focusing on enhancing the decontamination effect through heat treatment and particle coating, and is suitable for general household cleaning.
[0060] Embodiment 2
[0061] Implementation steps:
[0062] Material selection and mixing:
[0063] 65% of low-melting fiber 4080 staple fiber and 35% of polyester staple fiber were selected.
[0064] Fiber web formation:
[0065] Combed into a uniform fiber web.
[0066] Needle punching:
[0067] The needle density is 550 needles / cm 2 , forming a preliminary non-woven fabric layer.
[0068] Heat Treatment:
[0069] Heat treatment was performed at 155°C for 90 seconds to form a reinforced fiber network.
[0070] Material application:
[0071] The citric acid material is applied using a dipping process and secured by mechanical locking.
[0072] Particle coating:
[0073] Quartz sand particles are applied to the surface to improve cleaning efficiency.
[0074] Summarize:
[0075] Embodiment 2 enhances the decontamination and adsorption capabilities of the material by increasing the needle punching density and adopting the immersion method, and is suitable for cleaning kitchen oil stains.
[0076] Embodiment 3
[0077] Implementation steps:
[0078] Material selection and mixing:
[0079] 70% of low-melting fiber 4080 staple fiber and 30% of polyester staple fiber are selected.
[0080] Fiber web formation:
[0081] Combed into a uniform fiber web.
[0082] Needle punching:
[0083] The needle density is 600 needles / cm 2 , forming a non-woven fabric layer.
[0084] Heat Treatment:
[0085] Heat treatment at 160°C for 120 seconds enhances the compactness of the fiber network.
[0086] Material application:
[0087] Walnut powder is applied through a spraying process to improve the degreasing ability of the product.
[0088] Particle coating:
[0089] The mixed particles (corundum and quartz sand) are applied using a sandblasting process to further enhance the cleaning power.
[0090] Summarize:
[0091] Embodiment 3 further increases the material ratio and heat treatment temperature, thereby enhancing the degreasing and wear resistance of the product, and is suitable for industrial decontamination.
[0092] Embodiment 4
[0093] Implementation steps:
[0094] Material selection and mixing:
[0095] It uses 68% low-melting fiber 4080 staple fiber and 32% polyester staple fiber.
[0096] Fiber web formation:
[0097] Combed into a uniform fiber web.
[0098] Needle punching:
[0099] The acupuncture density is maintained at 580 needles / cm 2.
[0100] Heat Treatment:
[0101] The heat treatment temperature was set to 158° C. and the time was set to 110 seconds.
[0102] Material application:
[0103] The tangerine peel powder material is applied using an impregnation method and is bonded by mechanical locking between the fibers.
[0104] Particle coating:
[0105] A double layer of particles is applied using a sandblasting process, ensuring both stain removal and protection.
[0106] Summarize:
[0107] Embodiment 4 further enhances the decontamination ability and cleaning durability by optimizing the impregnation process and heat treatment, and is suitable for daily maintenance of sanitary facilities.
[0108] Embodiment 5
[0109] Implementation steps:
[0110] Material selection and mixing:
[0111] It adopts 70% low melting fiber 4080 staple fiber and 30% polyester staple fiber.
[0112] Fiber web formation:
[0113] Combed into a uniform fiber web.
[0114] Needle punching:
[0115] The acupuncture density is 600 needles / cm 2 , forming a compact non-woven fabric layer.
[0116] Heat Treatment:
[0117] Heat treatment at 160°C for 120 seconds maximizes the reinforcement fiber network.
[0118] Material application:
[0119] Apply mixed materials by a combination of spraying and dipping for increased product versatility.
[0120] Particle coating:
[0121] Use advanced sandblasting equipment to apply high hardness particles for comprehensive cleaning performance.
[0122] Summarize:
[0123] Example 5 achieves the highest level in terms of decontamination ability and product stability, and achieves a wide range of cleaning applications through the use of mixed materials.
[0124] Summary:
[0125] These five examples show the preparation process of scouring pads from basic to advanced. By gradually optimizing the material ratio, process flow and treatment technology, not only the decontamination and wear resistance performance are improved, but also the application range of the product is expanded. Each example innovates on the basis of the previous one, and finally achieves excellent performance in different application scenarios. Through these design and process improvements, the new scouring pad provides a more efficient and environmentally friendly solution for household, industrial and professional cleaning.
[0126] Experimental design
[0127] Experiment 1: Wear resistance test
[0128] Objective: To verify the improved wear resistance of the new scouring pad compared to the traditional scouring pad.
[0129] Material:
[0130] New scouring pad sample (Example 5)
[0131] Traditional Scouring Pad Sample
[0132] Traditional Scouring Pad Sample Description
[0133] Sample Description:
[0134] Material composition: Traditional scouring pads are usually made of polyester fiber (PET) and adhesive. Its typical composition is 90-100% polyester fiber, which is bonded by glue to form a fiber layer.
[0135] Manufacturing process: Needle punching technology is used, but glue is used to bond the fiber layers to improve structural strength. Usually a simple heat pressing treatment is performed on the surface.
[0136] Specifications:
[0137] Mass per unit area: usually 100-130g / m 2
[0138] Thickness: 1.0-2.5mm
[0139] Acupuncture density: 400-500 needles / cm 2
[0140] Surface treatment: Usually does not have a microscopic uneven structure, is relatively smooth, and may contain a small amount of abrasive particles.
[0141] Experimental comparison background:
[0142] Abrasion resistance: Traditional scouring pads often delaminate under long-term friction due to glue bonding in abrasion resistance tests.
[0143] Decontamination ability: The decontamination ability of traditional scouring pads mainly depends on their mechanical friction and does not have its own decontamination chemical components.
[0144] Structural stability: After use in water, delamination or falling off is likely to occur due to the solubility of the glue.
[0145] Environmental performance: Due to the use of non-degradable adhesives, traditional scouring pads degrade slowly during the biodegradation process.
[0146] equipment:
[0147] Taber Wear Tester
[0148] Balance
[0149] step:
[0150] Prepare 10 new scouring pad samples and 10 traditional scouring pad samples.
[0151] The wear resistance of each sample was tested by applying a friction force of 500 g to each sample using a Taber abrasion tester.
[0152] The test rotation number was 1000 revolutions, and the mass lost by each sample after the wear test was recorded.
[0153] Table 1:
[0154] Sample No. Initial mass (g) Weight after test (g) Loss mass (g) Loss percentage (%) New 1 10.00 9.95 0.05 0.50 New Type 2 10.00 9.94 0.06 0.60 New 3 10.00 9.93 0.07 0.70 New 4 10.00 9.96 0.04 0.40 New 5 10.00 9.95 0.05 0.50 New Average 10.00 9.946 0.054 0.54 Tradition 1 10.00 9.85 0.15 1.50 Tradition 2 10.00 9.83 0.17 1.70 Tradition 3 10.00 9.84 0.16 1.60 Tradition 4 10.00 9.86 0.14 1.40 Tradition 5 10.00 9.82 0.18 1.80 Traditional average 10.00 9.84 0.16 1.60
[0155] Result analysis:
[0156] The average mass loss of the new scouring pad was 0.054 g (0.54%), while that of the traditional scouring pad was 0.16 g (1.60%).
[0157] The new scouring pad showed better wear resistance in the wear resistance test, with a lower loss rate, and is suitable for longer repeated use.
[0158] Experiment 2: Decontamination Test
[0159] Objective: To verify the efficiency of a new scouring pad in removing oil stains.
[0160] Material:
[0161] New scouring pad sample (Example 3)
[0162] Traditional scouring pad sample (same as experiment 1)
[0163] Rapeseed Oil
[0164] equipment:
[0165] Oil stain test board
[0166] Electronic scale
[0167] Standard sink
[0168] step:
[0169] Evenly apply 10g of rapeseed oil on the oil stain test plate.
[0170] Use the new and traditional scouring pad samples to wipe the oil stains. Measure and record the weight of the remaining oil stains on the board after wiping.
[0171] Table 2:
[0172]
[0173]
[0174] Result analysis:
[0175] The new scouring pad removed an average of 8.96 g of oil stains (89.60% removal rate), while the traditional scouring pad removed an average of 6.86 g (68.60% removal rate).
[0176] The new scouring pad demonstrates stronger stain removal ability, especially in cleaning oil stains.
[0177] Experiment 3: Structural stability test
[0178] Objective: To verify the structural stability of a new scouring pad after use in water.
[0179] Material:
[0180] New scouring pad sample (Example 4)
[0181] Traditional scouring pad sample (same as experiment 1)
[0182] equipment:
[0183] sink
[0184] Electronic scale
[0185] step:
[0186] The new and traditional scouring pad samples were soaked in water for 30 minutes respectively.
[0187] Remove the sample, gently remove excess water, and measure its mass.
[0188] Observe and record whether the sample has delamination or slag.
[0189] Table 3:
[0190]
[0191]
[0192] Result analysis:
[0193] The new scouring pad showed no delamination or residue falling off after soaking, and the average weight gain was 1.07g, reflecting its excellent water absorption.
[0194] Traditional scouring pads generally show delamination, with an average weight gain of 0.50g, indicating poor structural stability.
[0195] Experiment 4: Environmental performance test
[0196] Objective: To evaluate the biodegradability of a new scouring pad.
[0197] Material:
[0198] New scouring pad sample (Example 2)
[0199] Traditional scouring pad sample (same as experiment 1)
[0200] equipment:
[0201] Soil biodegradation device
[0202] Electronic scale
[0203] step:
[0204] Equal amounts of the new and traditional scouring pad samples were buried in the soil.
[0205] Samples were taken out every month and their remaining mass was measured.
[0206] The degradation was recorded and monitored continuously for 6 months.
[0207] Table 4:
[0208]
[0209] Result analysis:
[0210] The average degradation rate of the new scouring pad is 60.30%, significantly higher than the 3.32% of the traditional scouring pad.
[0211] The new scouring pad showed excellent environmental performance in biodegradation tests.
[0212] Summary:
[0213] Through the above four experiments, we verified the significant advantages of the new scouring pad in the following aspects:
[0214] Wear resistance: In the wear resistance test, the new scouring pad showed stronger wear resistance, and the loss rate was only one-third of that of traditional products.
[0215] Decontamination ability: Decontamination experiments show that the new scouring pad has a much better ability to remove oil stains than traditional scouring pads, with a decontamination rate of nearly 90%.
[0216] Structural stability: After being used in water, the new scouring pad maintains its structure intact without any delamination, showing excellent stability.
[0217] Environmental performance: In the degradation test, the degradation rate of the new scouring pad reached 60.30%, which is significantly better than the traditional scouring pad and meets environmental protection standards.
[0218] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A new type of scouring pad, characterized in that: The invention comprises a needle-punched non-woven fabric layer, wherein the non-woven fabric layer is composed of 50-70% of low-melting fiber 4080 staple fibers and 30-50% of polyester staple fibers according to weight percentage.
2. A new type of scouring pad according to claim 1, characterized in that: The needle-punched nonwoven fabric layer has a unit area mass of 120-180 g / m2, a thickness of 1.5-3 mm before heat treatment, and a needle-punching density of 450-600 needles / cm 2 .
3. A new type of scouring pad according to claim 1, characterized in that: The surface of the non-woven fabric layer has a microscopic concave-convex structure.
4. A novel method for preparing a scouring pad, characterized in that: The preparation method of the novel scouring pad component according to any one of claims 1 to 3 comprises the following steps: S1, mixing 50-70% of low-melting fiber 4080 staple fiber and 30-50% of polyester staple fiber, and combing them into a fiber web; S2, forming a preliminary non-woven fabric layer by a needle punching process; S3, performing heat treatment to form a fiber network; S4, applying material to the surface of the nonwoven fabric layer by spraying or dipping; S5. Apply particles to the surface of the nonwoven fabric layer using a sandblasting process.
5. A method for preparing a new type of scouring pad according to claim 4, characterized in that: The fiber network formed by the non-woven fabric layer after heat treatment in step S3 has a physically interlocking structure.
6. A method for preparing a novel scouring pad according to claim 4, characterized in that: In the step S4, the material applied on the surface of the non-woven fabric layer is selected from one of baking soda, citric acid, walnut powder or tangerine peel powder.
7. A method for preparing a novel scouring pad according to claim 6, characterized in that: The surface application material is bonded to the nonwoven fabric layer by mechanical locking between the fibers.
8. A method for preparing a novel scouring pad according to claim 4, characterized in that: The particles applied in step S5 include corundum or quartz sand.
9. A method for preparing a novel scouring pad according to claim 4, characterized in that: In the step S3, during the heat treatment of the needle-punched nonwoven fabric layer, the fiber shrinkage rate is controlled by adjusting the heat treatment temperature between 140-180° C. and the time between 30-120 seconds.
10. A method for preparing a novel scouring pad according to claim 4, characterized in that: The nonwoven fabric finally prepared in step S5 is suitable for a variety of applications, including but not limited to household cleaning, industrial decontamination, kitchen oil stain cleaning, and daily maintenance of sanitary facilities.