Process for separating ilmenite from pyroxene peridotite type low-grade vanadium-titanium magnetite ore iron separation tailings

Through the pulsating high-gradient magnetic separation-grinding-vibration pulsating high-gradient magnetic separation-flotation process, the problems of difficult separation and complex flotation process in olgaslo vanadium titanium magnetite ore are solved, and efficient Titanium concentrate production and low-cost flotation process.

CN119016187APending Publication Date: 2024-11-26PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411408184.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The separation of ilmenite in olgastic vanadium titanium magnetite iron tailings is difficult, the flotation process is complex, and the production cost is high. The traditional methods have the problems of long titanium selection process and large chemical consumption.

Method used

The process of pulsating high-gradient magnetic separation-grinding-vibration pulsating high-gradient magnetic separation-floating is adopted to further separate ilmenite from other minerals with different magnetization coefficients through pulsating vibration magnetic separator, improve the sorting accuracy and reduce flotation The amount of floating ore is injected to increase the capture efficiency of flotation agents.

Benefits of technology

The production of titanium concentrate with high TiO2 grade is achieved, which shortens the flotation process, reduces the consumption of flotation agents, reduces production costs, and improves the recovery rate and sorting efficiency of ilmenite.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016187A_ABST
    Figure CN119016187A_ABST
Patent Text Reader

Abstract

The invention discloses a process for separating ilmenite from pyroxene peridotite type low-grade vanadium-titanium magnetite ore iron separation tailings, and belongs to the technical field of ore separation. The invention provides a process for separating ilmenite from pyroxene peridotite type low-grade vanadium-titanium magnetite ore, which comprises the following steps: feeding iron separation tailings into a pulsating high-gradient magnetic separator for separation, carrying out ball milling on obtained titanium rough concentrate I, feeding an obtained ore grinding product I into a pulsating vibration magnetic separator for concentration and separation, and carrying out magnetic separation on the ore grinding product I; and the obtained titanium rough concentrate II is subjected to size mixing and then subjected to flotation desulfurization, obtained desulfurized tailings are subjected to size mixing and then subjected to flotation concentration, and titanium concentrate is obtained. According to the method, vibration pulsation high-gradient magnetic separation with higher separation precision is introduced, so that the flotation titanium concentrate yield is reduced, the flotation TiO2 grade is improved, and the purposes of shortening the flotation process, reducing the flotation reagent consumption and reducing the production cost are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ore dressing, and in particular relates to a process for separating titanium ore from iron tailings of olivine-type low-grade vanadium-titanium magnetite ore. Background Art

[0002] Panxi area in Sichuan is the world's largest titanium resource base, with reserves accounting for 90.54% of the total domestic reserves and 35.17% of the world's total reserves. The typical vanadium-titanium magnetite ore types in the region are gabbro-type and olivine-type. Among them, the vein mineral composition of olivine-type vanadium-titanium magnetite is complex and difficult to sort. At the same time, with the increase in mining depth, the content of difficult-to-select olivine increases, the quality and selectivity of ilmenite resources are declining, and the low precision of pulsating high-gradient magnetic separation brings increasingly prominent problems to subsequent flotation.

[0003] Specifically, the TiO2 grade of the feed ore of the titanium beneficiation process in some mining areas is 9-10%. The TiO2 grade can be increased to 18-22% through pulsating high gradient magnetic separation, the operating TiO2 recovery rate is 70-75%, and the TiO2 grade of the tailings is reduced to 3.5-4.0%; then, the qualified titanium concentrate with a TiO2 grade of 47% is produced through the flotation process, and the TiO2 recovery rate of the whole process is 30-40%. However, for olivine-type deposits, the TiO2 grade of the feed ore of the titanium beneficiation process is only 3-4%, and the TiO2 grade can only be increased to 8-10% through pulsating high gradient magnetic separation, and the operating titanium recovery rate is reduced to about 70%. The TiO2 grade and recovery rate have dropped significantly, which has significantly increased the process complexity and production cost of producing qualified titanium concentrate through subsequent flotation and concentration operations.

[0004] CN116441035A discloses a beneficiation method for fine-grained olivine-type ilmenite, comprising: concentrating fine-grained tailings, wherein the fine-grained tailings are fine-grained olivine-type ilmenite in which material particles with a particle size of less than 0.074 mm account for 50% to 90%; performing a cyclone classification after sand settling and iron removal in the concentrated stage; reselecting the sand settling in the cyclone classification to obtain a first material with a certain titanium grade; performing graded grinding on the first material to obtain a second material with a certain fineness; and After the second stage of iron removal, the second material is subjected to sulfur and titanium floating in turn to obtain coarse-grained titanium concentrate; the overflow of the first stage cyclone classification is subjected to strong magnetism; the strong magnetic concentrate is subjected to two-stage concentration; the sediment of the second stage concentration is subjected to sulfur and titanium floating in turn to obtain fine-grained titanium concentrate; the gravity separation tailings and the strong magnetic tailings are subjected to three-stage cyclone classification; the overflow of the three-stage cyclone classification, the first stage concentration and the second stage concentration is subjected to three-stage concentration; the sediment of the three-stage concentration is subjected to cyclone desludging and then sulfur and titanium floating are carried out in turn to obtain ultra-fine-grained titanium concentrate. However, this method has the problems of long titanium selection process, high grade of floating TiO2, and high reagent consumption.

[0005] Therefore, it is urgent to develop a new process that can efficiently separate ilmenite from the iron tailings of olivine vanadium-titanium magnetite ore to reduce the complexity of the flotation process and production costs. Summary of the invention

[0006] The purpose of the present invention is to provide a new process for separating ilmenite concentrate from vanadium-titanium magnetite iron tailings, which has the characteristics of good ilmenite separation effect, low magnetic separation titanium concentrate yield (i.e., floatation amount), high TiO2 grade (i.e., floatation grade), and further has the characteristics of short flotation process, reduced flotation agent consumption and low production cost.

[0007] To achieve the above object, the present invention provides a process for separating titanium concentrate from iron tailings of olivine-type low-grade vanadium-titanium magnetite ore, which comprises the following steps:

[0008] A. Feeding the olivine-type low-grade vanadium-titanium magnetite iron ore tailings into a pulsating high-gradient magnetic separator for separation to obtain titanium coarse concentrate I and tailings I; in step A, during the separation process, the background magnetic induction intensity of the pulsating high-gradient magnetic separator is controlled to be 0.4-1.0T, the diameter of the magnetic medium is 1.0-5.0mm, and the pulsating pulse frequency is 50-300rpm;

[0009] B. ball-milling the titanium coarse concentrate I obtained in step A (generally, the titanium coarse concentrate I is fed into a ball mill for ball milling), grinding to -0.074 mm with a content of 50-70%, to obtain a grinding product I;

[0010] C. Feeding the grinding product I obtained in step B into a pulsating vibration magnetic separator for separation and selection to obtain titanium coarse concentrate II and tailings II; in step B, during the separation and selection process, the background magnetic field strength of the pulsating vibration magnetic separator is controlled to be 0.4-1.0T, the diameter of the magnetic medium is 1.0-5.0mm, the pulsating impulse is 50-300rpm, the vibration frequency of the magnetic medium is 1000-3000rpm, and the vibration amplitude is 1-5mm;

[0011] D. Slurrying the titanium crude concentrate II obtained in step C, feeding the slurry after slurrying into a flotation machine for flotation desulfurization, the flotation desulfurization process is one roughing, one sweeping and four refining or one roughing, two sweeping and four refining, to obtain sulfur-cobalt concentrate and desulfurized tailings;

[0012] E. The desulfurized tailings obtained in step D are slurried and fed into a flotation machine for flotation separation. The flotation separation process is one roughing, one sweeping and three finishing or one roughing, two sweeping and four finishing to obtain titanium concentrate and tailings III.

[0013] Among them, in the above-mentioned process for sorting titanium concentrate from olivine-type low-grade vanadium-titanium magnetite ore iron-separating tailings, in step A, the TFe grade of the olivine-type low-grade vanadium-titanium magnetite ore iron-separating tailings is 3.5% to 17%, and the TiO2 grade is 3.5% to 15%.

[0014] Wherein, in the above-mentioned process for separating titanium concentrate from iron-separating tailings of olivine-type low-grade vanadium-titanium magnetite ore, in step D, the concentration of the slurry after slurry adjustment is controlled to be 30wt% to 65wt%.

[0015] In the above process for separating titanium concentrate from iron tailings of olivine-type low-grade vanadium-titanium magnetite ore, in step D, sulfuric acid is added as a pH adjuster and xanthate is used as a collector during flotation desulfurization. # Oil is used as a foaming agent in amounts of 500-2000 g / t titanium rough concentrate II, 50-300 g / t titanium rough concentrate II and 20-100 g / t titanium rough concentrate II, respectively.

[0016] Wherein, in the above-mentioned process for separating titanium concentrate from iron tailings of olivine-type low-grade vanadium-titanium magnetite ore, in step E, the concentration of the slurry after slurry adjustment is controlled to be 30wt% to 65wt%.

[0017] Among them, in the above-mentioned process for sorting titanium concentrate from olivine-type low-grade vanadium-titanium magnetite iron ore tailings, in step E, during the flotation selection process, sulfuric acid is added as a pH adjuster, a mixture of MOH and U-Ti No. 3 is used as a collector, and diesel is used as an auxiliary collector, and the amounts used are 1000-5000 g / t titanium rough concentrate II, 500-3000 g / t titanium rough concentrate II, and 50-800 g / t titanium rough concentrate II, respectively.

[0018] Among them, in the above-mentioned process for sorting titanium concentrate from iron tailings of olivine-type low-grade vanadium-titanium magnetite ore, the yield of the sulfur-cobalt concentrate obtained in step D is 0.1-0.5%, and the TiO2 grade is 4.0-6.25wt%.

[0019] Among them, in the above-mentioned process for sorting titanium concentrate from iron tailings of olivine-type low-grade vanadium-titanium magnetite ore, the yield of titanium concentrate obtained in step E is 3-12%, the TiO2 grade is 46.5-48.5wt%, and the S grade is ≤0.2%.

[0020] Among them, in the above-mentioned process for sorting titanium concentrate from the iron-separating tailings of olivine-type low-grade vanadium-titanium magnetite ore, tailings I obtained in step A, tailings II obtained in step C and tailings III obtained in step E are combined into total tailings; the yield of the total tailings is 87.5-96.9%, and the TiO2 grade is 2.0-4.5wt%.

[0021] The beneficial effects of the present invention are:

[0022] The present invention adopts a separation process of pulsating high gradient magnetic separation-grinding-vibration pulsating high gradient magnetic separation-flotation. Compared with the traditional pulsating high gradient magnetic separation-grinding-pulsating high gradient magnetic separation-flotation, by introducing vibration pulsating high gradient magnetic separation with higher separation accuracy, the grinding product is fed into the vibration pulsating high gradient magnetic separator for highly selective separation, so that the dissociated ilmenite and pyrrhotite, pyroxene, olivine and other gangue with larger specific magnetic susceptibility and chlorite, feldspar and other gangue with smaller specific magnetic susceptibility are further efficiently separated to obtain titanium rough concentrate II with high TiO2 grade, thereby reducing the amount of flotation ore, reducing the yield of titanium concentrate, and improving the grade of TiO2 entering the flotation, so as to achieve the purpose of shortening the flotation process, reducing the consumption of flotation reagents and reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0024] Specifically, a process for separating titanium concentrate from iron tailings of olivine-type low-grade vanadium-titanium magnetite ore comprises the following steps:

[0025] A. Feeding the olivine-type low-grade vanadium-titanium magnetite iron ore tailings into a pulsating high-gradient magnetic separator for separation to obtain titanium coarse concentrate I and tailings I; in step A, during the separation process, the background magnetic induction intensity of the pulsating high-gradient magnetic separator is controlled to be 0.4-1.0T, the diameter of the magnetic medium is 1.0-5.0mm, and the pulsating pulse frequency is 50-300rpm;

[0026] B. ball-milling the titanium coarse concentrate I obtained in step A (generally, the titanium coarse concentrate I is fed into a ball mill for ball milling), grinding to -0.074 mm with a content of 50-70%, to obtain a grinding product I;

[0027] C. Feeding the grinding product I obtained in step B into a pulsating vibration magnetic separator for separation and selection to obtain titanium coarse concentrate II and tailings II; in step B, during the separation and selection process, the background magnetic field strength of the pulsating vibration magnetic separator is controlled to be 0.4-1.0T, the diameter of the magnetic medium is 1.0-5.0mm, the pulsating impulse is 50-300rpm, the vibration frequency of the magnetic medium is 1000-3000rpm, and the vibration amplitude is 1-5mm;

[0028] D. Slurrying the titanium crude concentrate II obtained in step C, feeding the slurry after slurrying into a flotation machine for flotation desulfurization, the flotation desulfurization process is one roughing, one sweeping and four refining or one roughing, two sweeping and four refining, to obtain sulfur-cobalt concentrate and desulfurized tailings;

[0029] E. The desulfurized tailings obtained in step D are slurried and fed into a flotation machine for flotation separation. The flotation separation process is one roughing, one sweeping and three finishing or one roughing, two sweeping and four finishing to obtain titanium concentrate and tailings III.

[0030] In step A of the present invention, the olivine-type low-grade vanadium-titanium magnetite iron-separation tailings are tailings produced by the iron-separation process of the olivine-type low-grade vanadium-titanium magnetite grinding stage, and its TFe grade is 3.5% to 17%, and its TiO2 grade is 3.5% to 15%; in addition, its useful minerals are mainly ilmenite and pyrrhotite, and the gangue minerals are mainly pyroxene, olivine, feldspar, chlorite, etc. The specific magnetic susceptibility of ilmenite and olivine is similar, and it is difficult to separate them by a traditional high-ladder magnetic separator.

[0031] In step A of the present invention, firstly, ilmenite, pyroxene, olivine with larger specific magnetic susceptibility and chlorite and feldspar with smaller specific magnetic susceptibility in vanadium-titanium magnetite ore are effectively separated by a pulsating high gradient magnetic separator to obtain a titanium rough concentrate, thereby reducing the subsequent grinding amount and reducing the ore mud, thereby reducing the grinding energy consumption. In step B, the titanium rough concentrate obtained by the pulsating high gradient magnetic separation is ground, and the titanium rough concentrate I is ball-milled to -0.074mm with a content of 50-70%, so that the ilmenite and gangue minerals such as pyroxene, olivine, and chlorite are fully dissociated, and the ilmenite and pyrrhotite are in a monomer dissociated state, which is beneficial to the subsequent step C vibration high gradient magnetic separation to obtain a qualified high-grade titanium rough concentrate II, and is also beneficial to the flotation desulfurization in step D and the flotation separation of ilmenite, pyrrhotite and gangue minerals in step E.

[0032] In step C of the present invention, the grinding product is fed into a vibrating pulsating high gradient magnetic separator for highly selective separation, so that the dissociated ilmenite is further efficiently separated from pyrrhotite, pyroxene, olivine, etc. with larger specific magnetic susceptibility and gangue such as chlorite and feldspar with smaller specific magnetic susceptibility, to obtain titanium rough concentrate II. During the vibrating pulsating high gradient magnetic separation process, the magnetic medium vibrates at a high frequency, so that the magnetic medium has an additional competitive force in the process of capturing weak magnetic mineral particles, and achieves highly selective capture of weak magnetic minerals, removes entrained gangue and poor intergrowths, and improves the selectivity of the magnetic medium in capturing weak magnetic ilmenite particles, thereby improving the TiO2 grade of the titanium rough concentrate II and reducing the amount of flotation ore.

[0033] In the traditional pulsating high gradient magnetic separation-grinding-pulsating high gradient magnetic separation process, the TiO2 grade of the obtained titanium rough concentrate is generally 7-11wt%; while the present invention optimizes the ball milling, especially the pulsating vibration magnetic separation, and optimizes the pulsating vibration magnetic separation parameters. In step C, a titanium rough concentrate II with a high TiO2 grade can be obtained, and its TiO2 grade can be more than 1 times that of the traditional one. For example, the TiO2 grade of the obtained titanium rough concentrate II in the embodiment of the present invention is 17.6wt%-22.5wt%.

[0034] In step D of the present invention, the concentration of the slurry after slurry adjustment is controlled to be 30wt% to 65wt%.

[0035] In step D of the present invention, sulfuric acid is added as a pH adjuster and xanthate is used as a collector during flotation desulfurization. # Oil is used as a foaming agent, and the dosage is 500-2000g / t titanium rough concentrate II, 50-300g / t titanium rough concentrate II and 20-100g / t titanium rough concentrate II. In the flotation desulfurization process, the flotation desulfurization process is a conventional process in the field, and the types of pH adjusters, collectors and foaming agents are not significantly changed compared with the traditional process, but because the present invention can obtain titanium rough concentrate II with high TiO2 grade, its dosage is reduced by about 1 / 5.

[0036] In step E of the present invention, the concentration of the slurry after slurry adjustment is controlled to be 30wt% to 65wt%.

[0037] In step E of the present invention, during the flotation and selection process, sulfuric acid is added as a pH adjuster, a mixture of MOH and excellent titanium No. 3 is used as a collector, and diesel is used as an auxiliary collector, and the dosage is 1000-5000g / t titanium rough concentrate II, 500-3000g / t titanium rough concentrate II, and 50-800g / t titanium rough concentrate II, respectively. According to the high TiO2 grade characteristics of the titanium rough concentrate II of the present invention, the present invention improves the flotation and selection process, adopts one roughing, one sweeping and three refining or one roughing, two sweeping and four refining, and the types of pH adjusters, collectors, and auxiliary collectors are not significantly changed compared to the traditional process, but because the present invention can obtain titanium rough concentrate II with a high TiO2 grade, its dosage is reduced by about 1 / 5-1 / 2.

[0038] The yield of the sulphur-cobalt concentrate obtained in step D of the present invention is 0.1-0.5%, and the TiO2 grade is 4.0-6.25wt%.

[0039] In step D, since the floatability of pyrrhotite is significantly enhanced after the reaction with xanthate, it is separated from ilmenite, pyroxene, olivine, etc. by flotation, so that the S grade of the titanium concentrate is ≤0.2%; in step E, chemical adsorption, electrostatic adsorption, etc. occur on the surface of ilmenite under the action of sulfuric acid, MOH, titanium dioxide, and diesel, and the floatability is increased, and it is separated from pyroxene, olivine, etc. by flotation. Therefore, the yield of the titanium concentrate obtained in step E of the present invention is 3-12%, the TiO2 grade is 46.5-48.5wt%, and the S grade is ≤0.2%.

[0040] Among them, in the above-mentioned process for sorting titanium concentrate from the iron-separating tailings of olivine-type low-grade vanadium-titanium magnetite ore, tailings I obtained in step A, tailings II obtained in step C and tailings III obtained in step E are combined into total tailings; the yield of the total tailings is 87.5-96.9%, and the TiO2 grade is 2.0-4.5wt%.

[0041] In steps D and E of the present invention, the sulfuric acid used as the pH adjuster is dilute sulfuric acid with a concentration of 5-20%, and its amount is calculated based on the mass of the titanium crude concentrate II obtained in step C, and the amount of sulfuric acid used is calculated based on the mass of pure H2SO4.

[0042] In step E of the present invention, the mixture of MOH and Uti 3 used as a collector is a conventional material in the art, and the mixing ratio of MOH and Uti 3 adopts the conventional ratio in the art. For example, the mixing mass ratio of MOH and Uti 3 used in the embodiment of the present invention is 1-3:1-2.

[0043] The present invention is further described in detail below by way of examples, but the protection scope of the present invention is not limited to the scope of the examples.

[0044] In the examples, the MOH used was purchased from Hubei Jingjiang Mineral Processing Reagent Co., Ltd.

[0045] Example 1

[0046] In this embodiment, the iron ore tailings of a certain ore dressing plant in Baima, Panzhihua are selected. The tailings contain a large amount of -38μm ilmenite, TFe grade is 10.54%, TiO2 grade is 4.32%, and the chemical composition analysis results are shown in Table 1. The main minerals in the iron ore tailings are olivine, pyroxene, ilmenite, and chlorite, and their mineral contents are 50.63%, 10.07%, 10.83%, and 8.27%, respectively. The specific magnetic susceptibility of ilmenite and olivine is similar, and it is difficult to separate them by a traditional high-ladder magnetic separator.

[0047] Table 1 Chemical composition analysis of iron tailings from a ore dressing plant in Baima, Panzhihua

[0048] element TFe <![CDATA[TiO2]]> MgO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO Grade / wt% 10.54 4.32 3.77 33.84 10.75 2.88

[0049] This embodiment specifically includes the following steps:

[0050] (1) feeding the above iron ore tailings into a pulsating high gradient magnetic separator for separation to obtain titanium coarse concentrate I and tailings I. During the separation process, the background magnetic field strength of the high gradient magnetic separator is controlled to be 0.7 T, the diameter of the magnetic medium is 2.0 mm, and the pulse frequency is 200 rpm;

[0051] (2) feeding the titanium coarse concentrate I in step (1) into a mill, grinding the titanium coarse concentrate to a content of -0.074 mm accounting for 65.00%, thereby obtaining a grinding product I;

[0052] (3) feeding the ground ore product I in step (2) into a pulsating vibration magnetic separator for separation and separation to obtain titanium coarse concentrate II (TiO2 grade 17.6wt%) and tailings II. During the separation process, the background magnetic field strength of the pulsating vibration magnetic separator is controlled to be 0.8T, the magnetic medium is 3mm, the impulse is 200rpm, the vibration frequency of the magnetic medium is 1800rpm, and the amplitude is 2mm;

[0053] (4) The titanium crude concentrate II obtained in step (3) is fed into a stirring tank for slurry adjustment to a concentration of 42 wt %. The slurry after slurry adjustment is fed into a flotation machine for flotation desulfurization. The flotation desulfurization process is one roughing, one sweeping and four refining. The flotation desulfurization obtains sulfur-cobalt concentrate and desulfurized tailings. During the flotation desulfurization process, sulfuric acid is added as a pH adjuster and xanthate is used as a collector. # Oil is a foaming agent, and its dosage is 1000g / t, 200g / t and 60g / t respectively relative to titanium crude concentrate II;

[0054] (5) The desulfurized tailings obtained in step (4) are fed into a stirring tank for slurry adjustment to a concentration of 40wt%, and then fed into a flotation machine for flotation selection. The flotation selection process is one roughing, one sweeping and three fines. The flotation selection obtains titanium concentrate and tailings III. During the flotation selection process, sulfuric acid is added as a pH adjuster, a mixture of MOH and UHT No. 3 (the mass ratio of MOH to UHT No. 3 is 1:1) as a collector, and diesel is used as an auxiliary collector. The amounts of the two are 3000 g / t, 2500 g / t and 500 g / t, respectively, relative to the titanium rough concentrate II;

[0055] (6) Tailings I, II and III are combined into the final total tailings.

[0056] (7) According to the above steps, the final product indicators can be obtained as shown in Table 2.

[0057] Table 2 Results of titanium recovery from iron ore tailings

[0058] Product Name Yield / % <![CDATA[TiO2 grade / wt%]]> <![CDATA[TiO2 recovery rate / %]]> Sulfur cobalt concentrate 0.25 5.23 0.30 Titanium Concentrate 4.89 47.47 53.72 Tailings 94.86 2.09 45.97 total 100.00 4.32 100.00

[0059] Example 2

[0060] This embodiment selects the iron tailings of a certain ore dressing plant in Midi, Panzhihua, which contains a large amount of -38μm ilmenite, with a TFe grade of 15.32% and a TiO2 grade of 8.95%. The chemical composition analysis results are shown in Table 3. The main minerals in the iron tailings are olivine, pyroxene, ilmenite, and chlorite, and their mineral contents are 30.63%, 18.55%, 15.83%, and 10.27%, respectively. The specific magnetic susceptibility of ilmenite and olivine is similar, and it is difficult to separate them by a traditional high-ladder magnetic separator.

[0061] Table 3 Chemical composition analysis of tailings from a ore dressing plant in Midi, Panzhihua

[0062] element TFe <![CDATA[TiO2]]> MgO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO Grade / wt% 15.32 8.95 2.94 20.01 7.23 4.32

[0063] This embodiment specifically includes the following steps:

[0064] (1) feeding the above iron ore tailings into a pulsating high gradient magnetic separator for separation to obtain titanium coarse concentrate I and tailings I. During the separation process, the background magnetic field strength of the high gradient magnetic separator is controlled to be 0.7 T, the diameter of the magnetic medium is 2.0 mm, and the pulse frequency is 200 rpm;

[0065] (2) feeding the titanium coarse concentrate I in step (1) into a mill, grinding the titanium coarse concentrate to a content of -0.074 mm accounting for 60.00%, thereby obtaining a grinding product I;

[0066] (3) feeding the ground ore product I in step (2) into a pulsating vibration magnetic separator for separation and concentrating to obtain titanium coarse concentrate II (TiO2 grade 22.5wt%) and tailings II. During the separation process, the background magnetic field strength of the pulsating vibration magnetic separator is controlled to be 0.8T, the magnetic medium is 2mm, the impulse is 300rpm, the vibration frequency of the magnetic medium is 2800rpm, and the amplitude is 1.5mm;

[0067] (4) The titanium crude concentrate II obtained in step (3) is fed into a stirring tank for slurry adjustment to a concentration of 40wt%, and the slurry after slurry adjustment is fed into a flotation machine for flotation desulfurization. The flotation desulfurization process is one roughing, two sweeping and four refining. The flotation desulfurization obtains sulfur-cobalt concentrate and desulfurized tailings. During the flotation desulfurization process, sulfuric acid is added as a pH adjuster, xanthate is used as a collector, and 2# oil is used as a frother. The amounts of these are 1500g / t, 150g / t and 60g / t, respectively, relative to the titanium crude concentrate II;

[0068] (5) The desulfurized tailings obtained in step (4) are fed into a stirring tank for slurry adjustment to a concentration of 38 wt %. After slurry adjustment, they are fed into a flotation machine for fine flotation. The flotation selection process is one roughing, two sweeping and four fines. The flotation selection obtains titanium concentrate and tailings III. During the flotation selection process, sulfuric acid is added as a pH adjuster, a mixture of MOH and UHT No. 3 (the mass ratio of MOH and UHT No. 3 is 3:2) as a collector, and diesel is used as an auxiliary collector. The total amount of the two is 2000 g / t, 2000 g / t and 200 g / t, respectively, relative to the titanium rough concentrate II;

[0069] (6) Tailings I, II and III are combined into the final total tailings.

[0070] (7) According to the above steps, the final product indicators can be obtained as shown in Table 4.

[0071] Table 4 Results of titanium recovery from iron ore tailings

[0072] Product Name Yield <![CDATA[TiO2 grade / %]]> <![CDATA[TiO2 recovery rate / %]]> Sulfur cobalt concentrate 0.35 5.74 0.22 Titanium Concentrate 10.82 47.54 57.47 Tailings 88.83 4.26 42.30 total 100.00 8.95 100.00

Claims

1. A process for separating ilmenite from olivine-type low-grade vanadium-titanium magnetite iron ore tailings, characterized by: The following steps are involved: A. Feeding the olivine-type low-grade vanadium-titanium magnetite iron ore tailings into a pulsating high-gradient magnetic separator for separation to obtain titanium coarse concentrate I and tailings I; in step A, during the separation process, the background magnetic induction intensity of the pulsating high-gradient magnetic separator is controlled to be 0.4-1.0T, the diameter of the magnetic medium is 1.0-5.0mm, and the pulsating pulse frequency is 50-300rpm; B. Ball milling the titanium coarse concentrate I obtained in step A to a fineness of -0.074 mm with a content of 50-70%, to obtain a grinding product I; C. Feeding the grinding product I obtained in step B into a pulsating vibration magnetic separator for separation and selection to obtain titanium coarse concentrate II and tailings II; in step B, during the separation and selection process, the background magnetic field strength of the pulsating vibration magnetic separator is controlled to be 0.4-1.0T, the diameter of the magnetic medium is 1.0-5.0mm, the pulsating impulse is 50-300rpm, the vibration frequency of the magnetic medium is 1000-3000rpm, and the vibration amplitude is 1-5mm; D. Slurrying the titanium crude concentrate II obtained in step C, feeding the slurry after slurrying into a flotation machine for flotation desulfurization, the flotation desulfurization process is one roughing, one sweeping and four refining or one roughing, two sweeping and four refining, to obtain sulfur-cobalt concentrate and desulfurized tailings; E. The desulfurized tailings obtained in step D are slurried and fed into a flotation machine for flotation separation. The flotation separation process is one roughing, one sweeping and three finishing or one roughing, two sweeping and four finishing to obtain titanium concentrate and tailings III.

2. The process for separating ilmenite from iron-separating tailings of olivine-type low-grade vanadium-titanium magnetite ore according to claim 1, characterized in that: In step A, the TFe grade of the olivine-type low-grade vanadium-titanium magnetite iron ore tailings is 3.50% to 17%, and the TiO2 grade is 3.5% to 15%.

3. The process for separating titanium concentrate from iron-separating tailings of olivine-type low-grade vanadium-titanium magnetite ore according to claim 1, characterized in that: In step D, the concentration of the slurry after slurry adjustment is controlled to be 30wt% to 65wt%.

4. The process for separating ilmenite from iron-separating tailings of olivine-type low-grade vanadium-titanium magnetite ore according to claim 1, characterized in that: In step D, during the flotation desulfurization process, sulfuric acid is added as a pH adjuster and xanthate is used as a collector. # Oil is used as a foaming agent in amounts of 500-2000 g / t titanium rough concentrate II, 50-300 g / t titanium rough concentrate II and 20-100 g / t titanium rough concentrate II, respectively.

5. The process for separating titanium concentrate from iron-separating tailings of olivine-type low-grade vanadium-titanium magnetite ore according to claim 1, characterized in that: In step E, the concentration of the slurry after slurry adjustment is controlled to be 30wt% to 65wt%.

6. The process for separating ilmenite from iron-separating tailings of olivine-type low-grade vanadium-titanium magnetite ore according to claim 1, characterized in that: In step E, during the flotation process, sulfuric acid is added as a pH adjuster, a mixture of MOH and Uti No. 3 is used as a collector, and diesel is used as an auxiliary collector. The amounts used are 1000-5000 g / t titanium rough concentrate II, 500-3000 g / t titanium rough concentrate II, and 50-800 g / t titanium rough concentrate II, respectively.

7. The process for separating ilmenite from iron-separating tailings of olivine-type low-grade vanadium-titanium magnetite ore according to claim 1, characterized in that: The yield of the sulphur-cobalt concentrate obtained in step D is 0.1-0.5%, and the TiO2 grade is 4.0-6.25wt%.

8. The process for separating titanium ore from iron-separating tailings of olivine-type low-grade vanadium-titanium magnetite ore according to claim 1, characterized in that: The yield of the titanium concentrate obtained in step E is 3-12%, the TiO2 grade is 46.5-48.5wt%, and the S grade is ≤0.2%.

9. The process for separating ilmenite from iron-separating tailings of olivine-type low-grade vanadium-titanium magnetite ore according to any one of claims 1 to 8, characterized in that: The tailings I obtained in step A, the tailings II obtained in step C and the tailings III obtained in step E are combined into total tailings; the yield of the total tailings is 87.5-96.9%, and the TiO2 grade is 2.0-4.5wt%.