Forging method of high-nitrogen non-magnetic stainless steel

By using two heating forging, water-cooling, warm forging and air-cooling methods at 1250~1270℃ during the forging of high-nitrogen magnetic stainless steel, the problem of insufficient strength and surface quality in the existing technology is solved, and high-nitrogen magnetic stainless steel is realized High material yield and excellent mechanical properties.

CN119016649APending Publication Date: 2024-11-26PANGANG GROUP JIANGYOU CHANGCHENG SPECIAL STEEL COMPANY LIMITED

Patent Information

Application Number
CN202411227941.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing high-nitrogen non-magnetic stainless steel forging methods cannot effectively ensure the strength and surface quality, resulting in insufficient strength of the finished sample and insufficient cracks and corrosion resistance.

Method used

The heating temperature and time of each stage are adjusted to eliminate internal stress, improve the uniformity of tissue and recrystallization of tissue, and improve the yield of materials.

Benefits of technology

The comprehensive performance of high-nitrogen non-magnetic stainless steel has good surface quality, no cracks, good strength and corrosion resistance, and the material yield is increased to more than 80%, and the mechanical properties are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention provides a forging method of high-nitrogen non-magnetic stainless steel. The forging method comprises the following steps that S1, a high-nitrogen non-magnetic stainless steel blank is heated at 1250-1270 DEG C, and cogging forging is conducted after heat preservation; (S2) the blank obtained in the step (S1) is heated at 1250-1270 DEG C, and after heat preservation, precision forging and water cooling are conducted; and S3) performing warm forging on the intermediate blank obtained in the step S2), and finally performing air cooling to room temperature. The invention provides a forging method of high-nitrogen non-magnetic stainless steel, which can improve the surface quality and the structure uniformity of the high-nitrogen non-magnetic stainless steel, eliminate the internal stress of the high-nitrogen non-magnetic stainless steel in the machining process and obtain a recrystallized structure beneficial to improving the self performance of the high-nitrogen non-magnetic stainless steel through the forging method of twice heating forging at 1250-1270 DEG C, water cooling, warm forging and air cooling. And the yield of the high-nitrogen non-magnetic stainless steel is increased to 80% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of iron and steel metallurgy, and in particular to a forging method for high-nitrogen non-magnetic stainless steel. Background Art

[0002] High nitrogen stainless steel is a new type of engineering material that has emerged in recent years with the advancement of metallurgical technology. Nitrogen, as a strong interstitial strengthening element, is added to stainless steel, which can greatly improve the stability of austenite, thereby partially or completely replacing expensive Ni, and through the synergistic effect with other alloying elements (Cr, Mo, V, etc.), it can improve various properties of steel, including strength, toughness, creep resistance, wear resistance and corrosion resistance, etc., and has good application prospects in the engineering field. With the advancement of high nitrogen stainless steel preparation technology and variety research and development and the expansion of application fields, the demand for Cr-Mn-(Mo)-N series high nitrogen stainless steel will exceed 100,000 tons in the next 5-10 years.

[0003] High nitrogen non-magnetic stainless steel has a high nitrogen content. During the preparation process, Mo alloying is required. It has high deformation resistance, is not easy to recrystallize during the deformation process, and has a high tendency to forging cracking. At the same time, in order to obtain high strength and high hardness, low-temperature deformation forging is required. Therefore, a suitable forging heating temperature is required to ensure the surface quality and organizational uniformity of high nitrogen non-magnetic stainless steel, improve the yield rate, and obtain high strength and high hardness properties.

[0004] The Chinese patent with publication number CN109182706A provides a high nitrogen non-magnetic stainless steel and its manufacturing method, which includes two forging heating operations, and the specific steps are: A) the heating temperature of the high temperature heat treatment furnace is 1180℃~1200℃, the holding time is more than 5h, and the final forging temperature of forging is 1090℃~1110℃; B) the heating temperature of the return furnace is 1150℃~1190℃, the heating time is 2h, the final forging deformation temperature of the radial forging machine is 900℃~930℃, and then water-cooled to the finished steel billet. In the process of preparing high nitrogen non-magnetic stainless steel, this patent is carried out by two lower temperature forging heating methods, the final forging temperature is low, and it is directly water-cooled after forging, and the strength of the finished product sample cannot be guaranteed. The Chinese patent with publication number CN111534754A provides a low segregation sensitivity and low magnetic stainless steel and a manufacturing method thereof, the process comprising the following steps: A) the continuous casting billet is heated and kept warm in a high temperature heat treatment furnace at a temperature of 1120°C to 1150°C, and the continuous casting billet is immediately subjected to continuous hot rolling to be processed into a hot rolled plate after the insulation is completed and the continuous casting billet is taken out of the furnace, and the final rolling temperature is not less than 980°C; B) the hot rolled plate is subjected to a solid solution treatment in a high temperature heat treatment furnace at a temperature of 1020°C to 1050°C, and immediately water cooled after the solid solution treatment; the preparation method is carried out by two low temperature forging heating methods, the final forging temperature is low, and the forging is directly water cooled after forging, and the strength of the finished product sample cannot be guaranteed.

[0005] Therefore, the above-mentioned stainless steel preparation method still cannot guarantee strength, and it is of great significance to provide a preparation method of high-nitrogen non-magnetic stainless steel to achieve good surface quality, no cracks, strong toughness and good corrosion resistance. Summary of the invention

[0006] The technical problem solved by the present invention is to provide a forging method for high-nitrogen non-magnetic stainless steel, which can improve the surface quality and structural uniformity of the high-nitrogen non-magnetic stainless steel, so that the stainless steel forgings have good surface quality, no cracks, good toughness and corrosion resistance.

[0007] In view of this, the present application provides a forging method for high-nitrogen non-magnetic stainless steel, comprising the following steps:

[0008] S1) heating the high nitrogen non-magnetic stainless steel billet at 1250-1270°C, keeping the temperature, and then forging the billet;

[0009] S2) heating the blank obtained in step S1) at 1250-1270° C., maintaining the temperature, and then fine forging and water cooling;

[0010] S3) warm forging the intermediate billet obtained in step S2) and finally air cooling it to room temperature.

[0011] Preferably, in step S1), the insulation time is 7 to 9 hours.

[0012] Preferably, in step S1), the final forging temperature of the blank forging is 1050-1100°C.

[0013] Preferably, in step S2), the insulation time is 2.5 to 3 hours.

[0014] Preferably, in step S2), the final forging temperature of the fine forging is 1050-1100°C.

[0015] Preferably, in step S3), the final forging temperature of the warm forging is 580-600°C.

[0016] Preferably, the high nitrogen non-magnetic stainless steel billet is a high nitrogen non-magnetic stainless steel electroslag ingot billet.

[0017] Preferably, in step S3), the composition of the high nitrogen non-magnetic stainless steel blank includes:

[0018] 0~0.040wt% C, 0~0.50wt% Si, 20.00~22.00wt% Mn, 19.00~20.00wt% Cr, 1.80~2.50wt% Ni, 0.50~0.75wt% Mo, 0.50~0.75wt% N, and the balance is Fe.

[0019] The present application provides a forging method for high-nitrogen non-magnetic stainless steel, which comprises the following steps: firstly, heating a high-nitrogen non-magnetic stainless steel billet at 1250-1270°C, forging the billet after heat preservation, then heating the obtained billet at 1250-1270°C, fine forging the billet after heat preservation, water cooling, then warm forging the obtained intermediate billet, and finally air cooling the billet to room temperature; the forging method for high-nitrogen non-magnetic stainless steel provided in the present application focuses on adjusting the heating temperature at each stage, thereby improving the surface quality and structural uniformity of the high-nitrogen non-magnetic stainless steel, eliminating the internal stress generated by the high-nitrogen non-magnetic stainless steel during the processing, obtaining a recrystallized structure that is beneficial to improving the performance of the material itself, and increasing the yield rate of the high-nitrogen non-magnetic stainless steel to more than 80%. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 These are comparison photos of the surface quality of high nitrogen non-magnetic stainless steel forgings after being treated with different forging heating processes in the embodiments of the present invention. DETAILED DESCRIPTION

[0021] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0022] In view of the requirements of the yield rate, strength and hardness of high-nitrogen non-magnetic stainless steel in the prior art, the present application provides a forging method of high-nitrogen non-magnetic stainless steel, which improves the surface quality and structural uniformity of high-nitrogen non-magnetic stainless steel by adopting a forging method of double heating forging at 1250~1270℃ + water cooling + warm forging + air cooling, eliminates the internal stress generated by high-nitrogen non-magnetic stainless steel during the processing, and can obtain a recrystallized structure that is beneficial to improving the performance of high-nitrogen non-magnetic stainless steel itself, and increases the yield rate of high-nitrogen non-magnetic stainless steel to more than 80%, producing high-nitrogen non-magnetic stainless steel with good surface quality, no cracks, strong toughness and corrosion resistance. Specifically, the embodiment of the present invention discloses a forging method of high-nitrogen non-magnetic stainless steel, comprising the following steps:

[0023] S1) heating the high nitrogen non-magnetic stainless steel billet at 1250-1270°C, keeping the temperature, and then forging the billet;

[0024] S2) heating the blank obtained in step S1) at 1250-1270° C., maintaining the temperature, and then fine forging and water cooling;

[0025] S3) warm forging the intermediate billet obtained in step S2) and finally air cooling it to room temperature.

[0026] In the forging process of high nitrogen non-magnetic stainless steel, the present application first performs open forging of the high nitrogen non-magnetic stainless steel billet, the heating temperature of the open forging is 1250~1270℃, and the holding time is 7~9h; specifically, the heating temperature of the open forging is 1250℃, 1255℃, 1260℃, 1265℃ or 1270℃, and the holding time is 7h, 7.5h, 8h, 8.5h or 9h. The open forging is fast forging, the open forging is forged to an intermediate billet of a specified size, and the final forging temperature of the open forging is 1050℃~1100℃. The higher heating temperature can make the high nitrogen non-magnetic stainless steel deform in a higher temperature range, so that the high nitrogen non-magnetic stainless steel in this temperature range has better plasticity, and can avoid the precipitation of carbonitrides during the forging deformation process; the higher final forging temperature can make the high nitrogen non-magnetic stainless steel fully recover and recrystallize in a relatively short time.

[0027] The present application further returns the obtained intermediate billet to the furnace for heat preservation at a temperature of 1250-1270°C for 2.5-3h; specifically, the heating temperature of the open forging is 1250°C, 1255°C, 1260°C, 1265°C or 1270°C, and the heat preservation time is 2.5h, 2.6h, 2.7h, 2.8h, 2.9h or 3h. After the return to the furnace for heat preservation, the fine forging is performed, and the billet is immediately water-cooled after forging to the required size of the finished steel billet. The final forging temperature is 1050-1100°C, at which time, the residual internal stress can be eliminated, the dynamic recrystallization is complete, and fine and uniform austenite grains are obtained.

[0028] According to the present invention, the water-cooled steel billet is then warm forged to be a finished steel billet, and the final forging temperature is 580-600° C. After warm forging, the mechanical properties of the steel billet are significantly improved.

[0029] Finally, the warm forged steel billet is air-cooled to room temperature to obtain a high-nitrogen non-magnetic stainless steel forging with uniform structure, good surface quality, excellent mechanical properties and corrosion resistance.

[0030] In the present application, the composition of the high nitrogen non-magnetic stainless steel is specifically: 0~0.040wt% C, 0~0.50wt% Si, 20.00~22.00wt% Mn, 19.00~20.00wt% Cr, 1.80~2.50wt% Ni, 0.50~0.75wt% Mo, 0.50~0.75wt% N, and the balance is Fe; in a specific embodiment, the composition of the high nitrogen non-magnetic stainless steel is: 0.025wt% C, 0.37wt% Si, 21.00wt% Mn, 19.82wt% Cr, 2.22wt% Ni, 0.60wt% Mo, 0.64wt% N, 0.024wt%, 0.005wt%, P, and the balance is Fe.

[0031] The present application provides a forging method for high-nitrogen non-magnetic stainless steel, which can improve the surface quality and structural uniformity of high-nitrogen non-magnetic stainless steel by heating and forging in a specific temperature range, eliminate the internal stress generated by high-nitrogen non-magnetic stainless steel during processing, obtain a recrystallized structure that is beneficial to improving the performance of high-nitrogen non-magnetic stainless steel, and increase the yield rate of high-nitrogen non-magnetic stainless steel to more than 80%. The forging method provided by the present application is scientific, reasonable, economical, efficient, and easy to operate.

[0032] In order to further understand the present invention, the forging method of high nitrogen non-magnetic stainless steel provided by the present invention is described in detail below in conjunction with embodiments, and the protection scope of the present invention is not limited by the following embodiments.

[0033] Example 1

[0034] Φ550mm high nitrogen non-magnetic stainless steel electroslag ingot blanks were selected and forged into Φ280mm bars. The electroslag ingots were heated at different soaking temperatures, forged after being taken out of the furnace, and then heated at different soaking temperatures for fine forging, then water-cooled for warm forging, and air-cooled to room temperature; the main components of the steel are shown in Table 1. Based on this, the surface conditions of the Φ280mm bars of the high nitrogen non-magnetic stainless steel were compared after different forging hot processing processes + water cooling + warm forging + air cooling.

[0035] Table 1 Chemical composition of high nitrogen non-magnetic stainless steel (wt%)

[0036]

[0037] The following three thermal processing processes are carried out respectively:

[0038] (1) The high nitrogen non-magnetic stainless steel electroslag ingot is heated to 1200~1220℃ in a heating furnace and kept warm for 8h. After being taken out of the furnace, it is forged for a final forging temperature of 990~1040℃. Then it is heated and kept warm for 2.5h at 1200~1220℃ for fine forging, and the final forging temperature is 990~1040℃. Then it is water-cooled and warm-forged, and the final forging temperature is 580~600℃. It is then air-cooled to room temperature.

[0039] (2) The high nitrogen non-magnetic stainless steel electroslag ingot is heated to 1225~1245℃ in a heating furnace and kept warm for 8h. After being taken out of the furnace, it is forged for a final forging temperature of 1015~1065℃. Then, it is heated and kept warm for 2.5h at 1225~1245℃ for fine forging, and the final forging temperature is 1015~1065℃. Then, it is water-cooled and warm-forged, and the final forging temperature is 580~600℃. It is then air-cooled to room temperature.

[0040] (3) The high nitrogen non-magnetic stainless steel electroslag ingot is heated to 1250~1270℃ in a heating furnace and kept warm for 8h. After being taken out of the furnace, it is forged for a final forging temperature of 1050~1100℃. Then, it is heated and kept warm for 2.5h at 1250~1270℃ for fine forging, and the final forging temperature is 1050~1100℃. Then, it is water-cooled and warm-forged, and the final forging temperature is 580~600℃. It is then air-cooled to room temperature.

[0041] Comparison of surface quality of high nitrogen non-magnetic stainless steel after different forging heating processes Figure 1 , Figure 1 Figure a is a surface quality photo of the high nitrogen non-magnetic stainless steel forgings produced by the first hot working process, Figure b is a surface quality photo of the high nitrogen non-magnetic stainless steel forgings produced by the second hot working process, and Figure c is a surface quality photo of the high nitrogen non-magnetic stainless steel forgings produced by the third hot working process.

[0042] Depend on Figure 1 It can be seen that compared with the two hot working processes (1) and (2), the surface quality of the high nitrogen non-magnetic stainless steel obtained by the hot working process (3) is greatly improved, and the scheme (3) has been recognized by users. According to the analysis of scanning electron microscopy and optical microscopy, the grains of the high nitrogen non-magnetic stainless steel forgings prepared by the hot working process (3) are finer and the recrystallization is complete; the finished product has high strength and high hardness.

[0043] The yield rates of high nitrogen non-magnetic stainless steel forgings produced by the above different hot working processes are shown in Table 2;

[0044] Table 2 Yield data of high nitrogen non-magnetic stainless steel forgings with different heating processes

[0045]

[0046] The experimental results show that the yield strength of high nitrogen non-magnetic stainless steel forgings produced by hot working process (3) can reach above 1050MPa, the tensile strength can reach above 1150MPa, and the intergranular corrosion can pass the test according to ASTM A262 E method.

[0047] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

[0048] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A forging method for high nitrogen non-magnetic stainless steel, comprising the following steps: S1) heating the high nitrogen non-magnetic stainless steel billet at 1250-1270°C, keeping the temperature, and then forging the billet; S2) heating the blank obtained in step S1) at 1250-1270° C., maintaining the temperature, and then fine forging and water cooling; S3) warm forging the intermediate billet obtained in step S2) and finally air cooling it to room temperature.

2. The forging method according to claim 1, characterized in that: In step S1), the insulation time is 7 to 9 hours.

3. The forging method according to claim 1, characterized in that: In step S1), the final forging temperature of the blank forging is 1050-1100°C.

4. The forging method according to claim 1, characterized in that: In step S2), the insulation time is 2.5 to 3 hours.

5. The forging method according to claim 1, characterized in that: In step S2), the final forging temperature of the fine forging is 1050-1100°C.

6. The forging method according to claim 1, characterized in that: In step S3), the final forging temperature of the warm forging is 580-600°C.

7. The forging method according to claim 1, characterized in that: The high nitrogen non-magnetic stainless steel blank is a high nitrogen non-magnetic stainless steel electroslag ingot blank.

8. The forging method according to any one of claims 1 to 7, characterized in that: In step S3), the composition of the high nitrogen non-magnetic stainless steel blank includes: 0~0.040wt% C, 0~0.50wt% Si, 20.00~22.00wt% Mn, 19.00~20.00wt% Cr, 1.80~2.50wt% Ni, 0.50~0.75wt% Mo, 0.50~0.75wt% N, and the balance is Fe.

Citation Information

Patent Citations

  • Novel high-nitrogen austenitic stainless steel for non-magnetic drill collar and manufacturing method of novel high-nitrogen austenitic stainless steel

    CN106702290A

  • High strength and toughness medium nitrogen non-magnetic stainless steel and manufacturing method thereof

    CN110205549A

  • Low-precipitation sensitivity high-performance non-magnetic stainless steel and manufacturing method thereof

    CN111304548A

  • Method for eliminating Cr-Mn-N non-magnetic steel forging circle flaw detection annular defect

    CN117102410A

Cited By

  • Ultrahigh-strength high-hardness extremely-low-magnetism stainless steel and manufacturing method thereof

    CN120945277A

  • A high-strength, high-hardness, and extremely low-magnetic stainless steel and its manufacturing method

    CN120945277B