Gold nanocluster aggregate with multiple stimulation responsiveness and preparation method and application thereof

The reaction of thiol-like purine ligands with gold ion sources to generate gold nanocluster aggregates is solved, and the problem of single luminescence color and performance of gold nanoclusters is achieved, multiple stimulus responsive discoloration luminescence is enhanced, which has enhanced its application potential in the field of optical.

CN119016735APending Publication Date: 2024-11-26SUZHOU INST OF NANO TECH & NANO BIONICS CHINESE ACEDEMY OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310609090.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The single luminous color and luminous properties of gold nanoclusters limit their application in the field of optical.

Method used

Gold nanoclusters are generated by reacting with a gold ion source using a thiol-based purine ligand and self-assembly to form gold nanocluster aggregates with aggregation-induced luminescence, excitation wavelength-dependent luminescence and mechanically discolored luminescence.

Benefits of technology

The multi-stimulus responsive discoloration luminescence of gold nanocluster aggregates has been realized, which has improved its application potential in the fields of imaging analysis, optoelectronic devices and optical anti-counterfeiting, and provides high-throughput and multi-dimensional optical anti-counterfeiting solutions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016735A_ABST
    Figure CN119016735A_ABST
Patent Text Reader

Abstract

The invention discloses a gold nano-cluster aggregate with multiple stimulation responsiveness as well as a preparation method and application of the gold nano-cluster aggregate. The preparation method comprises the following steps: reacting sulfydryl purine ligands with gold ions to generate gold nano-clusters, and carrying out self-assembly on a plurality of gold nano-clusters to obtain the gold nano-cluster aggregate. The preparation method of the gold nano-cluster aggregate provided by the invention is simple, green and environment-friendly; meanwhile, the prepared gold nano-cluster aggregate is good in stability and not prone to oxidation, has a multi-stimulus-responsive color-changing luminescence mode integrating aggregation-induced luminescence, excitation wavelength-dependent luminescence and mechanical color-changing luminescence properties, can effectively solve the problems that an existing luminescent material is single in luminescence mode and the like, and has good application prospects. The limitation of the gold nanocluster in the application fields of imaging analysis, photoelectric devices, optical anti-counterfeiting and the like is broken through, and the gold nanocluster has important application prospects in the aspect of realizing high-throughput and multi-dimensional optical anti-counterfeiting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of new functional nanomaterials, and relates to a gold nanocluster aggregate with multiple stimulus responsiveness, a preparation method and an application thereof, and in particular to a construction method for synthesizing a new type of gold nanocluster aggregate through a self-assembly process, and a multiple stimulus responsive color-changing luminescent material that integrates aggregation-induced luminescence, excitation wavelength-dependent luminescence and mechanical color-changing luminescence properties. Background Art

[0002] As an emerging nanomaterial, gold nanoclusters are generally composed of several to dozens of atoms. Because their size is comparable to the Fermi wavelength of electrons, they form discontinuous electronic energy levels and molecular-like properties of size-dependent fluorescence. Gold nanoclusters are widely used in electronic devices, catalysis, bioimaging, and chemical sensors due to their unique electrical, optical, and chemical properties. Compared with quantum dots and organic dyes, gold nanoclusters have potential application prospects in biosensing, imaging analysis, and optoelectronic devices due to their excellent photostability, large Stokes shift, and good biocompatibility. However, the quantum yield of most gold nanoclusters is less than 0.1%, which greatly limits their application in the optical field.

[0003] Stimuli-responsive color-changing materials have fascinating color changes under different external stimuli. They have attracted widespread attention due to their adjustable thermochromic, electrochromic, photochromic, vapor-phase and mechanochromic properties, and have broad application prospects in anti-counterfeiting, optoelectronic devices and information storage. As a typical photochromic material, the excitation wavelength-dependent luminophore is an excitation-responsive smart material that achieves non-invasive emission color switching by changing the excitation energy. It shows great application potential in advanced anti-counterfeiting labels, flexible three-dimensional objects and optoelectronic devices. In addition, mechanochromic luminescent materials have been widely studied due to their advantages such as reversible color change under mechanical force, good stability and recyclability. However, most luminescent materials are prepared by doping multiple luminescent components in a mixed system for selective excitation, and only have one color-changing luminescent property. These materials usually face phase separation, poor reproducibility or quenching effects caused by aggregation.

[0004] Aggregation-induced emission refers to a special photophysical phenomenon in which fluorescent materials emit bright fluorescence in aggregated or solid states due to restricted intramolecular motion. Currently, most luminescent materials face a relatively single emission mode, so breaking the limitations of gold nanoclusters in application fields such as imaging analysis, optoelectronic devices, and optical anti-counterfeiting, and solving the problem of single emission color and luminescent performance currently faced by gold nanoclusters is an urgent problem to be solved. Summary of the invention

[0005] The main purpose of the present invention is to provide a gold nanocluster aggregate with multiple stimulus responsiveness and its preparation method and application, so as to solve the problem of single luminescent color and luminescent performance currently faced by gold nanoclusters.

[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0007] An embodiment of the present invention provides a method for preparing gold nanocluster aggregates with multi-stimulus responsiveness, which comprises: reacting a thiol purine ligand with a gold ion source to generate gold nanoclusters, and allowing a plurality of the gold nanoclusters to self-assemble to obtain gold nanocluster aggregates.

[0008] The embodiment of the present invention also provides a gold nanocluster aggregate with multiple stimulus responsiveness obtained by the aforementioned preparation method.

[0009] The present invention also provides a method for controlling the luminescence properties of the aforementioned gold nanocluster aggregates, which comprises:

[0010] Irradiating the gold nanocluster aggregates with excitation light, and changing the wavelength of the excitation light within the range of 340 to 600 nm, so that the wavelength of the emission light generated by the gold nanocluster aggregates under excitation changes within the range of 440 to 700 nm;

[0011] Alternatively, the gold nanocluster aggregates are ground so that the wavelength of emission light generated by the ground gold nanocluster aggregates under irradiation with a specified excitation light is red-shifted compared to the gold nanocluster aggregates before grinding.

[0012] The embodiments of the present invention also provide the application of the aforementioned gold nanocluster aggregates with multiple stimulus responsiveness in the field of high-throughput and multi-dimensional optical anti-counterfeiting.

[0013] Compared with the prior art, the present invention has the following beneficial effects:

[0014] (1) The present invention uses thiol purine as a synthetic ligand of gold nanoclusters. The purine structure on the ligand contains a large number of hydrogen bond donors and acceptors, which can self-assemble to form a stable layered motif structure. The gold nanocluster aggregates can be regulated by self-assembly to achieve aggregation-induced luminescence, so that the gold nanocluster aggregates have stable luminescence properties;

[0015] (2) The gold nanocluster aggregates prepared by the present invention have an excitation wavelength-dependent luminescence property, and the emission wavelength moves with the movement of the excitation wavelength, thereby achieving color-changing luminescence that can be adjusted over a wide range;

[0016] (3) The emission wavelength of the gold nanocluster aggregates prepared by the present invention is red-shifted under the same excitation wavelength before and after drying and grinding. Under the irradiation of ultraviolet light of a specific wavelength, the fluorescence color changes from green to orange, showing a mechanical color-changing luminescence property;

[0017] (4) The present invention synthesizes gold nanocluster aggregates through a one-step method. The synthesis process is very simple, green and environmentally friendly, highly operable, and has very strong stability, providing important ideas and values ​​for achieving high-throughput and multi-dimensional optical anti-counterfeiting applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 is a schematic diagram of the preparation of gold nanocluster aggregates in a typical embodiment of the present invention;

[0020] Figure 2 is a transmission electron microscopy image of the gold nanocluster aggregates prepared in Example 1 of the present invention in a dispersed state;

[0021] Figure 3 is a transmission electron microscopy image of the gold nanocluster aggregates prepared in Example 1 of the present invention in an aggregated state;

[0022] Figure 4 is a fluorescence spectrum of the gold nanocluster aggregates prepared in Example 1 of the present invention, which is enhanced as the volume fraction of the water / organic solvent mixed solution increases under irradiation with an excitation wavelength of 330 nm;

[0023] Figure 5 is a fluorescence spectrum of the gold nanocluster aggregates prepared in Example 1 of the present invention at different excitation wavelengths;

[0024] Figure 6a-Figure 6b is a fluorescence spectrum of the gold nanocluster aggregates prepared in Example 1 of the present invention before and after grinding at an excitation wavelength of 400 nm;

[0025] Figure 7a-7d This is a picture taken during the grinding process of the gold nanocluster aggregates prepared in Example 1 of the present invention under irradiation with a 365nm ultraviolet lamp. DETAILED DESCRIPTION

[0026] In view of the defects of the prior art, the inventors of this case have proposed the technical solution of the present invention after long-term research and extensive practice. The present invention designs a self-assembled and regulated gold nanocluster aggregate, which can effectively improve the luminescence performance of gold nanoclusters while having a multiple stimulus-responsive color-changing luminescence mode that integrates aggregation-induced luminescence, excitation wavelength-dependent luminescence and mechanical color-changing luminescence properties. It can effectively solve the problem of relatively single luminescence mode faced by most luminescent materials, break the limitations of gold nanoclusters in application fields such as imaging analysis, optoelectronic devices and optical anti-counterfeiting, and provide important ideas and values ​​for realizing high-throughput and multi-dimensional optical anti-counterfeiting applications.

[0027] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Specifically, as one aspect of the technical solution of the present invention, a method for preparing a gold nanocluster aggregate with multiple stimulus responsiveness includes: reacting a thiol purine ligand with a gold ion source to generate gold nanoclusters, and allowing a plurality of the gold nanoclusters to self-assemble to obtain gold nanocluster aggregates.

[0029] In some preferred embodiments, the method for preparing the gold nanocluster aggregates having multiple stimulus responsiveness comprises:

[0030] At least an alkaline solution containing a thiol purine ligand, a gold ion source, water and an organic solvent are mixed and reacted at room temperature, and after the reaction is completed, the obtained reaction mixture is fully allowed to stand at room temperature, and then the gold nanocluster aggregates are separated.

[0031] Furthermore, the molar ratio of the thiol purine ligand to the gold ion source is 2:1 to 8:1.

[0032] Furthermore, the thiol purine ligand includes mercaptopurine and / or mercaptoguanine, but is not limited thereto.

[0033] Furthermore, the gold ion source includes chloroauric acid or gold acetate, etc., but is not limited thereto.

[0034] Furthermore, the organic solvent includes any one of methanol, ethanol, and DMF or a combination of two or more thereof, but is not limited thereto.

[0035] Further, the alkaline substance in the alkaline solution includes sodium hydroxide, but is not limited thereto.

[0036] Furthermore, the pH value of the alkaline solution containing the thiol purine ligand is 8-12.

[0037] Furthermore, the reaction is carried out under continuous stirring conditions, with a stirring rate of 500 to 5000 r / min and a stirring time of 48 to 96 h.

[0038] Furthermore, the standing time is 24 to 72 hours.

[0039] Furthermore, after the obtained reaction mixture is allowed to stand at room temperature, the gold nanocluster aggregates are separated from the reaction mixture by at least centrifugation, wherein the centrifugal speed of the centrifugation is 5000-10000 r / min and the time is 5-20 min.

[0040] In some more specific embodiments, the method for preparing the gold nanocluster aggregates having multiple stimulus responsiveness comprises:

[0041] (1) preparing a certain concentration of mercaptopurine alkaline solution;

[0042] (2) preparing chloroauric acid solution;

[0043] (3) mixing the mercaptopurine solution, chloroauric acid solution, ultrapure water and methanol, and stirring at room temperature for reaction;

[0044] (4) After the reaction is completed, the product is allowed to stand at room temperature and the supernatant is removed by centrifugation to obtain a gold nanocluster aggregate precipitate.

[0045] The molar ratio of mercaptopurine to chloroauric acid in the mixed solution is 2:1 to 8:1, the stirring speed of the mixed reaction is 500 to 5000 rpm, the reaction time of the stirring reaction is 48 to 96 hours, the standing time after the reaction is 24 to 72 hours, the centrifugal speed is 5000 to 10000 rpm, and the centrifugal time is 10 minutes.

[0046] Another aspect of the embodiments of the present invention further provides gold nanocluster aggregates with multiple stimulus responsiveness obtained by the aforementioned preparation method.

[0047] Furthermore, the gold nanocluster aggregates have a sheet-like aggregate structure.

[0048] Furthermore, the sheet-like structure of the gold nanocluster aggregate has a length of 0.1 to 20 μm and a width of 0.1 to 5 μm.

[0049] Furthermore, the gold nanocluster aggregates are in a spherical structure in a dispersed state, and the particle size is 1 to 10 nm.

[0050] In some preferred embodiments, the wavelength of the emission light generated by the gold nanocluster aggregates under the irradiation of the excitation light changes as the wavelength of the excitation light changes;

[0051] Furthermore, before and after the gold nanocluster aggregates are ground, the wavelength of the emitted light generated under the same excitation light will be red-shifted.

[0052] The luminescence intensity of the gold nanocluster aggregates in the aggregated state is several times that in the dispersed state, showing aggregation-induced luminescence properties; when the excitation wavelength of the gold nanocluster aggregates moves between 340 and 600 nm, the emission wavelength moves between 440 and 700 nm, showing excitation wavelength-dependent luminescence properties; before and after grinding, the gold nanocluster aggregates are irradiated with the same excitation wavelength, and the emission wavelength undergoes a red shift of about 110 nm, and under irradiation with a 365 nm ultraviolet lamp, the fluorescence color changes from green to orange, showing mechanical color-changing luminescence properties.

[0053] Compared with single gold nanoclusters that are almost non-luminescent, the gold nanoclusters prepared by the present invention form luminescent aggregates in the aqueous phase through a self-assembly process, showing typical aggregation-induced luminescence properties; the maximum emission peak of the prepared gold nanocluster aggregates red-shifts with the increase of the excitation wavelength, showing excitation wavelength-dependent luminescence characteristics, and realizing wide-range adjustable photoluminescence. Before and after solid grinding of the prepared gold nanocluster aggregates after drying, the emission wavelength is red-shifted by 110nm under the same excitation wavelength, and at the same time, under the irradiation of ultraviolet light of a specific wavelength, the fluorescence color changes from green to orange, showing mechanical color-changing luminescence characteristics. The preparation method provided by the present invention is simple, green and environmentally friendly, and the obtained gold nanocluster aggregates have good stability and are not easy to oxidize. They have a multi-stimulus responsive color-changing luminescence mode that integrates aggregation-induced luminescence, excitation wavelength-dependent luminescence and mechanical color-changing luminescence properties, which can effectively solve the problem of a relatively single luminescence mode faced by most luminescent materials, break the limitations of gold nanoclusters in the application fields of imaging analysis, optoelectronic devices and optical anti-counterfeiting, and have important application prospects in achieving high-throughput and multi-dimensional optical anti-counterfeiting.

[0054] Another aspect of the embodiments of the present invention further provides a method for changing the luminescent properties of the aforementioned gold nanocluster aggregates, comprising:

[0055] Irradiating the gold nanocluster aggregates with excitation light, and changing the wavelength of the excitation light within the range of 340 to 600 nm, so that the wavelength of the emission light generated by the gold nanocluster aggregates under excitation changes within the range of 440 to 700 nm;

[0056] Alternatively, the gold nanocluster aggregates are ground so that the wavelength of emission light generated by the ground gold nanocluster aggregates under irradiation with a specified excitation light is red-shifted compared to the gold nanocluster aggregates before grinding.

[0057] In some preferred embodiments, the designated excitation light is ultraviolet light, and the emission light generated by the gold nanocluster aggregates before and after being ground changes from green to orange under the irradiation of the ultraviolet light.

[0058] Furthermore, the wavelength of the ultraviolet light is 365 nm.

[0059] Another aspect of the embodiments of the present invention further provides the application of the aforementioned gold nanocluster aggregates with multiple stimulus responsiveness in the field of high-throughput and multi-dimensional optical anti-counterfeiting.

[0060] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.

[0061] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.

[0062] Example 1

[0063] This embodiment relates to a method for preparing gold nanocluster aggregates. Figure 1 As shown, the specific steps are as follows:

[0064] (1) Weigh 88 mg of mercaptopurine powder and mix them evenly with ultrapure water and methanol, add 50 μL of 0.1 M sodium hydroxide solution to obtain a mercaptopurine alkaline solution (pH ~ 8). Stir the prepared chloroauric acid solution (0.1 M) at room temperature and add it dropwise into the mercaptopurine alkaline solution. The stirring speed of the mixed reaction is 2000 rpm and the reaction is carried out for 48 hours.

[0065] (2) After the reaction is completed, the product is allowed to stand at room temperature for 24 hours, and the supernatant is removed by centrifugation at a speed of 8000 rpm for 10 minutes to obtain a gold nanocluster aggregate precipitate.

[0066] Example 2

[0067] This example is the characterization of the gold nanocluster aggregates prepared in Example 1:

[0068] (1) The purified gold nanocluster aggregates were precipitated and dissolved in different organic solvents, including ethanol, methanol, N,N-dimethylformamide, acetonitrile, tetrahydrofuran, petroleum ether, ethyl acetate, etc., and the gold nanocluster aggregates were optimized to be dispersed in methanol. The gold nanocluster aggregates were characterized by transmission electron microscopy. The results are as follows: Figure 2 As shown, the gold nanocluster aggregates are uniform in size and spherical in the dispersed state, with a particle size range of 1 to 10 nm.

[0069] (2) The purified gold nanocluster aggregate precipitate was diluted with ultrapure water to prepare the aggregated state of the gold nanocluster aggregate, which was characterized by transmission electron microscopy. The results are as follows: Figure 3 The aggregated structure of the gold nanocluster aggregates is in the form of sheets, with a length and width of 0.1 to 20 μm and 0.1 to 5 μm, respectively.

[0070] Example 3

[0071] This example is to optimize the optimal luminescence intensity of the gold nanocluster aggregates prepared in Example 1 in the aggregated state and the dispersed state:

[0072] Ultrapure water and the optimized organic solvent were prepared in different volume ratios, including 0%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 95% and 100%, to prepare mixed solutions of different proportions. The same mass of gold nanocluster aggregates were diluted in the mixed solutions of different proportions to test their luminescence intensity. Figure 4 As shown in the figure, as the volume ratio of ultrapure water and organic solvent increases, the luminescence intensity of the emission peak of the gold nanocluster aggregates at 400nm gradually increases under the irradiation of the excitation wavelength of 330nm. The luminescence intensity of the prepared gold nanocluster aggregates in the optimal aggregation state is 7 times that of the dispersed state, indicating that mercaptopurine is used as a synthetic ligand of gold nanoclusters. The purine structure on the ligand contains a large number of hydrogen bond donors and acceptors, which can self-assemble to form a stable layered motif structure, and can achieve aggregation-induced emission by self-assembly regulation of gold nanocluster aggregates, so that the gold nanocluster aggregates have stable luminescence properties.

[0073] Example 4

[0074] This example is an excitation wavelength-dependent luminescence test of the gold nanocluster aggregates prepared in Example 1:

[0075] The fluorescence emission spectra of gold nanocluster aggregates in ultrapure water were tested under different excitation wavelengths, such as Figure 5 As shown, under the irradiation of excitation wavelengths with a red shift interval of 20nm from 340nm to 600nm, its emission peak moves from 440nm to 700nm, showing excitation wavelength-dependent luminescence properties, achieving color-changing luminescence that can be adjusted over a wide range.

[0076] Example 5

[0077] This example is a mechanical color change luminescence test of the gold nanocluster aggregates prepared in Example 1:

[0078] The solid obtained by drying the prepared gold nanocluster aggregates was ground, and the fluorescence excitation and emission spectra were tested under an excitation wavelength of 400 nm before and after grinding. Figure 6a-Figure 6b As shown. The gold nanocluster aggregates before grinding showed strong fluorescence emission near 500nm under the irradiation of excitation wavelength of 400nm, as shown Figure 6a As shown. The ground gold nanocluster aggregates exhibit weak fluorescence emission near 610nm under the same excitation wavelength, as shown Figure 6b Therefore, the gold nanocluster aggregates before and after grinding show a red shift of about 110nm under the same excitation wavelength. Figure 7a-7d As shown, the grinding process of the prepared gold nanocluster aggregates observed with the naked eye under 365nm ultraviolet light shows that the gold nanocluster aggregates before grinding emit green fluorescence. As the grinding force increases, the fluorescence gradually changes from green to orange, indicating that the prepared gold nanocluster aggregates have mechanical color-changing luminescence properties.

[0079] Example 6

[0080] This embodiment relates to a method for preparing gold nanocluster aggregates, and the specific steps are as follows:

[0081] (1) Weigh 88 mg of mercaptopurine powder and mix them evenly with ultrapure water and ethanol, add 100 μL of 0.1 M sodium hydroxide solution to obtain a mercaptopurine alkaline solution (pH ~ 9). Stir the prepared chloroauric acid solution (0.1 M) at room temperature and add it dropwise to the mercaptopurine alkaline solution. The stirring speed of the mixed reaction is 5000 rpm and the reaction is carried out for 48 hours.

[0082] (2) After the reaction is completed, the product is allowed to stand at room temperature for 24 hours, and the supernatant is removed by centrifugation at a speed of 8000 rpm for 10 minutes to obtain a gold nanocluster aggregate precipitate.

[0083] Example 7

[0084] This embodiment relates to a method for preparing gold nanocluster aggregates, and the specific steps are as follows:

[0085] (1) Weigh 58 mg of mercaptoguanine powder and mix them evenly with ultrapure water and methanol, add 25 μL of 0.1 M sodium hydroxide solution to obtain a mercaptopurine alkaline solution (pH ~ 8). Stir the prepared chloroauric acid solution (0.1 M) at room temperature and add it dropwise into the mercaptopurine alkaline solution. The stirring speed of the mixed reaction is 2000 rpm and the reaction is carried out for 72 hours.

[0086] (2) After the reaction is completed, the product is allowed to stand at room temperature for 48 hours, and the supernatant is removed by centrifugation at a speed of 10,000 rpm for 15 minutes to obtain a gold nanocluster aggregate precipitate.

[0087] Comparative Example 1

[0088] In general, the emission wavelength of gold nanocluster aggregates prepared by using common reducing agents such as glutathione does not change under different excitation wavelengths, and does not have the excitation wavelength-dependent luminescence characteristics. In addition, the emission wavelength does not change under the same excitation wavelength before and after grinding, and does not have the mechanical color change characteristics.

[0089] Compared with Control Example 1, the gold nanocluster aggregates prepared by the present invention using thiol purine ligands not only have excitation wavelength-dependent luminescence characteristics, but also have mechanical color-changing characteristics. They can effectively solve the problem that the luminescence mode of existing luminescent materials is relatively single, and break the limitations of gold nanoclusters in application fields such as imaging analysis, optoelectronic devices, and optical anti-counterfeiting. They have important application prospects in achieving high-throughput and multi-dimensional optical anti-counterfeiting.

[0090] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0091] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.

Claims

1. A method for preparing a gold nanocluster aggregate with multiple stimulus responsiveness, characterized in that: include: The thiol-based purine ligand is reacted with a gold ion source to generate gold nanoclusters, and a plurality of the gold nanoclusters are self-assembled to obtain gold nanocluster aggregates.

2. The preparation method according to claim 1, characterized in that: Specifically include: At least an alkaline solution containing a thiol purine ligand, a gold ion source, water and an organic solvent are mixed and reacted at room temperature, and after the reaction is completed, the obtained reaction mixture is fully allowed to stand at room temperature, and then the gold nanocluster aggregates are separated.

3. The preparation method according to claim 2, characterized in that: The molar ratio of the thiol purine ligand to the gold ion source is 2:1 to 8:

1.

4. The preparation method according to claim 2, characterized in that: The thiol purine ligands include mercaptopurine and / or mercaptoguanine; And / or, the gold ion source includes chloroauric acid and / or gold acetate; and / or, the alkaline substance in the alkaline solution includes sodium hydroxide; And / or, the pH value of the alkaline solution is 8 to 12; And / or, the organic solvent includes any one of methanol, ethanol, and DMF, or a combination of two or more thereof.

5. The preparation method according to claim 2, characterized in that: The reaction is carried out under continuous stirring conditions, with a stirring rate of 500 to 5000 r / min and a stirring time of 48 to 96 h; And / or, the standing time is 24 to 72 hours; And / or, after the obtained reaction mixture is allowed to stand at room temperature, the gold nanocluster aggregates are separated from the reaction mixture by at least centrifugation, wherein the centrifugal speed of the centrifugation is 5000-10000 r / min and the time is 5-20 min.

6. Gold nanocluster aggregates with multi-stimulus responsiveness obtained by the method according to any one of claims 1 to 5.

7. The gold nanocluster aggregate according to claim 6, characterized in that: The gold nanocluster aggregates have a sheet-like aggregate structure; preferably, the sheet-like structure of the gold nanocluster aggregates has a length of 0.1 to 20 μm and a width of 0.1 to 5 μm; Preferably, the gold nanocluster aggregates are spherical in structure when dispersed, and have a particle size of 1 to 10 nm.

8. The gold nanocluster aggregate according to claim 6, characterized in that: The wavelength of the emitted light generated by the gold nanocluster aggregate under the irradiation of the excitation light changes as the wavelength of the excitation light changes; Furthermore, before and after the gold nanocluster aggregates are ground, the wavelength of the emitted light generated under the same excitation light will be red-shifted.

9. A method for changing the luminescent properties of the gold nanocluster aggregates according to any one of claims 6 to 8, characterized in that: include: Irradiating the gold nanocluster aggregates with excitation light, and changing the wavelength of the excitation light within the range of 340 to 600 nm, so that the wavelength of the emission light generated by the gold nanocluster aggregates under excitation changes within the range of 440 to 700 nm; Alternatively, the gold nanocluster aggregates are ground so that the wavelength of emission light generated by the ground gold nanocluster aggregates under irradiation with a specified excitation light is red-shifted compared to the gold nanocluster aggregates before grinding.

10. The method according to claim 9, characterized in that: The designated excitation light is ultraviolet light, and the emission light generated by the gold nanocluster aggregates before and after being ground changes from green to orange under the irradiation of the ultraviolet light; Preferably, the wavelength of the ultraviolet light is 254-380 nm.

11. Application of the gold nanocluster aggregates with multi-stimulus responsiveness according to any one of claims 6 to 8 in the field of high-throughput and multi-dimensional optical anti-counterfeiting.