HgCdTe chip and cutting method thereof

By using a combination of secondary cutting process and protective layer during cutting of mercury cadmium tellurium chips, the problem of excessive defect stress during cutting is solved, the probability of chip breakage is reduced, and high-quality cutting effect is ensured.

CN119017567APending Publication Date: 2024-11-26安徽光智科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411378099.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, when cutting mercury cadmium tellurium chips, the defects are subjected to excessive force instantly, causing the chip to easily break down, resulting in fragments or lobes, which makes it difficult to effectively reduce the chance of damage.

Method used

The secondary cutting process is adopted, through a combination of primary cutting and secondary cutting, the cutting depth and rate are controlled, and the protective layer and appropriate bonding method are used to reduce the instantaneous stress of defects and reduce the diameter of the edge of the chip.

Benefits of technology

It effectively reduces the chance of mercury cadmium tellurium chips breaking during cutting, ensuring that the diameter of the edges around the chip edge is less than 10μm, meeting production needs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of semiconductors, and discloses a mercury-cadmium-telluride chip and a cutting method thereof.The mercury-cadmium-telluride chip is fixed to a scribing table, and then a scribing knife is used for primary cutting to obtain a primary cutting chip; carrying out secondary cutting on the primary cutting chip by using a scribing knife to obtain a cut tellurium-cadmium-mercury chip; wherein the thickness of the tellurium-cadmium-mercury chip is 1 mm, the primary cutting depth is 0.50-0.65 mm, and the secondary cutting depth is 0.50-0.35 mm; in addition, the invention further discloses the tellurium-cadmium-mercury chip which is obtained through the cutting method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a mercury cadmium telluride chip and a cutting method thereof. Background Art

[0002] Mercury cadmium telluride (HgCdTe, or MCT) is a semiconductor material commonly used in infrared detectors and imaging devices, with good photoelectric response, especially in the infrared band. Its cutting technology is one of the key steps in manufacturing high-performance infrared detectors.

[0003] Among them, Chinese patent application 202310253513.2 discloses a method for dividing a mercury cadmium telluride infrared detector chip, which is: using a protective layer to protect the chip area, corroding and removing the passivation layer and the mercury cadmium telluride layer in the cutting path area, forming a cutting groove in the cutting path area, exposing the surface of the cadmium zinc telluride layer in the cutting groove; cutting the cadmium zinc telluride layer from the cutting groove to obtain a mercury cadmium telluride infrared detector chip.

[0004] In this case, the stress during cutting was reduced by etching away the HgCdTe layer before cutting the CdZnTe layer, thereby reducing the probability of damage to the HgCdTe infrared detector chip.

[0005] Chinese patent application 202311315836.6 discloses a method for preparing a mercury cadmium telluride infrared detector and its chip, and the preparation method is: forming a first protective layer and a second protective layer on a substrate in sequence, wherein the first protective layer and the second protective layer at least cover the chip area on the substrate; cutting or thinning the substrate, and then removing the second protective layer and the first protective layer in batches.

[0006] In this solution, two protective layers are formed on the substrate, and the protective layers are removed in batches after the thinning or slicing process. A large amount of debris will be removed along with the second protective layer, reducing chip damage.

[0007] The problem that this solution needs to solve is: how to propose a mercury cadmium telluride chip and a cutting method thereof. Summary of the invention

[0008] The purpose of the present invention is to provide a method for cutting mercury cadmium telluride chips, which reduces the probability of chips being broken due to excessive force at the moment of defects and causing fragments or cracks through a secondary cutting process.

[0009] To achieve the above object, the present application discloses a mercury cadmium telluride chip and a cutting method thereof, which comprises the following steps:

[0010] Step 1: Fix the mercury cadmium telluride chip on a dicing table, and then use a dicing knife to cut it once to obtain a single-cut chip;

[0011] Step 2: Use a dicing knife to perform a second dicing on the once-cut chip to obtain a cut mercury cadmium telluride chip;

[0012] Among them, the thickness of the mercury cadmium telluride chip is 1mm, the first cutting depth is 0.50~0.65mm, and the second cutting depth is 0.50~0.35mm.

[0013] More preferably, the primary cutting depth is 0.56-0.60 mm, and the secondary cutting depth is 0.44-0.40 mm.

[0014] Preferably, the surface of the mercury cadmium telluride chip in step 1 further has a layer of photoresist for protecting the chip, and the thickness of the photoresist is 5-8 μm.

[0015] Preferably, the cutting speed of the dicing knife in step 1 and step 2 is 0.5-1 mm / s, and the cutting angle is 90°.

[0016] Preferably, the fixing method in step 1 is: bonding the mercury cadmium telluride chip to a substrate, and then bonding the substrate to a dicing table, and the flatness of the substrate is less than 3 μm;

[0017] During the secondary cutting, the dicing knife needs to penetrate 20 to 30 μm into the substrate.

[0018] Preferably, the binder is at least one of paraffin wax and water-soluble glue.

[0019] Preferably, the substrate material is selected from at least one of a silicon wafer, a quartz wafer, and silicon nitride.

[0020] In addition, a mercury cadmium telluride chip is also disclosed, which is prepared by the mercury cadmium telluride chip cutting method.

[0021] The beneficial effects of the present invention are:

[0022] The invention provides a method for cutting a mercury cadmium telluride chip. After multiple experiments, it is found that there are certain defects (such as hard impurities or overgrown grains) inside the mercury cadmium telluride chip itself. If the chip is directly cut by one-time cutting, the defect will be broken due to excessive force at the moment, resulting in the chip being fragmented or split. The invention uses a secondary cutting process to effectively reduce the probability of the defect being broken due to excessive force at the moment, resulting in the chip being fragmented or split, and obtains a chip with a chip edge diameter of less than 10μm around the edge when observed under a bright field of a metallographic microscope at 100 times magnification. DETAILED DESCRIPTION

[0023] In the description of the present invention, it should be noted that, if the specific conditions are not specified in the examples, the experiments were carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.

[0024] Example 1

[0025] Step 1: Bond the mercury cadmium telluride chip to the blue film, then fix it to the silicon wafer with paraffin wax, and use a dicing knife to perform a single cut with a single cutting rate of 0.8 mm / s and a cutting depth of 0.58 mm to obtain a single-cut chip;

[0026] Step 2: Use a dicing knife to perform a second dicing on the once-cut chip, with a dicing rate of 0.8 mm / s and a dicing depth of 0.42 mm to obtain a cut mercury cadmium telluride chip;

[0027] After cutting, the diameter of the chip edge chipping was 3.5μm under 100x bright field observation of a metallographic microscope.

[0028] Example 2

[0029] Same as Example 1, except that the first cutting depth is 0.50 mm and the second cutting depth is 0.50 mm;

[0030] After cutting, the diameter of the chip edge chipping was 9.2μm under 100x bright field observation of a metallographic microscope.

[0031] Example 3

[0032] It is basically the same as Example 1, except that the first cutting depth is 0.65 mm and the second cutting depth is 0.35 mm;

[0033] After cutting, the diameter of the chip edge chipping was 8.8μm under 100x bright field observation of a metallographic microscope.

[0034] Example 4

[0035] It is basically the same as Example 1, except that the first cutting depth is 0.56 mm and the second cutting depth is 0.44 mm;

[0036] After cutting, the diameter of the chip edge chipping was 5.6μm under 100x bright field observation of a metallographic microscope.

[0037] Example 5

[0038] It is basically the same as Example 1, except that the first cutting depth is 0.60 mm and the second cutting depth is 0.40 mm;

[0039] After cutting, the diameter of the chip edge chipping was 7.1μm under 100x bright field observation of a metallographic microscope.

[0040] Example 6

[0041] It is basically the same as Example 1, except that the first cutting depth is 0.70 mm and the second cutting depth is 0.30 mm;

[0042] After cutting, the diameter of the chip edge chipping was 12.4μm under 100x bright field observation of a metallographic microscope.

[0043] Example 7

[0044] It is basically the same as Example 1, except that the first cutting depth is 0.40 mm and the second cutting depth is 0.60 mm;

[0045] After cutting, the diameter of the chip edge chipping was 13.5μm under 100x bright field observation of a metallographic microscope.

[0046] Example 8

[0047] It is basically the same as Example 1, except that the primary cutting rate and the secondary cutting rate are both 0.5 mm / s;

[0048] After cutting, the diameter of the chip edge chipping was 3.4μm under 100x bright field observation of a metallographic microscope.

[0049] Example 9

[0050] It is basically the same as Example 1, except that the primary cutting rate and the secondary cutting rate are both 1 mm / s;

[0051] After cutting, the diameter of the chip edge chipping was 7.2μm under 100x bright field observation of a metallographic microscope.

[0052] Example 10

[0053] It is basically the same as Example 1, except that the primary cutting rate and the secondary cutting rate are both 1.2 mm / s;

[0054] After cutting, the diameter of the chip edge chipping was 10.9μm under 100x bright field observation of a metallographic microscope.

[0055] Comparative Example 1

[0056] The method is basically the same as Example 1, except that the mercury cadmium telluride chip is cut only once, and the cutting depth is 1 mm;

[0057] After cutting, the diameter of the chip edge chipping was observed under a metallographic microscope at 100 times the bright field and was 15 μm.

[0058] Comparative Example 2

[0059] The method is basically the same as Example 1, except that when the mercury cadmium telluride chip is cut, the secondary cutting is performed directly without bonding the substrate underneath, and cracks occur at a part of the chip during cutting.

[0060] Conclusion analysis:

[0061] 1. It can be seen from Examples 1-5 that when the primary cutting depth is greater than 0.58 mm or less than 0.58 mm, as the primary cutting depth changes, the diameter of the edge chipping of the mercury cadmium telluride chip continues to increase, but the obtained chip still meets the production requirements;

[0062] In contrast, in Examples 6-7 and Comparative Example 1, when the cutting depth is greater than 0.65 mm or less than 0.50 mm, or when the cutting is performed directly through the chip, the defects inside the chip will be subjected to excessive stress instantly, causing the chip edge to have a diameter greater than 10 μm, and the chip cannot be used for production.

[0063] 2. It can be seen from Examples 1 and 8-10 that when the cutting rate is between 0.5 mm and 0.8 mm, the cutting rate does not affect the diameter of the chip edge chipping, but as the rate continues to increase, the diameter of the chip edge chipping also continues to increase.

[0064] 3. It can be seen from Example 1 and Comparative Example 2 that when the chip is bonded to the substrate, it also helps to reduce the diameter of the chip edge chipping.

[0065] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement methods and shall be included in the protection scope of the present invention.

Claims

1. A method for cutting mercury cadmium telluride chips, characterized in that: The following steps are involved: Step 1: Fix the mercury cadmium telluride chip on a dicing table, and then use a dicing knife to cut it once to obtain a single-cut chip; Step 2: Use a dicing knife to perform a second dicing on the once-cut chip to obtain a cut mercury cadmium telluride chip; The thickness of the mercury cadmium telluride chip is 1 mm, the primary cutting depth is 0.50-0.65 mm, and the secondary cutting depth is 0.50-0.35 mm.

2. The cutting method according to claim 1, characterized in that: The primary cutting depth is 0.56-0.60 mm, and the secondary cutting depth is 0.44-0.40 mm.

3. The cutting method according to claim 1, characterized in that: The surface of the mercury cadmium telluride chip in step 1 is also provided with a layer of photoresist for protecting the chip, and the thickness of the photoresist is 5-8 μm.

4. The cutting method according to claim 1, characterized in that: The cutting speed of the dicing knife in step 1 and step 2 is 0.5-1 mm / s, and the cutting angle is 90°.

5. The cutting method according to claim 1, characterized in that: The fixing method in step 1 is: bonding the mercury cadmium telluride chip to a substrate, and then bonding the substrate to a dicing table, wherein the flatness of the substrate is less than 3 μm; During the secondary cutting, the dicing knife needs to penetrate 20 to 30 μm into the substrate.

6. The cutting method according to claim 5, characterized in that: The binder is at least one of paraffin wax and water-soluble glue.

7. The cutting method according to claim 5, characterized in that: The substrate material is selected from at least one of a silicon wafer, a quartz wafer, and silicon nitride.

8. A mercury cadmium telluride chip, characterized in that: The method is prepared by the mercury cadmium telluride chip cutting method according to any one of claims 1 to 7.