Walnut green seedcase carbon quantum dot and rail fastener cleaning agent

By using the microwave method to combine the cleaning agent of walnut green carbon quantum dots and other components on the track fastener, the problem of cleaning of track fasteners in the existing technology is solved, and efficient decontamination, rapid drying and film formation are achieved, and environmentally friendly and safe The effect improves the safety and stability of railway lines.

CN119018881APending Publication Date: 2024-11-26BEIJING RAILWELD NEW MATERIAL TECH CO LTD +4
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410998120.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-03-26
Filing Date
2024-07-24
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently clean without disassembling the rail fastener, and the permeability, wetting and environmental protection performance of the cleaning agent are insufficient, affecting the safety and stability of the railway line.

Method used

The walnut green-skin carbon quantum dots prepared by microwave method are used as the main component of the cleaning agent, combining diethanolamine, styrene triazole, sodium citrate, fatty alcohol polyoxyethylene ether E1008AC and trans polyether to form a highly efficient The cleaning agent can remove dirt and form a protective film without removing the fastener to prevent corrosion.

Benefits of technology

This cleaning agent has high efficiency decontamination ability, rapid drying and film formation, strong corrosion resistance, environmental protection and safety, meets environmental and human safety requirements, and increases cleaning effect through foam spraying and simplifies operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018881A_ABST
    Figure CN119018881A_ABST
Patent Text Reader

Abstract

The invention provides walnut green seedcase carbon quantum dots and a cleaning agent composition containing the walnut green seedcase carbon quantum dots. The cleaning agent composition is prepared from 1%-2% of the walnut green seedcase carbon quantum dots, 3%-5% of diethanol amine, 13%-15% of triethanolamine, 2%-3% of benzotriazole (BTA), 3%-5% of sodium citrate or potassium citrate, 4%-5% of fatty alcohol-polyoxyethylene ether E1008AC, 3%-5% of trans-polyether and the balance water. The invention further provides application of the cleaning agent to cleaning of track fasteners.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemistry and cleaning agents, and particularly relates to walnut green peel carbon quantum dots and a cleaning agent containing the walnut green peel carbon quantum dots and used for cleaning track fasteners along railways. Background Art

[0002] Track fasteners are an important component used to fix railway tracks. They are composed of multiple steel parts. They play a vital role in ensuring the stability and safe operation of railway tracks. Due to long-term direct exposure to harsh environments, a large amount of dirt and impurities will accumulate on the surface of the fasteners. If they are not cleaned in time, not only will the appearance be affected, but metal corrosion will also occur, which will have a negative impact on the mechanical properties and service life of the fasteners, and may eventually threaten the safety and stability of the railway line. Therefore, it is necessary to regularly clean the track fasteners in service. Due to the large number of fasteners and the complex disassembly and assembly process of the fasteners, it is not guaranteed that all fasteners will be disassembled, cleaned and assembled during the window period; in addition, if a component is not installed correctly, the fastener will be damaged or the track cannot be fixed. Therefore, it is not feasible to disassemble the fasteners first and then clean them offline in actual operation. It is necessary to develop a fastener cleaning agent that can be cleaned online without disassembly. Online cleaning also places high requirements on the permeability, wettability and environmental protection performance of the cleaning agent.

[0003] Carbon quantum dots (Carbon Quantum Dots) are a new type of carbon nanofunctional material, and its particle size is generally less than 10nm. Carbon quantum dots have the advantages of high stability, environmental friendliness, and good water solubility. In recent years, the application of carbon quantum dots in cleaning, descaling, and scale inhibition has also attracted people's attention. Li Hui used citric acid and L-ascorbic acid and L-lysine and anhydrous citric acid as raw materials, respectively, and synthesized L-CCQDs and Ly-CCQDs carbon quantum dot scale inhibitors by a one-pot hot melt polycondensation method (Li Hui. Preparation and performance study of carboxyl carbon quantum dot scale inhibitor [D]. Northeast Petroleum University. June 6, 2023). The invention patent application with publication number CN116376642A "An environmentally friendly nano-insulator cleaning agent and its preparation method" (publication date July 4, 2023) discloses a cleaning agent containing 0.2-0.8% carbon quantum dots, which are prepared by microwave method using ethylenediamine and citric acid as raw materials.

[0004] There is currently no application of carbon quantum dots in rail fastener cleaning. Summary of the invention

[0005] In order to overcome the deficiencies of the prior art, the present invention provides a walnut green peel carbon quantum dot, and then provides a cleaning agent containing the walnut green peel carbon quantum dot and its application in cleaning rail fasteners. The cleaning agent of the present invention has high decontamination efficiency, is safe and environmentally friendly, and can form a protective film on the surface of the fastener after cleaning, playing a certain anti-corrosion role.

[0006] In order to achieve the above technical effects, the invention adopts the following technical solutions:

[0007] A walnut green peel carbon quantum dot exhibits blue fluorescence under ultraviolet light with a wavelength of 480nm, and is prepared by a method comprising the following steps:

[0008] I. Preparation of walnut green peel dry powder:

[0009] Take fresh mature walnuts, remove the outer green skin, wash, dry, and crush through a 40-60 mesh sieve to obtain walnut green skin dry powder;

[0010] II. Preparation of walnut peel extract

[0011] The walnut green peel dry powder obtained in step I is extracted by heating and refluxing with 2 to 5 times the weight of 50 to 70% ethanol for 3 times, each time for 3 to 8 hours, filtered while hot, combined with the filtrate, filtered by suction, the filtrate is solvent recovered until there is no alcohol taste, extracted and defatted with petroleum ether at 45 to 55° C., and the petroleum ether layer is discarded; the remaining part is concentrated and dried to obtain a walnut green peel extract;

[0012] III. Preparation of walnut green peel carbon quantum dots

[0013] The walnut green peel extract obtained in step II is evenly dispersed in water, and then citric acid is added, and the reaction is carried out in a microwave reaction device for 0.5-2 hours at a reaction temperature of 200-220° C.; naturally cooled to room temperature, high-speed centrifuged, filtered, and the filter cake is vacuum freeze-dried to obtain walnut green peel carbon quantum dots.

[0014] Preferably, in step I, the drying conditions are: 60-70°C for 24-72 hours; more preferably 65°C for 48 hours.

[0015] Preferably, in step II, the concentration of ethanol is 60%.

[0016] Preferably, in step II, before the first reflux extraction, the soaking is performed for 3-8 hours; more preferably, the soaking is performed for 5 hours.

[0017] Preferably, in step II, each reflux extraction is performed for 5 hours.

[0018] Also preferably, in the step II, the volume ratio of petroleum ether to the filtrate is 1:3-1:4; more preferably 1:2.

[0019] Preferably, in step III, the mass ratio of the walnut green peel extract to water is 1:1-1:2.

[0020] Preferably, the walnut green peel extract is evenly dispersed in water by ultrasound for 20-30 minutes.

[0021] Preferably, the mass ratio of the walnut green peel extract to citric acid is 1:150-1:175; more preferably 1:155-1:170.

[0022] Preferably, the citric acid is added in the form of an aqueous solution with a mass percent concentration of 15%-35%.

[0023] More preferably, the mass percentage concentration of the citric acid aqueous solution is 30%.

[0024] Preferably, in step III, the microwave power is 700-800W.

[0025] Preferably, in step III, the reaction temperature of the walnut green peel extract and citric acid is 210°C.

[0026] Preferably, in step III, the walnut green peel extract and citric acid are reacted in a microwave reaction equipment for 1 hour.

[0027] Also preferably, in step III, the rotation speed of the high-speed centrifugation is 10000 r / min, and the centrifugation is performed for 5-10 min.

[0028] The second object of the present invention is to provide a cleaning agent composition, comprising the walnut green peel carbon quantum dots of the present invention.

[0029] As a preferred embodiment, the present invention provides a cleaning composition, the total weight of which is 100%, comprising:

[0030] The invention comprises 1-2% of walnut green peel carbon quantum dots, 3-5% of diethanolamine, 13-15% of triethanolamine, 2-3% of benzotriazole (BTA), 3-5% of sodium citrate or potassium citrate, 4-5% of fatty alcohol polyoxyethylene ether E1008AC, 3-5% of trans-polyether, and the balance of water.

[0031] The cleaning agent composition of the present invention has the following functions:

[0032] Walnut green skin carbon quantum dots: cleaning, corrosion inhibition, self-cleaning;

[0033] Fatty alcohol polyoxyethylene ether E1008AC: scale inhibition, dispersion, and enhanced permeability;

[0034] Trans-polyether: enhances permeability.

[0035] Another object of the present invention is to provide a method for preparing the above-mentioned cleaning agent composition, comprising the following steps:

[0036] S1: Prepare various raw materials according to weight percentage;

[0037] S2: Add water to a mixing device with a stirring device, add diethanolamine, triethanolamine, benzotriazole and sodium citrate while stirring, and stir to react for 1-2 hours; then add fatty alcohol polyoxyethylene ether E1008AC and trans-polyether in sequence, and stir to react for 2-3 hours; finally, add walnut green peel carbon quantum dots, and stir to react for 0.5-1 hour to obtain.

[0038] Preferably, in step S2, the stirring speed is 500-700 r / min.

[0039] The present invention also provides application of the cleaning agent composition in cleaning rail fasteners.

[0040] Specifically, the application includes the following operations:

[0041] The cleaning agent composition of the present invention is loaded into a foam generating device, which is started to spray the foam directly onto the surface of the rail fastener to be cleaned until the fastener is covered, and the foam is left to stand for 10-20 minutes, and then rinsed with water to remove the foam and dried naturally.

[0042] In this specification, unless otherwise specified, the "water" is purified water, such as deionized water, distilled water, double distilled water, etc. In this specification, the concentration of ethanol is the volume percentage concentration.

[0043] The cleaning agent provided by the present invention has the following advantages:

[0044] 1. High-efficiency decontamination: The cleaning agent has a strong decontamination ability and can effectively remove stains and impurities on the surface of the spring clip fastener, such as dirt, rust, paint, etc. The cleaning agent of the present invention has a high foaming rate and fine foam, which increases the bonding area between the cleaning agent and the fastener, and helps the cleaning agent to remove dirt.

[0045] 2. Rapid drying and film formation: The cleaning agent remaining on the surface of the fastener can quickly dry and form a film, thereby providing temporary protection for the metal surface and preventing sudden contact with air after cleaning, which may cause secondary oxygen corrosion.

[0046] 3. Corrosion resistance: The cleaning agent of the present invention uses plant-derived walnut green peel carbon quantum dots as corrosion inhibitors to reduce corrosion and damage to spring clip fasteners.

[0047] 4. Environmental protection and safety: The cleaning agent of the present invention does not contain harmful chemical substances such as N and P, is harmless to the environment and human body, and meets environmental protection requirements.

[0048] 5. Easy to use: The cleaning agent of the present invention is easy to use, simple to operate, and easy to clean, and does not require special equipment and manpower.

[0049] Walnut green peel is rich in polyphenols. The present invention prepares it into carbon quantum dots and applies it to the cleaning of rail fasteners, turning the walnut green peel into "treasure", providing a way to generate good social and economic benefits for the walnut green peel. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] The present invention will be further described below in conjunction with the accompanying drawings.

[0051] Figure 1 It is the Nyquist plot of the 45# steel test piece in Example 1 immersed in corrosion inhibitor aqueous solutions of different concentrations.

[0052] Figure 2 It is a polarization curve diagram of the 45# steel test piece in Example 1 immersed in corrosion inhibitor aqueous solutions of different concentrations.

[0053] Figure 1 and Figure 2 middle,

[0054] 1: 3% HCl (500 ml);

[0055] 2: 3% HCl (500ml) + 300mg / L walnut green peel carbon quantum dots aqueous solution 30ml;

[0056] 3: 3% HCl (500ml) + 30ml of 600mg / L walnut peel carbon quantum dots aqueous solution.

[0057] Figure 3 Atomic force images of the 45# steel specimens in Example 1 after being immersed in corrosion inhibitor aqueous solutions of different concentrations for 24 hours; wherein:

[0058] (a): Atomic force image of a 45# steel specimen after being immersed in 500 ml 3% HCl for 24 hours;

[0059] (b): Atomic force image of 45# steel specimen after being immersed in 500ml 3% HCl + 300mg / L walnut green peel carbon quantum dot aqueous solution 30ml corrosion inhibitor aqueous solution for 24 hours;

[0060] (c) Atomic force image of a 45# steel specimen after being immersed in a corrosion inhibitor aqueous solution of 500ml 3% HCl + 30ml 600mg / L walnut green peel carbon quantum dots aqueous solution for 24 hours.

[0061] Figure 4 This is a SEM picture of the metal surface after cleaning with the cleaning agent of Example 4 after the oil cleaning power was measured in Test Example 1.

[0062] Figure 5 This is a photo of the track fasteners before and after cleaning in Application Example 1, where:

[0063] (a): Photo before cleaning;

[0064] (b): Photo being cleaned;

[0065] (c): Photo after cleaning. DETAILED DESCRIPTION

[0066] The present invention is described below with reference to specific examples. It will be appreciated by those skilled in the art that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention in any way.

[0067] The experimental methods in the following examples are conventional methods unless otherwise specified. The raw materials, reagents, etc. used in the following examples are commercially available products unless otherwise specified. The purchase of some raw materials and reagents is as follows:

[0068] Trans-polyether: purchased from Shanghai Lingjin Chemical Technology Co., Ltd.

[0069] Example 1 Preparation and performance study of walnut green peel carbon quantum dots

[0070] 1. Preparation of Walnut Peel Carbon Quantum Dots

[0071] 1.1 Preparation of walnut green peel carbon quantum dots by microwave method:

[0072] I. Preparation of walnut green peel dry powder

[0073] Take fresh mature walnuts, take 10 kg of the outer green peel, wash it, dry it at 65°C for 48 hours, and crush it through a 60-mesh sieve to obtain 1 kg of walnut green peel dry powder.

[0074] II. Preparation of walnut peel extract

[0075] The walnut green peel dry powder obtained in step I is soaked in 5 times by weight of 60% (v / v) ethanol for about 5 hours, heated and refluxed for extraction for 5 hours, and filtered while hot; the residue is heated and refluxed for extraction twice with 60% (v / v) ethanol, each time with 5 times by weight of ethanol, each time refluxed for extraction for about 5 hours, filtered while hot, the filtrates of each time are combined, filtered with suction, the filtrate is extracted and filtered at 50° C., and degreased with petroleum ether twice the volume of the filtrate, and the petroleum ether layer is discarded; the remaining part is concentrated and dried to obtain a walnut green peel extract;

[0076] III. Preparation of walnut green peel carbon quantum dots

[0077] III-1: Disperse 100 mg of the walnut peel extract obtained in step II in 100 ml of water, ultrasonicate for 30 minutes until uniformly dispersed, then add 50 ml of 30% (w / w) citric acid aqueous solution (density 1.12 g / ml), react in a microwave reaction equipment for 1 hour, and the reaction temperature is 210°C; naturally cool to room temperature, high-speed centrifuge at 10000 r / min, filter, and vacuum freeze-dry the filter cake to obtain 27 mg of walnut peel carbon quantum dots, which exhibit blue fluorescence under ultraviolet light at 480 nm.

[0078] III-2: Disperse 100 mg of the walnut peel extract obtained in step II in 100 ml of water, ultrasonicate for 30 minutes until uniformly dispersed, then add 50 ml of 30% (w / w) citric acid aqueous solution (density 1.12 g / ml), react in a microwave reaction equipment for 1 hour, and the reaction temperature is 190°C; naturally cool to room temperature, high-speed centrifuge at 10000 r / min, filter, and vacuum freeze-dry the filter cake to obtain 16 mg of walnut peel carbon quantum dots, which exhibit blue fluorescence under ultraviolet light at 480 nm.

[0079] III-3: Disperse 100 mg of the walnut peel extract obtained in step II in 100 ml of water, ultrasonicate for 30 minutes until uniformly dispersed, then add 50 ml of 30% (w / w) citric acid aqueous solution (density 1.12 g / ml), react in a microwave reaction equipment for 1 hour, and the reaction temperature is 230°C; naturally cool to room temperature, high-speed centrifuge at 10000 r / min, filter, and vacuum freeze-dry the filter cake to obtain 13 mg of walnut peel carbon quantum dots, which exhibit blue fluorescence under ultraviolet light at 480 nm.

[0080] The microwave reaction temperature has an effect on the yield of walnut green peel carbon quantum dots. The reaction yield is highest when the reaction temperature is 210°C, which is the preferred condition of the present invention.

[0081] The walnut green peel carbon quantum dots prepared under the above three temperature conditions were combined for performance research and measurement.

[0082] 2. Study and determination of the properties of walnut green peel carbon quantum dots

[0083] 2.1 Study on biodegradability

[0084] According to GB / T15818-2018 "Biodegradation Test Method", walnut green peel carbon quantum dots were tested. The foam method was used for determination:

[0085] The degradation degree of 20 mg / L walnut peel carbon quantum dots solution was 100% on the 20th day.

[0086] This indicates that the walnut green peel carbon quantum dots of the present invention have good environmental performance and can be slowly degraded in the natural environment.

[0087] 2.2 Study on corrosion inhibition performance

[0088] Walnut green peel carbon quantum dots were prepared into 300 mg / L and 600 mg / L aqueous solutions with water, 30 ml of the aqueous solution was added into 500 ml of 3% HCl aqueous solution, and mixed evenly to obtain corrosion inhibitor solutions of different concentrations.

[0089] The 45# steel specimens were immersed in the above-mentioned corrosion inhibitor solutions of different concentrations and 3% HCl aqueous solution for 24 h, and the electrochemical impedance was measured using an electrochemical workstation to obtain the Nyquist plots and polarization curves of the steel in the corrosion inhibitor solutions of different concentrations, as shown in Figure 1. Figure 1 and Figure 2 The larger the radius of the capacitive arc in the Nyquist diagram, the smaller the corrosion rate of the metal, that is, the higher the corrosion inhibition efficiency of the corrosion inhibitor. In the polarization curve diagram, the lower the corrosion current density, the higher the corrosion inhibition efficiency.

[0090] like Figure 1 As shown in the figure, with the increase of the concentration of walnut peel carbon quantum dots, the radius of the capacitive reactance arc also increases, indicating that walnut peel carbon quantum dots can significantly reduce the corrosion of steel, especially when the concentration is 600 mg / L, the corrosion inhibition effect is the best.

[0091] like Figure 2 As shown in the figure, with the increase of the concentration of walnut green peel carbon quantum dots, the corrosion current density continues to decrease and the corrosion inhibition efficiency increases.

[0092] Atomic force microscopy is a powerful tool for observing surface microstructures. The 45# steel specimens immersed in different concentrations of corrosion inhibitor solutions and 3% HCl aqueous solution for 24 hours were photographed under an atomic force microscope, and the atomic force images of each steel specimen were obtained by processing with the software Gwyddion. Figure 3 .

[0093] Figure 3 (a) shows that after the steel is immersed in a 3% HCl solution without the addition of the walnut green peel carbon quantum dots of the present invention for 24 hours, it corrodes severely and forms many large pit-peak rough structures; after being immersed in a corrosion inhibitor solution containing walnut green peel carbon quantum dots for 24 hours, the surface of the steel becomes relatively flat, indicating that the corrosion rate is significantly reduced, and this trend becomes more obvious as the concentration of walnut green peel carbon quantum dots increases ( Figure 3 (b) and (c)).

[0094] In summary, the walnut green peel carbon quantum dots of the present invention have good anti-corrosion and corrosion inhibition effects. In addition, walnut green peel is widely available, cheap and easy to obtain. The present invention also provides a way to create value for the walnut green peel that is usually discarded, thereby turning waste into treasure.

[0095] Example 2-4 A cleaning agent composition

[0096] The cleaning compositions of Examples 2-4 all include walnut green peel carbon quantum dots prepared according to the method of Example 1, and the specific composition is shown in Table 1. They are prepared by the following method:

[0097] S1. Prepare each component according to mass percentage;

[0098] S2. Add water to a mixing device with a stirring device, add diethanolamine, triethanolamine, benzotriazole and sodium citrate at a stirring speed of 600r / min, and stir to react for 1-2 hours; then add fatty alcohol polyoxyethylene ether E1008AC and trans-polyether in sequence, maintain the stirring speed, and react for 2-3 hours; finally, add walnut peel carbon quantum dots, maintain the stirring speed, and react for 0.5-1 hour. The resulting transparent solution is the target product.

[0099] Comparative Example 1-3 A cleaning agent composition

[0100] The specific compositions of the cleaning compositions of Comparative Examples 1-3 are shown in Table 1, and are prepared by the same method and steps as Examples 2-5.

[0101] Table 1 Composition of the cleaning composition of Examples 2-4 and Comparative Examples 1-3 (unit: % w / w)

[0102]

[0103] Test Example 1 Performance Determination of the Cleaning Compositions of the Examples and Comparative Examples

[0104] 1. Oil cleaning power:

[0105] According to the provisions of Q / CR468-2015 "EMU External Surface Cleaning Agent", a paint coating test piece is used. Take 500ml of the cleaning agent of Examples 2-4 and Comparative Examples 1-3 respectively and place it in a beaker, and then put the beaker into a (40±2)℃ constant temperature water bath. Fix the oily test piece (pre-weighed) to the fixture of the swing washing machine, and immerse it in the cleaning agent in each beaker, soak and swing wash for 3 minutes. After taking out, put the test piece into a (50±2)℃ oven, dry, cool, weigh, and calculate the cleaning power. The results are shown in Table 2.

[0106] Table 2 Determination results of the cleaning power of the cleaning agent compositions of the examples and comparative examples

[0107] Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Cleaning power 83% 89% 93% 73% 68% 80%

[0108] The results show that the cleaning composition of each example has better degreasing ability than each comparative example, and the cleaning composition of Example 4 has the best degreasing ability.

[0109] SEM images were taken of the metal surface cleaned by the cleaning agent composition of Example 4 to test whether walnut green husk carbon quantum dots existed on the metal surface. Figure 4 As shown in the figure, the black dots on the surface of the substrate are carbon quantum dots. These carbon quantum dots adhere to the surface of the substrate to form a protective film, which temporarily protects the metal, thereby preventing the cleaned metal from being immediately corroded by corrosive components in the air, and extending the service life of the fastener.

[0110] 2. Metal Corrosion

[0111] The cleaning agent compositions of Examples 2-4 and Comparative Examples 1-3 were respectively prepared with deionized water into solutions with a mass percentage concentration of 5% to obtain test solutions. Brass, aluminum alloy, and steel sheets were weighed using a balance, respectively placed in the prepared test solutions, and then placed in a (40±2)℃ constant temperature water bath for 4 hours. After the test, the test pieces were taken out, rinsed with clean water, then washed twice with anhydrous ethanol, dried with hot air, dried, cooled, and the appearance of the test pieces was observed and rated. The results are shown in Table 3.

[0112] Table 3 Metal corrosion test results of the cleaning agent compositions of the examples and comparative examples

[0113] Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 brass Level 0 Level 0 Level 0 Level 0 Level 1 Level 1 Aluminum Alloy Level 1 Level 1 Level 0 Level 2 Level 1 Level 2 Steel sheet Level 1 Level 0 Level 0 Level 1 Level 1 Level 2

[0114] Note: Level 0: No discoloration or loss of gloss on the metal surface;

[0115] Level 1: The metal surface loses its gloss or changes color slightly, but still has metallic luster;

[0116] Level 2: The metal surface is obviously dull, discolored, or has spots.

[0117] The results show that the metal corrosiveness of the cleaning composition of the present invention is less than that of the comparative example, and the corrosiveness of Example 4 is the lowest.

[0118] 3. Contact angle test

[0119] According to GB / T 30693-2014 Measurement of contact angle between plastic film and water, the contact angle of the cleaning composition of each embodiment and comparative example on the plastic surface was measured using a video contact angle meter. The results are shown in Table 4.

[0120] The results show that the water contact angles of the detergent compositions of the present invention are significantly greater than those of the comparative examples, and the contact angle of Example 4 is the largest, indicating that the detergent compositions of the present invention can impart a certain self-cleaning ability to the surface.

[0121] Table 4 Contact angles of the cleaning compositions of Examples and Comparative Examples with water

[0122] serial number Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Contact angle 120° 120° >150° 50° 100° 20°

[0123] 4. Foaming

[0124] According to the method specified in GB / T13173, the instantaneous foam height of the cleaning agent composition of each embodiment and comparative example was tested at (40±2)°C / mm. The results are shown in Table 5.

[0125] Table 5 Foaming test results of the cleaning composition of the examples and comparative examples

[0126] serial number Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Foaming / mm 90 100 105 75 50 80

[0127] The higher the instant height of the foam of the detergent, the better its cleaning performance. The results show that the instant height of the foam of the detergent composition of the present invention is significantly higher than that of the comparative example, among which the instant height of Example 4 is the highest, indicating that it has the best cleaning performance.

[0128] Through the testing of the cleaning agent composition's decontamination ability, metal corrosion, contact angle, foaming property and other properties, the cleaning agent of the present invention is generally superior to the comparative examples, wherein Example 4 is a preferred embodiment of the present invention.

[0129] Application Example 1 On-site application of the cleaning composition of Example 4

[0130] Before cleaning the rail fasteners, there are many stains on the surface, such as Figure 5 The cleaning agent composition prepared according to the formula and preparation method of Example 4 is sprayed on the surface of the fastener through a foam generating device (spray can) to cover the fastener, such as Figure 5 After 15 minutes, rinse the fastener with tap water, and all stains on the fastener surface have been completely removed, revealing the base color, as shown in (b). Figure 5 as shown in (c).

Claims

1. A walnut green peel carbon quantum dot, which exhibits blue fluorescence under ultraviolet light with a wavelength of 480nm, is prepared by a method comprising the following steps: I. Preparation of walnut green peel dry powder: Take fresh mature walnuts, remove the outer green skin, wash, dry, and crush through a 40-60 mesh sieve to obtain walnut green skin dry powder; II. Preparation of walnut peel extract The walnut green peel dry powder obtained in step I is extracted by heating and refluxing with 2 to 5 times the weight of 50 to 70% ethanol for 3 times, each time for 3 to 8 hours, filtered while hot, combined with the filtrate, filtered by suction, the filtrate is solvent recovered until there is no alcohol taste, extracted and defatted with petroleum ether at 45 to 55° C., and the petroleum ether layer is discarded; the remaining part is concentrated and dried to obtain a walnut green peel extract; III. Preparation of walnut green peel carbon quantum dots The walnut green peel extract obtained in step II is evenly dispersed in water, and then citric acid is added, and the reaction is carried out in a microwave reaction device for 0.5-2 hours at a reaction temperature of 200-220° C.; naturally cooled to room temperature, high-speed centrifuged, filtered, and the filter cake is vacuum freeze-dried to obtain walnut green peel carbon quantum dots.

2. The walnut green peel carbon quantum dots according to claim 1, characterized in that In step I, the drying conditions are: 60-70°C for 24-72 hours; more preferably 65°C for 48 hours.

3. The walnut green peel carbon quantum dots according to claim 1, characterized in that In step II, the concentration of ethanol is 60%; Preferably, in step II, before the first reflux extraction, the mixture is soaked for 3-8 hours; more preferably, for 5 hours; Preferably, in step II, each reflux extraction is performed for 5 hours; Also preferably, in the step II, the volume ratio of petroleum ether to the filtrate is 1:3-1:4; more preferably 1:

2.

4. The walnut green peel carbon quantum dots according to claim 1, characterized in that In the step III, the mass ratio of the walnut green peel extract to water is 1:1-1:2; Preferably, the walnut green peel extract is evenly dispersed in water by ultrasound for 20-30 minutes; Preferably, the mass ratio of the walnut green peel extract to citric acid is 1:150-1:175; more preferably 1:155-1:170; Preferably, the citric acid is added in the form of an aqueous solution with a mass percentage concentration of 15%-35%; More preferably, the mass percentage concentration of the citric acid aqueous solution is 30%.

5. The walnut green peel carbon quantum dots according to claim 1 or 4, characterized in that: In step III, the microwave power is 700-800W; Preferably, in step III, the reaction temperature of the walnut green peel extract and citric acid is 210° C.; Preferably, in step III, the walnut green peel extract and citric acid are reacted in a microwave reaction device for 1 hour; Also preferably, in step III, the rotation speed of the high-speed centrifugation is 10000 r / min, and the centrifugation is performed for 5-10 min.

6. A cleaning agent composition comprising the walnut green peel carbon quantum dots according to any one of claims 1 to 5.

7. The cleaning composition according to claim 6, comprising: The walnut green peel carbon quantum dots are 1-2%, diethanolamine is 3-5%, triethanolamine is 13-15%, benzotriazole (BTA) is 2-3%, sodium citrate or potassium citrate is 3-5%, fatty alcohol polyoxyethylene ether E1008AC is 4-5%, trans-polyether is 3-5%, and the balance is water.

8. A method for preparing the cleaning composition according to claim 6 or 7, comprising the following steps: S1: Prepare various raw materials according to weight percentage; S2: Add water to a mixing device with a stirring device, add diethanolamine, triethanolamine, benzotriazole and sodium citrate while stirring, and stir to react for 1-2 hours; then add fatty alcohol polyoxyethylene ether E1008AC and trans-polyether in sequence, and stir to react for 2-3 hours; finally, add walnut green peel carbon quantum dots, and stir to react for 0.5-1 hour to obtain; Preferably, in step S2, the stirring speed is 500-700 r / min.

9. Use of the cleaning agent composition according to claim 6 or 7 or the cleaning agent composition prepared according to the preparation method according to claim 8 in cleaning rail fasteners.

10. The use according to claim 9, characterized in that: The application includes the following operations: The cleaning agent composition according to claim 6 or 7 or the cleaning agent composition prepared by the preparation method according to claim 8 is loaded into a foam generating device, the foam generating device is started, and the foam is directly sprayed onto the surface of the rail fastener to be cleaned until the fastener is covered, and the foam is allowed to stand for 10-20 minutes, and then rinsed with water to remove the foam and dried naturally.