High-tap-density layered oxide positive electrode material precursor for sodium ion battery as well as preparation method and application of high-tap-density layered oxide positive electrode material precursor
By regulating the process parameters during the co-precipitation of sodium ion batteries, a high-voltage sodium positive electrode material precursor was prepared, which solved the problem of low tap density in the existing technology, improved the energy density and cycle life of the battery, and improved the energy density and cycle life of the battery. electrochemical properties.
Patent Information
- Application Number
- CN202411130936.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
The precursors of the layered transition metal oxide positive electrode materials of existing sodium ion batteries have the problem of low tap density in industrial mass production, which affects the energy density and cycle life of the battery.
By co-precipitation, the process parameters such as rotation speed, solid-liquid ratio, pH and complexing agent concentration are coordinated to regulate the density of the precursor, and a precursor with relatively dense particle morphology and high tap density are prepared. .
It improves the energy density and cycle life of sodium ion batteries, improves electrochemical performance, and is suitable for the industrial production of different series of sodium-electric layered oxide positive electrode material precursors.
Smart Images

Figure CN119018943A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a high-tap layered oxide positive electrode material precursor for sodium ion batteries, and a preparation method and application thereof. Background Art
[0002] Sodium-ion batteries have attracted more and more attention due to their advantages of low cost and high safety. The key material of sodium-ion batteries is the cathode material, and its production cost is one of the main factors determining the cost of sodium-ion batteries. The development of advanced cathode materials with large-scale production capacity is the key to realizing the commercial application of sodium-ion batteries.
[0003] Layered transition metal oxide cathode materials for sodium ion batteries (Na x TMO 2 TM=Fe, Mn, Ni, Cu, Zn, etc.) is not only low in cost, with a wide range of raw materials, but also simple in synthesis process, which is convenient for large-scale industrial production. It also has the advantages of high energy density, high voltage platform, excellent comprehensive performance, and flexible chemical composition design. It is the mainstream research direction of positive electrode materials for sodium ion batteries. Among them, Fe, Mn, Ni, Cu and Zn are the best elements for building low-cost commercial layered oxide positive electrode materials.
[0004] Since the precursor directly determines the core electrochemical properties of the cathode material, the precursor of the layered oxide cathode material (Ni x TM 1-x (OH) 2 The research on )(0<x<1, TM=Fe, Mn, Cu, Zn, etc.) is of great significance to the development of sodium-ion batteries. At present, the precursors of layered oxide cathode materials for sodium-ion batteries are mainly produced in large quantities industrially by liquid phase co-precipitation method. High tap density precursor materials generally have low specific surface area, which is beneficial to improve the tap density and compaction density of cathode materials, as well as improve the energy density and cycle life of sodium-ion batteries. Therefore, the development of high tap density sodium cathode material precursors is crucial to improving the electrochemical performance of sodium-ion batteries.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] One of the purposes of the present invention is to provide a method for preparing a high-tap layered oxide positive electrode material precursor for a sodium ion battery. During the coprecipitation process, the density of the primary particle stacking of the precursor is effectively regulated by the coordinated regulation of process parameters such as rotation speed, solid-liquid ratio, pH and complexing agent concentration. The obtained sodium battery precursor has a relatively dense particle morphology and a relatively high tap density, and has good sphericity.
[0007] A second object of the present invention is to provide a sodium ion battery positive electrode material, which is beneficial to improving the energy density and cycle life of the battery.
[0008] A third object of the present invention is to provide a sodium ion battery with excellent electrochemical performance.
[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0010] In a first aspect, a method for preparing a high-tap layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0011] Passing a mixed metal salt solution, a precipitant and a complexing agent into a reactor in which a base liquid has been adjusted to perform a coprecipitation reaction, controlling the concentration of the mixed metal salt solution to be ≤2.0 mol / L, the concentration of the precipitant to be ≤11.0 mol / L, and the concentration of the complexing agent to be ≤10.0 mol / L, and coordinating and controlling the process parameters such as the rotation speed, solid-liquid ratio, pH and complexing agent concentration, continuously passing an inert gas during the reaction, and continuing the reaction until the particle size of the product reaches the target particle size, thereby obtaining the positive electrode material precursor;
[0012] In the granulation stage, the pH value in the reaction kettle is controlled to be a first pH value, the complexing agent value is a first complexing agent concentration value, and the rotation speed value is a first rotation speed value; in the growth stage, the pH value in the reaction kettle is controlled to be a second pH value, the complexing agent value is a second complexing agent concentration value, and the rotation speed value is a second rotation speed value;
[0013] Wherein, 12.50>first pH value>second pH value>9.50, 0.01mol / L≤first complexing agent concentration value<second complexing agent concentration value≤1.0mol / L, 800r / min≥first speed value>second speed value≥300r / min;
[0014] The solid-liquid ratio in the coprecipitation process is 300 g / L or above.
[0015] Furthermore, the chemical composition of the positive electrode material precursor is as follows:
[0016] Ni x TM 1-x (OH) 2 , 0<x<1, TM is a metal ion;
[0017] Wherein, TM is selected from one or more of Fe, Mn, Cu and Zn.
[0018] Furthermore, the preparation method comprises the following steps:
[0019] (a) According to the chemical composition of the positive electrode material precursor, metal salts are mixed to obtain a mixed metal salt solution:
[0020] (b) The mixed metal salt solution of step (a) is first subjected to a nucleation reaction in the presence of a complexing agent and a precipitant, and then subjected to a growth reaction until the D50 particle size of the product reaches a target particle size, and the product is sequentially aged, centrifuged, dried, sieved, demagnetized and packaged to obtain a sodium cathode material precursor.
[0021] Furthermore, the particle size D50 of the positive electrode material precursor is 3.0-15.0 um.
[0022] Further, the precipitant is sodium hydroxide or potassium hydroxide;
[0023] Preferably, the complexing agent is ammonia water or oxalic acid solution;
[0024] Preferably, the reaction temperature is 30-70°C;
[0025] Preferably, the reaction speed is 300-800r / min;
[0026] Preferably, the inert gas is nitrogen or argon.
[0027] Furthermore, the precipitant is sodium hydroxide, the complexing agent is ammonia water or oxalic acid solution, and the inert gas is nitrogen.
[0028] In a second aspect, a sodium ion battery layered oxide positive electrode material precursor is prepared by any of the preparation methods described above.
[0029] Furthermore, the tap density of the positive electrode material precursor is 1.30-2.20 g / cm 3 .
[0030] In a third aspect, a positive electrode material for a sodium ion battery is mainly prepared using the positive electrode material precursor described above.
[0031] In a fourth aspect, a sodium ion battery is provided, wherein the positive electrode of the sodium ion battery comprises the positive electrode material described above.
[0032] Compared with the prior art, the present invention has at least the following beneficial effects:
[0033] The invention provides a method for preparing a high-tap layered oxide positive electrode material precursor (sodium battery precursor) for a sodium ion battery. The method coordinately controls process parameters such as rotation speed, solid-liquid ratio, pH value and complexing agent concentration during a coprecipitation process. Through the synergistic effect of the parameters, the density of the primary particle stacking of the precursor is effectively controlled. The obtained sodium battery precursor has a relatively dense particle morphology and a relatively high tap density, and has good sphericity.
[0034] The purpose of regulating the rotation speed is: within the appropriate range, if the stirring speed is too low, the precursor crystal particles will grow too fast, the sphericity will deteriorate, the particle voids will increase, and the specific surface area will increase; while if the stirring speed is appropriately increased, the fluid shear stress on the precursor crystal particles will become stronger, the growth rate of new grains on the original secondary particles will slow down, the primary particles will be more densely packed, the particle voids will decrease, the specific surface area will decrease, the tap density will increase, and the sphericity will also improve.
[0035] The purpose of regulating the solid-liquid ratio is: in the precursor reaction process, the solid-liquid ratio refers to the ratio of the solid mass to the liquid mass of the precursor slurry. Different solid-liquid ratios have different effects on product performance. Properly increasing the solid-liquid ratio can reduce the growth rate of secondary particles, make the primary particles more compact, and thus optimize the product morphology and increase the product tap density.
[0036] The purpose of regulating pH and complexing agent is: high pH value is conducive to the formation of crystal nuclei, low pH value is conducive to the growth of crystal nuclei, and complexing agent achieves the purpose of co-precipitation by complexing metal ions first and then precipitating. The appropriate concentration can effectively complex metal ions in the solution and reduce the growth rate of precursor crystal particles. In the nucleation stage and growth stage, the growth rate of secondary particles can be effectively regulated by synergistically regulating pH and complexing agent concentration, thereby regulating the tap density of the product.
[0037] Therefore, by synergistically controlling process parameters such as rotation speed, solid-liquid ratio, pH and complexing agent concentration, a synergistic effect can be achieved, thereby synergistically controlling the growth rate of precursor crystal particles and ultimately controlling the tap density of the product.
[0038] At the same time, the preparation method of the present invention is suitable for preparing different series of sodium electrode layered oxide positive electrode material precursors, such as nickel manganese (NiMn), nickel iron manganese (NiFeMn), nickel iron manganese zinc (NiFeMnZn) and nickel iron manganese copper (NiFeMnCu) series. It not only has a wide range of applications, but is also easy to operate and control, and is very suitable for industrial production.
[0039] The sodium ion battery layered oxide positive electrode material precursor provided by the present invention has a relatively dense particle morphology and a relatively high tap density, and has good sphericity.
[0040] The sodium ion battery positive electrode material provided by the present invention is beneficial to improving the battery energy density and cycle life.
[0041] The sodium ion battery provided by the present invention has excellent electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0043] Figure 1 A flow chart for preparing a sodium electrode precursor provided in one embodiment of the present invention;
[0044] Figure 2 This is a SEM image of the sodium electrode precursor provided in Example 1 of the present invention;
[0045] Figure 3 This is a SEM image of the sodium electrode precursor provided in Example 2 of the present invention;
[0046] Figure 4 This is a SEM image of the sodium electrode precursor provided in Example 3 of the present invention;
[0047] Figure 5 This is a SEM image of the sodium electrode precursor provided in Example 4 of the present invention;
[0048] Figure 6 This is a SEM image of the sodium electrode precursor provided in Example 5 of the present invention;
[0049] Figure 7 This is a SEM image of the sodium electrode precursor provided in Comparative Example 1 of the present invention;
[0050] Figure 8 This is a SEM image of the sodium electrode precursor provided in Comparative Example 2 of the present invention;
[0051] Fig. 9 This is a SEM image of the sodium electrode precursor provided in Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0052] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] According to a first aspect of the present invention, there is provided a method for preparing a high-tap layered oxide positive electrode material precursor for a sodium ion battery, comprising the following steps:
[0054] A mixed metal salt solution, a precipitant and a complexing agent are introduced into a reactor in which a base liquid has been adjusted to perform a co-precipitation reaction, the concentration of the mixed metal salt solution is controlled to be ≤2.0 mol / L, the concentration of the precipitant is ≤11.0 mol / L, and the concentration of the complexing agent is ≤10.0 mol / L, and the process parameters such as the rotation speed, solid-liquid ratio, pH and complexing agent concentration are coordinated and regulated. An inert gas is continuously introduced during the reaction, and the reaction is continued until the particle size of the product reaches the target particle size, thereby obtaining a positive electrode material precursor;
[0055] In the granulation stage, the pH value in the reaction kettle is controlled to be a first pH value, the complexing agent value is a first complexing agent concentration value, and the rotation speed value is a first rotation speed value; in the growth stage, the pH value in the reaction kettle is controlled to be a second pH value, the complexing agent value is a second complexing agent concentration value, and the rotation speed value is a second rotation speed value;
[0056] Wherein, 12.50>first pH value>second pH value>9.50, 0.01mol / L≤first complexing agent concentration value<second complexing agent concentration value≤1.0mol / L, 800r / min≥first speed value>second speed value≥300r / min;
[0057] The solid-liquid ratio during the co-precipitation process is 300 g / L or above.
[0058] The preparation method of the present invention coordinates and controls the process parameters such as the rotation speed, solid-liquid ratio, pH and complexing agent concentration in the liquid phase co-precipitation process. Under the coordinated cooperation of various parameters, the density of the primary particle accumulation of the sodium battery precursor is effectively controlled. The obtained sodium battery precursor has a relatively dense particle morphology and a relatively high tap density, and has good sphericity.
[0059] At the same time, the preparation method of the present invention is suitable for preparing different series of sodium electrode layered oxide positive electrode material precursors, such as nickel manganese (NiMn), nickel iron manganese (NiFeMn), nickel iron manganese zinc (NiFeMnZn) and nickel iron manganese copper (NiFeMnCu) series. It not only has a wide range of applications, but is also easy to operate and control, and is suitable for industrial mass production.
[0060] In a preferred embodiment, the chemical composition of the sodium positive electrode material precursor is as follows:
[0061] Ni x TM 1-x (OH) 2 , 0<x<1, TM is a metal ion;
[0062] Wherein, TM is selected from one or more of Fe, Mn, Cu and Zn.
[0063] In a preferred embodiment, the preparation method of the present invention comprises the following steps:
[0064] (a) According to the chemical composition of the positive electrode material precursor, metal salts are mixed to obtain a mixed metal salt solution:
[0065] (b) The mixed metal salt solution of step (a) is first subjected to a nucleation reaction in the presence of a complexing agent and a precipitant, and then subjected to a growth reaction until the D50 particle size of the product reaches a target particle size, and the product is sequentially aged, centrifuged, dried, sieved, demagnetized and packaged to obtain a sodium cathode material precursor.
[0066] In the present invention, the complexing agent may be ammonia water or oxalic acid, and the precipitating agent includes but is not limited to sodium hydroxide. Using ammonia water or oxalic acid as the complexing agent and sodium hydroxide as the precipitating agent is more conducive to realizing different series of sodium electrode precursors (Ni x TM 1-x (OH) 2 , TM=Fe, Mn, Cu, Zn, etc.) secondary particles grow smoothly.
[0067] In a preferred embodiment, the reaction temperature may be 30-70°C, typical but non-limiting temperatures include 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C.
[0068] In a preferred embodiment, the reaction speed may be 300-800 r / min, and typical but non-limiting speeds may be 400 r / min, 450 r / min, 500 r / min, 550 r / min, 600 r / min, 650 r / min, 700 r / min.
[0069] The flow chart of the preparation method of the present invention is shown in Figure 1 , a mixed metal salt solution, a complexing agent and a precipitant are pumped into a reactor at the same time for a co-precipitation reaction. First, a nucleation reaction is carried out, and then a growth reaction is carried out. During the co-precipitation process, by synergistically controlling process parameters such as stirring speed, pH value, complexing agent concentration, solid-liquid ratio and reaction temperature, the density of the precursor primary particle accumulation is effectively controlled with the coordinated cooperation of various parameters. Then, post-treatment is carried out in sequence, including aging, centrifugation, drying, screening, demagnetization and packaging. After the physical and chemical indicators are tested to be qualified, a sodium electric precursor is obtained.
[0070] According to a second aspect of the present invention, there is provided a sodium ion battery layered oxide positive electrode material precursor, which is prepared by any of the preparation methods described above and has a relatively dense particle morphology and a relatively high tap density, and good sphericity.
[0071] In the present invention, the tap density of the cathode material precursor can be 1.30-2.20 g / cm 3 .
[0072] According to a third aspect of the present invention, there is provided a sodium ion battery layered positive electrode material, which is prepared using the high-tap positive electrode material precursor described above, and is beneficial to improving the energy density and cycle life of the battery.
[0073] According to a fourth aspect of the present invention, a sodium ion battery is provided, wherein the positive electrode of the sodium ion battery comprises the positive electrode material described above and has excellent electrochemical performance.
[0074] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.
[0075] Example 1
[0076] A method for preparing a high-tap layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0077] S1: pure water was added to the reactor and heated to 35°C, and nitrogen was introduced at a flow rate of 30L / h, and then an ammonia solution was added to adjust the ammonium concentration of the bottom liquid to 0.18mol / L, and then a sodium hydroxide solution was added to adjust the pH value of the bottom liquid to 12.20, and the stirring blade inside the reactor was stirred at a speed of 600r / min to mix the bottom liquid evenly to obtain the bottom liquid of the coprecipitation reaction;
[0078] S2: 2.0 mol / L nickel-manganese mixed salt solution, 11.0 mol / L sodium hydroxide solution, and 7.5 mol / L ammonia solution are simultaneously pumped into the above reactor, and the molar ratio of nickel and manganese is controlled to be 50:50. The reaction is carried out for 1 hour under the conditions that the pH value in the reactor is maintained at 12.20 and the ammonium concentration is maintained at 0.18 mol / L to complete the nucleation task;
[0079] S3: After completing the nucleation task, the process is switched to a growth process, the pH value of the reactor is gradually reduced to 10.60, the ammonium concentration is increased to 0.36 mol / L, the reaction temperature is increased to 49°C, the speed is adjusted to 500 r / min, and the solid-liquid ratio of the system is controlled to be 300 g / L or above during the process, and the reaction is continued until the D50 particle size of the product reaches 4.0 μm;
[0080] S4: The slurry product is pumped into the aging tank through the discharge port, and the sodium nickel-manganese binary precursor (Ni 0.50 Mn 0.50 (OH) 2 ), and its scanning electron microscope image is shown in Figure 2 As shown in the figure, it can be seen that it has a relatively dense particle morphology, good sphericity, and a relatively high tap density (1.75g / cm 3 ).
[0081] Example 2
[0082] A method for preparing a high-tap layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0083] S1: pure water was added to the reactor and heated to 45°C, and nitrogen was introduced at a flow rate of 30 L / h, and then an ammonia solution was added to adjust the ammonium concentration of the bottom liquid to 0.20 mol / L, and then a sodium hydroxide solution was added to adjust the pH value of the bottom liquid to 12.20, and the stirring blade inside the reactor was stirred at a speed of 700 r / min to mix the bottom liquid uniformly to obtain the bottom liquid of the coprecipitation reaction;
[0084] S2: 2.0 mol / L nickel-iron-manganese mixed salt solution, 11.0 mol / L sodium hydroxide solution, and 7.5 mol / L ammonia solution are simultaneously pumped into the above reactor, and the molar ratio of nickel-iron-manganese is controlled to be 25:35:40. The reaction is carried out for 1 hour under the conditions that the pH value in the reactor is maintained at 12.20 and the ammonium concentration is maintained at 0.20 mol / L to complete the nucleation task;
[0085] S3: After completing the nucleation task, the process is switched to a growth process, the pH value of the reactor is gradually reduced to 10.90, the ammonium concentration is increased to 0.30 mol / L, the reaction temperature is increased to 55°C, the speed is adjusted to 600 r / min, and the solid-liquid ratio of the system is controlled to be 400 g / L or above during the process, and the reaction is continued until the D50 particle size of the product reaches 4.0 μm;
[0086] S4: The slurry product is pumped into an aging tank through a discharge port, and then aged, centrifuged, dried, screened, demagnetized and packaged to obtain a sodium-electro-nickel-iron-manganese ternary precursor (Ni 0.25 Fe 0.35 Mn 0.40 (OH) 2 ), and its scanning electron microscope image is shown in Figure 3 As shown in the figure, it can be seen that it has a relatively dense particle morphology, good sphericity, and a relatively high tap density (1.77 g / cm 3 ).
[0087] Example 3
[0088] A method for preparing a high-tap layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0089] S1: pure water was added to the reactor and heated to 50°C, and nitrogen was introduced at a flow rate of 30L / h, and then an ammonia solution was added to adjust the ammonium concentration of the bottom liquid to 0.10mol / L, and then a sodium hydroxide solution was added to adjust the pH value of the bottom liquid to 12.20, and the stirring blade inside the reactor was stirred at a speed of 700r / min to mix the bottom liquid evenly to obtain the bottom liquid of the coprecipitation reaction;
[0090] S2: Pump 2.0 mol / L nickel-iron-manganese-zinc mixed salt solution, 11.0 mol / L sodium hydroxide solution, and 7.5 mol / L ammonia solution into the above reactor at the same time, control the molar ratio of nickel-iron-manganese-zinc to be 23.2:31.8:37.3:7.8, and react for 1 hour under the conditions of maintaining the pH value at 12.20 and the ammonium concentration at 0.10 mol / L in the reactor to complete the nucleation task;
[0091] S3: After completing the nucleation task, the process is switched to a growth process, the pH value of the reactor is gradually reduced to 11.20, the ammonium concentration is increased to 0.20 mol / L, the reaction temperature is increased to 70°C, the speed is adjusted to 600 r / min, and the solid-liquid ratio of the system is controlled to be 500 g / L or above during the process, and the reaction is continued until the D50 particle size of the product reaches 4.0 μm;
[0092] S4: The slurry product is pumped into an aging tank through a discharge port, and then aged, centrifuged, dried, screened, demagnetized and packaged to obtain a sodium-electro-nickel-iron-manganese-zinc quaternary precursor (Ni 0.232 Fe 0.318 Mn 0.373 Zn 0.078 (OH) 2 ), and its scanning electron microscope image is shown in Figure 4 As shown in the figure, it can be seen that it has a relatively dense particle morphology, good sphericity, and a relatively high tap density (1.43g / cm 3 ).
[0093] Example 4
[0094] A method for preparing a high-tap layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0095] S1: pure water was added to the reactor and heated to 40°C, and nitrogen was introduced at a flow rate of 30 L / h, and then oxalic acid solution was added to adjust the oxalate concentration of the bottom liquid to 0.10 mol / L, and then sodium hydroxide solution was added to adjust the pH value of the bottom liquid to 11.80, and the stirring blade inside the reactor was stirred at a speed of 700 r / min to mix the bottom liquid evenly to obtain the bottom liquid of the coprecipitation reaction;
[0096] S2: Pump 2.0 mol / L nickel-iron-manganese-zinc mixed salt solution, 11.0 mol / L sodium hydroxide solution, and 1.5 mol / L oxalic acid solution into the above reactor at the same time, control the molar ratio of nickel-iron-manganese-zinc to be 23.2:31.8:37.3:7.8, and react for 0.5 hour under the condition that the pH value in the reactor is maintained at 11.80 and the oxalate concentration is maintained at 0.10 mol / L to complete the nucleation task;
[0097] S3: After completing the nucleation task, the process is switched to a growth process, the pH value of the reactor is gradually reduced to 11.30, the oxalate concentration is increased to 0.20 mol / L, the reaction temperature is increased to 60°C, the speed is adjusted to 600 r / min, and the solid-liquid ratio of the system is controlled to be 400 g / L or above during the process, and the reaction is continued until the D50 particle size of the product reaches 10.0 μm;
[0098] S4: The slurry product is pumped into the aging tank through the discharge port, and the sodium-electro-nickel-iron-manganese-zinc quaternary precursor (Ni 0.232 Fe 0.318 Mn 0.373 Zn 0.078 (OH) 2 ), and its scanning electron microscope image is shown in Figure 5 As shown in the figure, it can be seen that it has a relatively dense particle morphology, good sphericity, and a relatively high tap density (2.05g / cm 3 ).
[0099] Example 5
[0100] A method for preparing a high-tap layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0101] S1: pure water was added to the reactor and heated to 40°C, and nitrogen was introduced at a flow rate of 30 L / h, and then oxalic acid solution was added to adjust the oxalate concentration of the bottom liquid to 0.10 mol / L, and then sodium hydroxide solution was added to adjust the pH value of the bottom liquid to 11.60, and the stirring blade inside the reactor was stirred at a speed of 700 r / min to mix the bottom liquid evenly to obtain the bottom liquid of the coprecipitation reaction;
[0102] S2: Pump 2.0 mol / L nickel-iron-manganese-copper mixed salt solution, 11.0 mol / L sodium hydroxide solution, and 1.5 mol / L oxalic acid solution into the above reactor at the same time, control the molar ratio of nickel-iron-manganese-copper to be 22:22:43.8:12.2, and react for 0.5 hour under the conditions of maintaining the pH value at 11.60 and the oxalate concentration at 0.10 mol / L in the reactor to complete the nucleation task;
[0103] S3: After completing the nucleation task, the process is switched to a growth process, the pH value of the reactor is gradually reduced to 11.30, the oxalate concentration is increased to 0.40 mol / L, the reaction temperature is increased to 60°C, the speed is adjusted to 600 r / min, and the solid-liquid ratio of the system is controlled to be 500 g / L or above during the process, and the reaction is continued until the D50 particle size of the product reaches 10.0 μm;
[0104] S4: The slurry product is pumped into an aging tank through a discharge port, and then aged, centrifuged, dried, screened, iron removed and packaged to obtain a sodium-electro-nickel-iron-manganese-copper quaternary precursor (Ni 0.220 Fe 0.220 Mn 0.438 Cu 0.122 (OH) 2 ), and its scanning electron microscope image is shown in Figure 6 As shown in the figure, it can be seen that it has a relatively dense particle morphology, good sphericity, and a relatively high tap density (1.33 g / cm 3 ).
[0105] Comparative Example 1
[0106] A method for preparing a layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0107] S1: pure water was added to the reactor and heated to 35°C, and nitrogen was introduced at a flow rate of 30 L / h, and then an ammonia solution was added to adjust the ammonium concentration of the bottom liquid to 0.18 mol / L, and then a sodium hydroxide solution was added to adjust the pH value of the bottom liquid to 12.10, and the stirring blade inside the reactor was stirred at a speed of 500 r / min to mix the bottom liquid evenly to obtain the bottom liquid for the coprecipitation reaction;
[0108] S2: 2.0 mol / L nickel-manganese mixed salt solution, 11.0 mol / L sodium hydroxide solution, and 7.5 mol / L ammonia solution are simultaneously pumped into the above reactor, and the molar ratio of nickel and manganese is controlled to be 50:50. The reaction is carried out for 1 hour under the conditions that the pH value in the reactor is maintained at 12.10 and the ammonium concentration is maintained at 0.18 mol / L to complete the nucleation task;
[0109] S3: After completing the nucleation task, the process is switched to a growth process, the pH value of the reactor is gradually reduced to 10.60, the ammonium concentration is increased to 0.36 mol / L, the reaction temperature is increased to 49°C, the speed is adjusted to 400 r / min, the solid-liquid ratio of the system is 200 g / L or less, and the reaction is continued until the D50 particle size of the product reaches 4.0 μm;
[0110] S4: The slurry product is pumped into the aging tank through the discharge port, and the sodium nickel-manganese binary precursor (Ni 0.50Mn 0.50 (OH) 2 ), and its scanning electron microscope image is shown in Figure 7 As shown in the figure, it can be seen that it has a relatively loose particle morphology, relatively poor sphericity, and a relatively low tap density (0.79 g / cm 3 ).
[0111] Comparative Example 2
[0112] A method for preparing a layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0113] S1: pure water was added to the reactor and heated to 45°C, and nitrogen was introduced at a flow rate of 30 L / h, and then an ammonia solution was added to adjust the ammonium concentration of the bottom liquid to 0.20 mol / L, and then a sodium hydroxide solution was added to adjust the pH value of the bottom liquid to 12.10, and the stirring blade inside the reactor was stirred at a speed of 500 r / min to mix the bottom liquid evenly to obtain the bottom liquid for the coprecipitation reaction;
[0114] S2: 2.0 mol / L nickel-iron-manganese mixed salt solution, 11.0 mol / L sodium hydroxide solution, and 7.5 mol / L ammonia solution are simultaneously pumped into the above reactor, and the molar ratio of nickel-iron-manganese is controlled to be 25:35:40. The reaction is carried out for 1 hour under the conditions that the pH value in the reactor is maintained at 12.10 and the ammonium concentration is maintained at 0.20 mol / L to complete the nucleation task;
[0115] S3: After completing the nucleation task, the process is switched to a growth process, the pH value of the reactor is gradually reduced to 10.90, the ammonium concentration is increased to 0.30 mol / L, the reaction temperature is increased to 55°C, the speed is adjusted to 400 r / min, the solid-liquid ratio of the system is 200 g / L or less, and the reaction is continued until the D50 particle size of the product reaches 4.0 μm;
[0116] S4: The slurry product is pumped into an aging tank through a discharge port, and then aged, centrifuged, dried, screened, demagnetized and packaged to obtain a sodium-electro-nickel-iron-manganese ternary precursor (Ni 0.25 Fe 0.35 Mn 0.40 (OH) 2 ), and its scanning electron microscope image is shown in Figure 8 As shown in the figure, it can be seen that it has a relatively loose particle morphology, relatively poor sphericity, and a relatively low tap density (1.13 g / cm 3 ).
[0117] Comparative Example 3
[0118] A method for preparing a layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0119] S1: pure water was added to the reactor and heated to 50°C, and nitrogen was introduced at a flow rate of 30L / h, and then an ammonia solution was added to adjust the ammonium concentration of the bottom liquid to 0.10mol / L, and then a sodium hydroxide solution was added to adjust the pH value of the bottom liquid to 12.10, and the stirring blade inside the reactor was stirred at a speed of 500r / min to mix the bottom liquid evenly to obtain the bottom liquid of the coprecipitation reaction;
[0120] S2: 2.0 mol / L nickel-iron-manganese-zinc mixed salt solution, 11.0 mol / L sodium hydroxide solution, and 7.5 mol / L ammonia solution are simultaneously pumped into the above reactor, and the molar ratio of nickel-iron-manganese-zinc is controlled to be 23.2:31.8:37.3:7.8. The reaction is carried out for 1 hour under the conditions that the pH value in the reactor is maintained at 12.10 and the ammonium radical concentration is maintained at 0.10 mol / L to complete the nucleation task;
[0121] S3: After completing the nucleation task, the process is switched to a growth process, the pH value of the reactor is gradually reduced to 11.20, the ammonium concentration is increased to 0.20 mol / L, the reaction temperature is increased to 70°C, the speed is adjusted to 400 r / min, the solid-liquid ratio of the system is 200 g / L or less, and the reaction is continued until the D50 particle size of the product reaches 4.0 μm;
[0122] S4: The slurry product is pumped into an aging tank through a discharge port, and then aged, centrifuged, dried, screened, demagnetized and packaged to obtain a sodium-electro-nickel-iron-manganese-zinc quaternary precursor (Ni 0.232 Fe 0.318 Mn 0.373 Zn 0.078 (OH) 2 ), and its scanning electron microscope image is shown in Fig. 9 As shown in the figure, it can be seen that it has a relatively loose particle morphology, relatively poor sphericity, and a relatively low tap density (0.85g / cm 3 ).
[0123] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a high-tap layered oxide positive electrode material precursor for a sodium ion battery, characterized in that: The steps include: Passing a mixed metal salt solution, a precipitant and a complexing agent into a reactor in which a base liquid has been adjusted to perform a co-precipitation reaction, controlling the concentration of the mixed metal salt solution to be ≤2.0 mol / L, the concentration of the precipitant to be ≤11.0 mol / L, and the concentration of the complexing agent to be ≤10.0 mol / L, and coordinating and controlling the process parameters such as the rotation speed, solid-liquid ratio, pH and complexing agent concentration, continuously passing an inert gas during the reaction, and continuing the reaction until the particle size of the product reaches the target particle size; In the granulation stage, the pH value in the reaction kettle is controlled to be a first pH value, the complexing agent value is a first complexing agent concentration value, and the rotation speed value is a first rotation speed value; in the growth stage, the pH value in the reaction kettle is controlled to be a second pH value, the complexing agent value is a second complexing agent concentration value, and the rotation speed value is a second rotation speed value; Wherein, 12.50>first pH value>second pH value>9.50, 0.01mol / L≤first complexing agent concentration value<second complexing agent concentration value≤1.0mol / L, 800r / min≥first speed value>second speed value≥300r / min; The solid-liquid ratio in the coprecipitation process is 300 g / L or above.
2. The preparation method according to claim 1, characterized in that: The chemical composition of the positive electrode material precursor is as follows: Ni x TM 1-x (OH)2, 0<x<1, TM is a metal ion; Wherein, TM is selected from one or more of Fe, Mn, Cu and Zn.
3. The preparation method according to claim 2, characterized in that: The preparation method comprises the following steps: (a) According to the chemical composition of the positive electrode material precursor, metal salts are mixed to obtain a mixed metal salt solution: (b) The mixed metal salt solution of step (a) is first subjected to a nucleation reaction in the presence of a complexing agent and a precipitant, and then subjected to a growth reaction until the D50 particle size of the product reaches a target particle size, and the product is sequentially aged, centrifuged, dried, sieved, demagnetized and packaged to obtain a sodium cathode material precursor.
4. The preparation method according to claim 3, characterized in that: The particle size D50 of the sodium positive electrode material precursor is 3.0-15.0 um.
5. The preparation method according to claim 3, characterized in that: The precipitant is sodium hydroxide or potassium hydroxide; Preferably, the complexing agent is ammonia water or oxalic acid solution; Preferably, the reaction temperature is 30-70°C; Preferably, the reaction speed is 300-800r / min; Preferably, the inert gas is nitrogen or argon.
6. The preparation method according to claim 5, characterized in that: The precipitant is sodium hydroxide, the complexing agent is ammonia water or oxalic acid solution, and the inert gas is nitrogen.
7. A sodium ion battery layered oxide positive electrode material precursor, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 6.
8. The sodium ion battery layered oxide positive electrode material precursor according to claim 7, characterized in that: The tap density of the positive electrode material precursor is 1.30-2.20 g / cm 3 .
9. A sodium ion battery positive electrode material, characterized in that: The positive electrode material precursor according to claim 8 is prepared, and the preparation method comprises the following steps: the sodium positive electrode material precursor is uniformly mixed with a sodium source, and then calcined at a high temperature to obtain a sodium layered oxide positive electrode material Na(Ni x TM 1-x )O2(0<x<1).
10. A sodium ion battery, characterized in that: The positive electrode of the sodium ion battery comprises the positive electrode material according to claim 9.
Citation Information
Patent Citations
Nickel-iron-manganese ternary precursor, preparation method and sodium ion battery positive electrode material
CN116239161A
Sodium-ion battery positive electrode precursor as well as preparation method and application thereof
CN118005098A
Cited By
Quaternary sodium electric precursor, preparation method thereof and sodium ion battery
CN121627080A