Organic silicon artificial leather for electronic products and manufacturing process
By designing functional layers and wear-resistant layers in polycarbonate materials, using materials such as diimine methyl silicone oil and MQ resin, the firm connection between the silicone rubber leather layer and the PC substrate layer is achieved, and the lack of adhesion is solved The problem is that the mechanical properties and wear resistance of electronic products are improved, the manufacturing process is simplified and the cost is reduced.
Patent Information
- Application Number
- CN202411023192.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-26
AI Technical Summary
In the prior art, the combination of polycarbonate material and silicone artificial leather has insufficient adhesion, resulting in low peel strength between the silicone rubber and the PC substrate layer and inability to form effective adsorption, which limits its application in electronic product shells.
Using PC substrate layer instead of the traditional base cloth substrate layer, through the design of the formula of functional layer and wear-resistant layer, and using materials such as diimine methyl silicone oil, MQ resin and peroxide vulcanizer to form chemical bonds and transition zones. , good bonding between the silicone rubber leather layer and the PC substrate layer is achieved without using adhesive.
The firm connection between the silicone rubber leather layer and the PC substrate layer is achieved, the mechanical properties and wear resistance of silicone artificial leather for electronic products is improved, the durability of use is enhanced, the manufacturing process is simplified, and the production cost is reduced.
Smart Images

Figure CN119019731A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of organosilicon artificial leather, in particular to organosilicon artificial leather for electronic products and a manufacturing process thereof. Background Art
[0002] As consumers' requirements for the appearance and touch of electronic products increase, leather products are increasingly used in electronic product design. Electronic products such as mobile phone back covers, tablet back covers, laptop back covers, refrigerator shells, air conditioner shells, Bluetooth speaker shells, etc. all have records of using leather on the surface of the shell.
[0003] For electronic products that need to be touched frequently, such as mobile phones and Bluetooth speakers, leather has a soft, delicate and smooth touch, which can provide a more comfortable hand-feeling experience than traditional metal or plastic materials. For the surfaces of products such as refrigerators and air conditioners, leather, as a high-end material, has a unique texture and luster, which can significantly enhance the overall texture of electronic products. In addition, although leather itself is not as hard as metal or plastic, it has good wear resistance and scratch resistance, which can protect electronic products to a certain extent and increase the durability of electronic products.
[0004] The invention patent with Chinese patent number ZL202110366061.X discloses a production process for a color-changing and anti-fouling mobile phone back cover. The process first forms a leather layer, and then covers the leather layer on a release film through an adhesive layer. During subsequent processing, the leather layer is first cut according to the size of the mobile phone back cover, and then the release film is peeled off, and the side of the leather layer with the adhesive layer is attached to the back cover of the mobile phone to obtain the final product.
[0005] The invention patent with Chinese application number 202010985778.8 discloses a carbon fiber and glass fiber mobile phone back cover molding process and a mobile phone back cover. The process first assembles the glass fiber and carbon fiber with a leather layer to obtain a semi-finished product, then cuts it to the same size as the mobile phone back cover, and then hot presses and bonds it to obtain the mobile phone back cover.
[0006] The invention patent with Chinese application number 202211237687.1 discloses a leather back cover and its preparation method, including a substrate layer, a reinforcement layer arranged on the surface of the substrate layer, and a silicone leather layer arranged on the surface of the reinforcement layer. The substrate layer is selected from a PC board or a PMMA / PC composite board, and the reinforcement layer is selected from one of glass fiber, carbon fiber, aramid fiber or glass fiber / carbon fiber composite material. The silicone leather layer includes a skin layer, an intermediate layer and an adhesive layer. The manufacturing process of the mobile phone back cover is to first bond and fix the silicone leather layer to the reinforcement layer, then bond the reinforcement layer to the substrate layer through UV glue, and finally obtain the product through high pressure molding and CNC processing.
[0007] The invention patent with Chinese patent number ZL202210654303.X discloses an ultra-thin backplane, including a silicone layer, a reinforcement layer and a polycarbonate layer. The reinforcement layer is a product of melt-extruded modified polycarbonate, reinforcing fiber, porous glass fiber and KH570, and mainly serves as a connecting layer between the silicone layer and the polycarbonate layer.
[0008] The above-mentioned patented products have room for improvement in technical aspects such as reducing thickness and improving processing efficiency. Summary of the invention
[0009] The first invention purpose of the present application is to provide a silicone artificial leather for electronic products. The silicone artificial leather is different from other leather products on the market. It at least adds an option when making leather shells for electronic products, brings a comfortable touch or appearance to the electronic products, and increases the durability of the electronic products.
[0010] To achieve the above-mentioned invention purpose, the present application adopts the following technical scheme: an organic silicone artificial leather for electronic products, comprising a PC substrate layer and a silicone rubber leather layer, the silicone rubber leather layer comprising a wear-resistant layer and a functional layer, the functional layer is attached to the PC substrate layer, the thickness of the functional layer is 0.1 to 0.25 mm, and the functional layer is made of the following materials: 100 parts of terminal vinyl dimethyl silicone oil; 20-30 parts of diiminomethyl silicone oil; 10-15 parts of MQ resin containing 1-5% silanol; Peroxide curing agent 0.1 to 0.5 parts.
[0011] Among them, the structural formula of diiminomethyl silicone oil is: ; Wherein, the ratio of M unit / Q unit of the MQ resin is 0.6-0.9.
[0012] In the above technical solution, the PC substrate layer is a polycarbonate material, whose mechanical and electrical properties are widely recognized, and has the characteristics of high strength, high transparency, impact resistance, high and low temperature resistance, etc. It is often used as a shell material for electronic products. The PC substrate layer is selected in this application so that the products of this application can be widely used in a variety of different electronic products. Silicone artificial leather is a material made of silicone rubber with good dielectric properties, environmental protection, green and good touch and appearance. In recent years, it has also been increasingly used in the field of electronic products. The silicone rubber leather layer selected in this application can make full use of the characteristics of silicone rubber and bring a good experience to consumers.
[0013] However, in the general understanding of those skilled in the art, if polycarbonate materials and silicone artificial leather are to be used together, the silicone artificial leather with a base fabric substrate layer is generally bonded to the polycarbonate film through an adhesive to form a composite material for reuse. Patent No. 202010985778.8 and Patent No. 202211237687.1 mentioned in the background technology are examples of such use. Even if the silicone artificial leather does not have a base fabric substrate layer, an adhesive or other material should be used to bond the silicone rubber leather layer and the PC substrate layer to obtain a composite material for use. Patent No. ZL202210654303.X is such an example. Those skilled in the art would not think of using polycarbonate material, i.e., PC substrate layer, to replace the base fabric substrate layer to form a new silicone rubber synthetic leather for use. This is because the adhesion between the heat-vulcanized silicone rubber and the PC substrate is far from meeting the requirements. Generally, the peel strength between the silicone rubber layer and the PC substrate layer is less than 10N / 15mm. Therefore, it can be considered that there will be no effective adsorption between silicone rubber and polycarbonate, while silicone rubber can form effective adsorption with the base fabric substrate layer with warp and weft interlaced. Generally, silicone rubber cannot be effectively peeled off from the base fabric substrate layer. The smooth surface of the PC substrate will not form physical adsorption dominated by van der Waals force with the vulcanized silicone rubber, nor will it form chemical adsorption dominated by chemical bond force and hydrogen bond force with the vulcanized silicone rubber. In addition, both silicone rubber and polycarbonate have non-polar characteristics and cannot form dispersion force. Those skilled in the art would not think of using polycarbonate to replace the base fabric as the substrate of silicone rubber synthetic leather, let alone directly making such silicone rubber synthetic leather into the shell of electronic products.
[0014] The silicone rubber leather layer of the present application is divided into a functional layer and a wear-resistant layer. The silicone rubber material of the functional layer is specially designed to form a good bond with the PC substrate layer. The imino group is introduced into the molecular weight of the silicone rubber, which can bond with the carbonyl group in the polycarbonate. "A nucleophilic reaction occurs to form" "Structure chemical bond, even if such a chemical bond cannot be completely formed, the tendency of the lone pair of electrons in the imino group to form a coordination bond with the carbonyl carbon can also make the bonding viscosity between the functional layer and the PC substrate layer higher, and the thickness is controlled within the overall thickness of the functional layer of 0.1 to 0.25 mm. The interface between the surface of the PC substrate layer and the functional layer will disappear, forming a transition zone, and finally achieving good bonding between the silicone rubber leather layer and the PC substrate layer without using an adhesive. It should be noted that if the thickness of the functional layer is designed to be too thin, it will not be easy to form a transition zone, and if the thickness of the functional layer is designed to be too thick, it will be difficult for the functional layer to be cured and formed.
[0015] In addition, the functional layer formula of the present application contains MQ resin with 1-5% silanol, and the ratio of M unit / Q unit is 0.6-0.9. This MQ resin can play a role in viscosity enhancement, improve the bonding strength between the silicone rubber leather layer and the PC substrate layer, and reduce the delamination phenomenon of the final product. In addition, the functional layer formula of the present application uses terminal vinyl dimethyl silicone oil as the main material of silicone rubber, and the peroxide vulcanizer is used as the curing agent in the functional layer formula, so that the silicone rubber material is effectively cured and formed. The peroxide vulcanizer can be selected from di(2,4-dichlorobenzoyl) peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, dibenzoyl peroxide or diisopropylbenzene peroxide.
[0016] Furthermore, the thickness of the PC substrate layer of the present application is 0.2-0.6 mm, and the thickness of the wear-resistant layer is 0.15-0.25 mm.
[0017] By adopting the above technical solution, the PC substrate layer with a thickness in the range of 0.2 to 0.6 mm can meet the use requirements of most types of electronic products, and the wear-resistant layer with a thickness of 0.15 to 0.25 mm can provide sufficient wear resistance for the leather and is easy to coat and process.
[0018] Furthermore, the wear-resistant layer is made of the following materials: 100 parts of vinyl silicone oil; 10-20 parts of hydrogen silicone oil; 10-30 parts of white carbon black; 0.1 to 0.5 parts of platinum catalyst.
[0019] In the above technical scheme, vinyl silicone oil is the main raw material of the wear-resistant layer silicone rubber, hydrogen-containing silicone oil can undergo addition reaction with vinyl silicone oil to increase the strength of the material after molding, and white carbon black, as a filler of the wear-resistant layer silicone rubber, also plays a role in increasing the strength of the material after molding. The platinum catalyst is a curing agent in the formula, which can promote the addition reaction of hydrogen-containing silicone oil and terminal vinyl dimethyl silicone oil.
[0020] Furthermore, the diiminomethyl silicone oil is prepared by hydrolyzing methyl hydrogen silicon dichloride and dimethyldiethoxysilane and then reacting with hexamethyldisiloxane.
[0021] In the above technical solution, dichloromethyl hydrogen silicon and dimethyl diethoxy silane are used as monomers of diimino methyl silicone oil, and hexamethyl disiloxane is prepared as a capping agent of diimino methyl silicone oil. In addition, the hydrolyzate of dichloromethyl hydrogen silicon and dimethyl diethoxy silane is used for preparation, mainly to avoid equipment corrosion caused by direct synthesis using dichloromethyl hydrogen silicon and dimethyl dichloro silane. This reaction has high requirements on the purity of dichloromethyl hydrogen silicon and dimethyl dichloro silane. Even if there are 100 micrograms per kilogram of impurities, it will affect the performance of the final product.
[0022] Furthermore, the preparation method of the diiminomethyl silicone oil comprises the following steps: Step 1: Mixing: Mixing methylsilane dichloride and dimethyldiethoxysilane in a mass ratio of 1.15:1 to obtain a mixture A; Step 2, hydrolysis of mixture A: add 1 / 3 of the total volume of 30wt% ammonia solution to the reactor, add mixture A dropwise under stirring at 20r / min, stop adding mixture A when the liquid level reaches 1 / 2 of the total volume, control the dropping time to 2h to 3h, control the temperature in the reactor not to exceed 60°C, and control the air pressure not to exceed 1.1 times the standard atmospheric pressure; after the dropwise addition is completed, add water so that the liquid in the reactor occupies 2 / 3 of the total volume, continue stirring for 20min, and then let stand for 20min, the resulting lower organic phase is the hydrolysis product B; Step 3, synthesis of diiminomethyl silicone oil; the hydrolyzate B, D4, MD2M and alkali glue are put into the reactor in a nitrogen atmosphere in sequence, and the vacuum pump is turned on after the materials are put in, the vacuum degree is -0.06 to -0.08Mpa, the reaction temperature is controlled at 80 to 90°C, the reaction is terminated after 10 hours of reaction, the vacuum pump is turned off, the temperature is raised to 180°C and maintained for 1 hour, and then maintained at 0.133kpa and 300°C for 30 minutes, and the diiminomethyl silicone oil is obtained after cooling.
[0023] In the above technical scheme, the mixing step of step one controls the mass ratio of dichloromethylsilane and dimethyldiethoxysilane to 1.15:1, mainly to ensure that the content of the imine group in the final product is appropriate, and compared with hydrolyzing dichloromethylsilane and dimethyldiethoxysilane separately and then mixing them, pre-mixing and hydrolysis can save the use of the reactor in the factory without affecting the reaction effect of the final synthesis step. The 30wt% ammonia solution in step two provides an alkaline hydrolysis environment in the entire reactor, which helps to neutralize the hydrochloric acid produced by the hydrolysis reaction, making the hydrolysis process more thorough. Adding mixture A dropwise to the ammonia solution can ensure that water is in an excessive state during the entire reaction process, and as the amount of mixture A added increases, water will be generated in the reactor due to the polymerization reaction. As long as the final liquid level of the added mixture A is controlled, the mixture A can be completely hydrolyzed. During the whole process of step 2, there will be an exothermic phenomenon, which will also cause the pressure in the reactor to increase. Although these phenomena are conducive to the hydrolysis reaction, they should also be controlled to a certain extent. The temperature control does not exceed 60°C and the pressure does not exceed 1.1 times the standard atmospheric pressure to avoid boiling in the reactor and reduce the loss of the reactor. In step 2, further adding water after the dropwise addition is to extract the inorganic matter in the organic phase. In step 3, D4 is the abbreviation of octamethylcyclotetrasiloxane and MD2M is the abbreviation of decamethyltetrasiloxane. These two substances mainly play the role of increasing the chain length and can also play the role of end-capping agent. Alkali glue, as a catalyst, can promote the polymerization of various substances in the reactor. Such a reaction can not only obtain the final product, but also control the content of imine groups in the final product by adjusting the addition amount of D4 and MD2M. Turn off the vacuum pump, raise the temperature to 180°C and maintain it for 1h to decompose the alkali glue. Then maintain it at 0.133kpa and 300°C for 30min to fully volatilize the small molecules that do not participate in the polymerization reaction.
[0024] Furthermore, the mass of each material involved in step 3 of the preparation method of diiminomethyl silicone oil is divided into: 100 parts of hydrolyzate B; D4 10-20 portions; MD2M 10-20 copies; 0.01-0.02 parts of alkali glue.
[0025] By adopting the above technical scheme, the final product diiminomethyl silicone oil has a moderate content of imino groups and its performance can meet the requirements.
[0026] Furthermore, the functional layer formula also includes 10 to 20 parts of white carbon black.
[0027] By adopting the above technical solution, the mechanical properties of the functional layer can be increased, thereby achieving an increase in the overall mechanical properties of the organosilicon artificial leather for electronic products.
[0028] Furthermore, the wear-resistant layer also includes 5 to 20 parts of color paste.
[0029] By adopting the above technical solution, the color paste can give the final silicone artificial leather for electronic products a variety of colors.
[0030] Furthermore, the silicone rubber leather layer also includes a surface treatment layer, and the surface treatment layer is coated on a side of the wear-resistant layer away from the functional layer.
[0031] By adopting the above technical solution, the surface treatment layer can improve the touch of the silicone artificial leather for electronic products and obtain a better sensory experience.
[0032] The second invention object of the present application is to provide a manufacturing process for silicone artificial leather for electronic products, which has the advantages of simple operation and high production efficiency. The obtained silicone artificial leather can be processed in various forms such as hot pressing, high pressure forming and punching in subsequent stages, thereby saving the cost of the entire process chain.
[0033] The above-mentioned invention object of the present application is achieved through the following technical scheme: a manufacturing process of silicone artificial leather for electronic products, using a polycarbonate film in the form of a roll as the PC substrate layer, and sequentially coating each layer of the silicone rubber leather layer on the surface of the PC substrate layer through a dry coating machine and curing and forming, and then winding it in the form of a roll to obtain the silicone artificial leather for electronic products.
[0034] In the above technical solution, since the PC substrate layer is in the form of a roll, it is convenient for upstream manufacturers to process it by cast extrusion or calendering extrusion. Since the finished product is rolled up in the form of a roll, it is convenient for downstream manufacturers to directly cut and use it. Compared with the existing technology, downstream manufacturers reduce the process of bonding leather and cloth, reduce production costs, and improve processing efficiency.
[0035] In summary, the invention of this application has at least the following beneficial effects: 1. The silicone artificial leather for electronic products obtained in the present application can bring a comfortable touch or look to the electronic products, increase the durability of the electronic products, and use a PC substrate layer instead of a base fabric substrate layer, which can not only make the overall design thinner, but also facilitate the subsequent processing into an electronic product housing.
[0036] 2. The silicone artificial leather for electronic products obtained in the present application has a PC substrate layer and a silicone rubber leather layer that are firmly connected, and meets the requirements of the silicone artificial leather for bonding the substrate and the leather layer without using an adhesive.
[0037] 3. The manufacturing process of the silicone artificial leather for electronic products of the present application has the advantages of simple operation and high production efficiency. The obtained silicone artificial leather can be processed in various forms such as hot pressing, high pressure forming and punching in subsequent stages, saving the cost of the entire process chain. DETAILED DESCRIPTION
[0038] The present application is described in further detail below.
[0039] Preparation Examples 1 to 10 Preparation Examples 1 to 10 are functional layer silicone rubber bases, and each preparation example is prepared by stirring according to the proportions of ingredients in Table 1.
[0040] Table 1 Ingredients of Preparation Examples 1 to 10
[0041] It should be noted that after the functional layer silicone rubber base is prepared, it needs to be processed and used in the next stage within 2 hours, otherwise the peroxide curing agent will cause the functional layer silicone rubber base to solidify and eventually become unusable. Among them, the terminal vinyl dimethyl silicone oil in the table was purchased from Dongguan Jingbo New Materials Co., Ltd., with a viscosity of 3000 centipoise. The peroxide curing agent in the table was purchased from diisopropylbenzene peroxide produced by Dongguan Yongzheng Chemical, with a brand name of LUPEROX DC. The MQ resin in the table uses the JSYA-MQ1002 product of Qianhai Jishengya Technology Co., Ltd., which has a hydroxyl content of 4-5% and an M:Q value of 0.60-0.80. White carbon black was purchased from Shandong Delan Chemical Co., Ltd. Fumed white carbon black DL-A200. In addition, although the selection of each material in the above preparation example is specifically disclosed, purchasing similar materials on the market can also achieve the invention purpose of this application, so different technical solutions generated only by different material purchases also fall within the scope of protection of this application.
[0042] The diiminomethyl silicone oils of Preparation Examples 1 to 10 were prepared from the same batch. The specific preparation process of the batch is as follows: Step 1: Mixing: Mixing methylsilane dichloride and dimethyldiethoxysilane in a mass ratio of 1.15:1 to obtain a mixture A; Step 2, hydrolysis of mixture A: add 1 / 3 of the total volume of 30wt% ammonia solution to the reactor, add mixture A dropwise under stirring at 20r / min, stop adding mixture A when the liquid level reaches 1 / 2 of the total volume, control the addition time to 3h, control the temperature in the reactor to 55°C, and control the air pressure to not exceed 1.1 times the standard atmospheric pressure; after the addition is completed, add water so that the liquid in the reactor occupies 2 / 3 of the total volume, continue stirring for 20min, and then let stand for 20min, and the resulting lower organic phase is the hydrolysis product B; Step 3, synthesis of diiminomethyl silicone oil; 100 parts of hydrolyzate B, 15 parts of D4, 15 parts of MD2M and 0.01 parts of alkali glue are sequentially put into a reactor under a nitrogen atmosphere. After the materials are put in, the vacuum pump is turned on, the vacuum degree is -0.08Mpa, the reaction temperature is controlled at 90°C, the reaction is terminated after 10 hours of reaction, the vacuum pump is turned off, the temperature is raised to 180°C and maintained for 1 hour, and then maintained at 0.133kpa and 300°C for 30 minutes, and the diiminomethyl silicone oil is obtained after cooling.
[0043] It should be noted that the reaction conditions in the preparation steps of other batches of diiminomethyl silicone oil can be slightly changed. Such simple changes in conditions are technical solutions that can achieve the purpose of the invention of this application and are also technical solutions claimed for protection in this application. The materials used in the preparation steps of this batch of diiminomethyl silicone oil are all derived from commercially available products, and products with a purity higher than 99.99% can be selected.
[0044] Preparation Examples 11 to 15 Preparation Examples 11 to 15 are silicone rubber bases for wear-resistant layers, and each preparation example is prepared by stirring according to the proportions of ingredients in Table 2.
[0045] Table 2 Ingredients of Preparation Examples 11 to 15
[0046] It is also important to note that after the wear-resistant silicone rubber base is prepared, it needs to be processed and used in the next stage within 2 hours, otherwise the platinum catalyst will cause the wear-resistant silicone rubber base to solidify and eventually become unusable. The vinyl silicone oil in the table is purchased from Anhui Mingyi Silicon Industry Co., Ltd., specifically the product with a viscosity of 1000 centipoise, a vinyl content of 0.18-0.26%, and a model of MY 273. The hydrogenated silicone oil in the table is selected from Anhui Mingyi Silicon Industry Co., Ltd., specifically 50-120mm 2 / s, with a hydrogen content of 0.18-0.36%, and a product model of MY 203. The platinum catalyst in the table was purchased from Shenzhen Sicheng Silica Gel Co., Ltd., with a concentration of 1000ppm. White carbon black was purchased from Shandong Delan Chemical Co., Ltd. Fumed white carbon black DL-A200. The color pastes of Preparation Examples 11 to 13 were respectively red, pure black, and pure white pastes produced by Guangdong Shell New Materials Technology Co., Ltd.
[0047] Example 1 An organic silicone artificial leather for electronic products includes a PC substrate layer and a silicone rubber leather layer, wherein the silicone rubber leather layer includes a wear-resistant layer and a functional layer, and the functional layer is attached to the PC substrate layer. In this embodiment, the thickness of the PC substrate layer is 0.4 mm, the thickness of the functional layer is 0.12 mm, and the thickness of the wear-resistant layer is 0.13 mm.
[0048] The functional layer of this embodiment is obtained by coating the functional layer silicone rubber base adhesive of Preparation Example 1 on the PC substrate layer and curing it. The wear-resistant layer of this embodiment is obtained by coating the wear-resistant layer silicone rubber base adhesive of Preparation Example 11 on the functional layer and curing it. Specifically, the manufacturing process of silicone artificial leather for electronic products adopted in this embodiment is as follows: a polycarbonate film in the form of a roll is used as the PC substrate layer, and each layer of the silicone rubber leather layer is sequentially coated on the surface of the PC substrate layer by a dry coating machine and cured to form. The line speed of the dry coating machine is set to 4.5m / s, and the six temperature zones of the tunnel furnace for curing silicone rubber on the dry coating machine are set to 80°C, 90°C, 125°C, 125°C, 120°C, and 120°C, respectively. After passing through the tunnel furnace, the product is rolled up in the form of a roll to obtain silicone artificial leather for electronic products.
[0049] Embodiments 2 to 7 The silicone artificial leather for electronic products, Examples 2 to 7 are substantially the same as Example 1, except that the functional layers of Examples 2 to 7 use the functional layer silicone rubber base of Preparation Examples 2 to 7, respectively.
[0050] Embodiments 8 to 12 The silicone artificial leather for electronic products, Examples 8 to 12 are substantially the same as Example 6, except that the wear-resistant layers of Examples 8 to 12 use the wear-resistant layer silicone rubber bases of Preparation Examples 11 to 15, respectively.
[0051] Example 13 A silicone artificial leather for electronic products, this embodiment is basically the same as embodiment 1, the only difference is that the silicone rubber leather layer of this example also includes a surface treatment layer, the surface treatment layer is coated on the side of the wear-resistant layer away from the functional layer, and the thickness is 0.02mm. Specifically, this embodiment uses the artificial leather feel agent coating agent 8209 produced by Hangzhou Yizhou Textile Auxiliary Co., Ltd. It should be noted that in other embodiments, coating other types of surface treatment agents, or slightly changing the coating thickness, are all technical solutions that can achieve the purpose of the invention of this application, and are also the technical solutions claimed for protection in this application.
[0052] Embodiments 14 to 17 Silicone artificial leather for electronic products, Examples 14 to 17 are basically the same as Example 1, except that the thickness of the functional layer, the wear-resistant layer and the PC substrate layer are different from those of Example 1. The specific differences are shown in Table 3 below.
[0053] Table 3 Thickness of each layer in Examples 17 to 20
[0054] It should be noted that the thickness of the wear-resistant layer, functional layer and PC substrate layer in the above-mentioned embodiment is only used as an example. The specific thickness of each layer can be selected according to actual conditions. The simple change of thickness selection should be considered as a technical solution within the design concept of this application, and should also be considered as the technical solution claimed for protection in this application.
[0055] Comparative Examples 1 to 3 The silicone artificial leather, Comparative Examples 1 to 3 are substantially the same as Example 1, except that Comparative Examples 1 to 3 use the functional layer silicone rubber base of Preparation Examples 8 to 10 to make the functional layer.
[0056] Comparative Example 4 The silicone artificial leather, Comparative Example 4 is substantially the same as Comparative Example 3, except that a sponge with a thickness of 0.2 mm is used in Comparative Example 4 to replace the PC substrate layer.
[0057] Comparative Example 5 The silicone artificial leather, Comparative Example 5 is substantially the same as Comparative Example 3, except that Comparative Example 5 uses a base fabric substrate layer instead of a PC substrate layer.
[0058] Examples 1 to 17 and comparative examples 1 to 5 were subjected to peel force test and 100-grid test. The peel force test standard was YBB00102003-2015, and the 100-grid test standard was GB9286-1998. The results are shown in Table 4 below.
[0059] Table 4 Peel force test and cross-sectional test results of various embodiments and comparative examples
[0060] It can be seen from the above table that the silicone artificial leather for electronic products claimed in the present application has a PC substrate layer and a silicone leather layer that are firmly bonded.
[0061] From the comparison between Comparative Example 3 and Example 1, it can be seen that the functional layer prepared by the MQ resin formula without the addition of diiminomethyl silicone oil and containing 1-5% silanol group has a low adhesion to the PC substrate layer, which is only 5N / 15mm, and it can be considered that it cannot meet the requirements of artificial leather.
[0062] From the comparison among Comparative Example 3, Comparative Example 1 and Example 1, it can be seen that the functional layer prepared by adding only the formula of MQ resin containing 1-5% silanol group has improved adhesion to the PC substrate layer, but it is still at a relatively low level of only 9N / 15mm, which can still be considered to be unable to meet the requirements of artificial leather.
[0063] From the comparison between Comparative Examples 3 and 2 and Example 1, it can be seen that the functional layer prepared by adding only the formula containing diiminomethyl silicone oil has improved adhesion to the PC substrate layer and the adhesion is at a relatively high level, reaching 24N / 15mm. However, there is still a gap between the functional layer prepared by adding both diiminomethyl silicone oil and the formula containing MQ resin containing 1-5% silanol groups in Example 1 and the optimal level has not been achieved.
[0064] From the comparison between Comparative Example 4 and Comparative Example 2, it can be seen that the bonding effect achieved by the technical solution of Comparative Example 2 in which only diiminomethyl silicone oil is added has exceeded the bonding effect between ordinary silicone rubber and the sponge layer.
[0065] From the comparison between Examples 1 to 17 and Comparative Example 1, it can be seen that the technical solution of the present application, which is added with diiminomethyl silicone oil and MQ resin containing 1 to 5% silanol group, has a bonding effect with the PC substrate layer that is similar to the bonding effect between typical silicone rubber and base cloth substrate layers in the prior art. It can be considered that the technical solution of the present application meets the bonding requirements of artificial leather for the leather layer and the substrate layer.
[0066] The technical solutions of Examples 1 to 5 of the present application were tested for surface resistance and volume resistivity in accordance with GBT 1410-2006 "Test method for volume resistivity and surface resistivity of materials", and the dielectric strength tester BDJC-50KV was used to perform a dielectric strength test. The results were integerized and the results obtained are shown in Table 5.
[0067] Table 5 Electrical performance test results of Examples 1 to 5
[0068] It can be seen from the above table that the silicone artificial leather for electronic products obtained by the technical solution of this application has good electrical properties and can meet the electrical performance requirements of most electronic products for the shell. Other embodiments are similar to the solutions of embodiments 1 to 5, and it can be considered that the electrical properties are also similar.
[0069] The technical solutions of Examples 1 to 5 of the present application were tested for wear resistance in accordance with GB / T5478-2008 "Test method for rolling wear of plastics", and for trouser-shaped tear strength in accordance with GB529-1999 "Determination of tear strength of vulcanized rubber or thermoplastic rubber (trouser-shaped, right-angled and crescent-shaped specimens)". The results are shown in Table 6.
[0070] Table 6 Abrasion resistance and trouser tear strength test results of Examples 1 to 5
[0071] It can be seen from the above table that the organosilicon artificial leather for electronic products obtained by the technical solution of the present application has good mechanical properties and can meet the requirements of leather for electronic product shells.
[0072] The above are all preferred embodiments of the present application, and are not intended to limit the protection scope of the present application. Any equivalent changes made based on the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A silicone artificial leather for electronic products, Features: It comprises a PC substrate layer and a silicone rubber leather layer, wherein the silicone rubber leather layer comprises a wear-resistant layer and a functional layer, the functional layer is attached to the PC substrate layer, and the thickness of the functional layer is 0.1 to 0.25 mm; Wherein, the functional layer is made of the following materials: 100 parts of terminal vinyl dimethyl silicone oil; 20-30 parts of diiminomethyl silicone oil; 10-15 parts of MQ resin containing 1-5% silanol; Peroxide curing agent 0.1-0.5 parts; Wherein, the structural formula of the diiminomethyl silicone oil is: ; Wherein, the ratio of M unit / Q unit of the MQ resin is 0.6-0.
9.
2. The silicone artificial leather for electronic products according to claim 1, Features: The thickness of the PC substrate layer is 0.2-0.6 mm, and the thickness of the wear-resistant layer is 0.15-0.25 mm.
3. The silicone artificial leather for electronic products according to claim 1, It is characterized in that The wear-resistant layer is made of the following materials: 100 parts of vinyl silicone oil; 10-20 parts of hydrogen silicone oil; 10-30 parts of white carbon black; 0.1 to 0.5 parts of platinum catalyst.
4. The silicone artificial leather for electronic products according to claim 1, Features: The diiminomethyl silicone oil is prepared by hydrolyzing dichloromethyl hydrogen silicon and dimethyl diethoxy silane with ammonia water and then adding hexamethyl disiloxane.
5. The silicone artificial leather for electronic products according to claim 1 or 4, It is characterized in that The preparation method of the diiminomethyl silicone oil comprises the following steps: Step 1: Mixing: Mixing methylsilane dichloride and dimethyldiethoxysilane in a mass ratio of 1.15:1 to obtain a mixture A; Step 2, hydrolysis of mixture A: add 1 / 3 of the total volume of 30wt% ammonia solution to the reactor, add mixture A dropwise under stirring at 20r / min, stop adding mixture A when the liquid level reaches 1 / 2 of the total volume, control the dropping time to 2h to 3h, control the temperature in the reactor not to exceed 60°C, and control the air pressure not to exceed 1.1 times the standard atmospheric pressure; after the dropwise addition is completed, add water so that the liquid in the reactor occupies 2 / 3 of the total volume, continue stirring for 20min, and then let stand for 20min, the resulting lower organic phase is the hydrolysis product B; Step 3, synthesis of diiminomethyl silicone oil; the ammonia hydrolysis product B and D4, MD2M and alkali glue are put into the reactor in sequence under a nitrogen atmosphere. After the materials are put in, the vacuum pump is turned on, the vacuum degree is -0.06~-0.08Mpa, the reaction temperature is controlled at 80~90℃, the reaction is terminated after 10h, the vacuum pump is turned off, the temperature is raised to 180℃ and maintained for 1h, and then maintained at 0.133kpa and 300℃ for 30min, and the diiminomethyl silicone oil is obtained after cooling.
6. The silicone artificial leather for electronic products according to claim 5, It is characterized in that The mass of each material involved in step 3 of the preparation method of diiminomethyl silicone oil is divided into: 100 parts of hydrolyzate B; D4 10-20 portions; MD2M 10-20 copies; 0.01-0.02 parts of alkali glue.
7. The silicone artificial leather for electronic products according to claim 1, Features: The functional layer formula also includes 10 to 20 parts of white carbon black.
8. The silicone artificial leather for electronic products according to claim 1, Features: The wear-resistant layer also includes 5 to 20 parts of color paste.
9. The silicone artificial leather for electronic products according to claim 1, Features: The silicone rubber leather layer further comprises a surface treatment layer, and the surface treatment layer is coated on a side of the wear-resistant layer away from the functional layer.
10. A process for manufacturing silicone artificial leather for electronic products according to any one of claims 1 to 9, Features: A polycarbonate film in roll form is used as the PC substrate layer, and each layer of the silicone rubber leather layer is coated on the surface of the PC substrate layer in sequence by a dry coating machine and cured and formed, and then wound in roll form to obtain silicone artificial leather for electronic products.