Water electret master batch, melt-blown cloth composition, melt-blown cloth, preparation method of melt-blown cloth and mask
By using water electret masterbatches and polypropylene polymers to prepare meltblown cloth, combined with specific process flow, the problems of poor ventilation effect and short charge residence time of existing meltblown cloth are solved, and high filtration efficiency and Low air resistance meltblown cloth, suitable for protective masks for children and the elderly.
Patent Information
- Application Number
- CN202411293366.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-26
AI Technical Summary
The existing meltblown cloth has poor ventilation when wearing masks, resulting in difficulty in breathing, especially among children and the elderly. The charge residence time of the electrostatic treated fibers of corona electret is short and the adsorption capacity is low.
Water electret masterbatches, including 60 to 80 parts by weight of polypropylene, 10 to 30 parts by weight of hindered amine polymer and silica complexes as electret agents, combined with antistatic agents, lubricants, and anti- Thermal oxygen aging agent and toughener are prepared with low gas outlet resistance meltblown cloths through plastic extrusion, filtration, spinning, drafting, cooling, lamination, spunlace and electret processes.
A meltblown cloth with high filtration efficiency and low gas resistance is achieved, and the fiber charge residence time can reach more than 2 years, which significantly reduces the gas resistance of the meltblown cloth and improves the ventilation effect and protective performance of the mask.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure HDA0005045239750000011
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of meltblown fabric production, and in particular to a water-electret masterbatch, a meltblown fabric composition, a meltblown fabric and a preparation method thereof, and a mask. Background Art
[0002] Medical protective masks have become a daily necessity for people due to their protective effects, and the market demand is huge. Protective masks mainly play a filtering role. The middle layer of the mask is meltblown nonwoven fabric, which is the key core material to achieve barrier protection function.
[0003] Meltblown nonwoven fabric is a kind of ultra-fine fiber material with the advantages of fine fiber diameter, excellent filtration performance, and large dust holding capacity. It can effectively adsorb, capture and isolate toxic and harmful substances. In order to improve the barrier performance of meltblown cloth, it is often necessary to increase the density of meltblown cloth, which causes breathing discomfort after users wear it for a long time. At present, ordinary protective masks use meltblown cloth with corona electret as the key material, and filtration is mainly based on electrostatic adsorption. The principle is to use corona treatment to make the fibers of meltblown cloth charged, and the Coulomb force of the charged fibers is used to capture dust, bacteria, and viruses, thereby improving the filtration efficiency of the mask.
[0004] However, corona electret also has obvious disadvantages. The electrostatically treated fibers of meltblown cloth have a short charge residence time, and the adsorption capacity of the mask is low. After years of research and improvement, meltblown water-electret nonwoven filter materials have obvious advantages over corona electret meltblown nonwoven filter materials. However, there are still shortcomings in this type of product: the current industry standard meltblown cloth has a large pressure difference, and the masks produced have poor ventilation during wearing, which seriously affects the breathing of the wearer. For children and the elderly, the demand for low ventilation resistance poses new challenges to meltblown cloth for protective masks. Summary of the invention
[0005] In view of this, the technical problem to be solved by the present invention is to provide a water-electret masterbatch, a meltblown fabric composition, a meltblown fabric and a preparation method thereof, and a mask. The water-electret masterbatch provided by the present invention is applied to the preparation of the meltblown fabric to obtain a meltblown fabric with low air resistance and small loading attenuation.
[0006] The present invention provides a water electret masterbatch, comprising:
[0007] 60 to 80 parts by weight of polypropylene;
[0008] 10 to 30 parts by weight of an electret agent, wherein the electret agent is selected from a compound of a hindered amine polymer and silicon dioxide;
[0009] 1 to 5 parts by weight of an antistatic agent;
[0010] 1 to 3 parts by weight of a lubricant;
[0011] 0.25 to 1 parts by weight of a heat-oxidative aging inhibitor;
[0012] 0.1 to 1 parts by weight of toughening agent.
[0013] The water electret masterbatch of the present invention comprises 10 to 30 parts by weight of an electret agent, preferably 26.2 parts by weight of an electret agent; the electret agent of the present invention is selected from a compound of a hindered amine polymer and silicon dioxide; the hindered amine copolymer is selected from poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-[(2,2,6,6,-tetramethyl-piperidinyl)imino]-1,6-hexanediol[(2,2,6,6-tetramethyl-4-piperidinyl)imino]}; the silicon dioxide is selected from fumed silica. The inventors of the present application creatively discovered that by using a compound of hindered amine polymer and silica as an electret agent to prepare an electret masterbatch and applying it to the preparation of a meltblown cloth, the obtained meltblown cloth has low air resistance and small loading attenuation, and that the compound of hindered amine polymer and silica can only exert such a good additional effect in a water electret masterbatch, but cannot provide an additional effect when used in an electric electret masterbatch.
[0014] In one embodiment, the electret agent in the water electret masterbatch of the present invention is selected from a compound of poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-[(2,2,6,6,-tetramethyl-piperidinyl)imino]-1,6-hexanediol[(2,2,6,6-tetramethyl-4-piperidinyl)imino]} and fumed silica. In certain embodiments of the present invention, the weight ratio of the hindered amine polymer to silica is (3:1) to (7:1), preferably 5:1.
[0015] The water electret masterbatch of the present invention further comprises 60 to 80 parts by weight of polypropylene, preferably 67.7 parts by weight of polypropylene. In one embodiment, the polypropylene in the water electret masterbatch of the present invention is selected from Basel 650X polypropylene.
[0016] The water electret masterbatch of the present invention also includes 1 to 5 parts by weight of an antistatic agent, preferably 3 parts by weight of an antistatic agent. In some embodiments, the antistatic agent in the water electret masterbatch of the present invention is selected from at least one of an amide antistatic agent or a stearamide antistatic agent. In one embodiment, the antistatic agent in the water electret masterbatch of the present invention is selected from (N, N'-ethylene bis stearamide), because its molecules have polar amide groups, and the polarity is large and it is easy to absorb moisture in the air, which is conducive to the antistatic effect. At the same time, due to the limited compatibility with the polymer, the mobility of the antistatic agent is large, which is conducive to the antistatic effect.
[0017] The water electret masterbatch of the present invention further comprises 1 to 3 parts by weight of a lubricant, preferably 2 parts by weight of a lubricant. In some embodiments, the lubricant in the water electret masterbatch of the present invention is selected from zinc stearate. In one embodiment, the lubricant in the water electret masterbatch of the present invention is selected from nano-grade zinc stearate.
[0018] The water electret masterbatch of the present invention further comprises 0.25 to 1 parts by weight of an anti-thermal oxidative aging agent, preferably 0.8 parts by weight of an anti-thermal oxidative aging agent. In certain embodiments of the present invention, the anti-thermal oxidative aging agent in the water electret masterbatch of the present invention is selected from at least one of a hindered phenol antioxidant or a phosphite antioxidant. In some embodiments, the anti-thermal oxidative aging agent in the water electret masterbatch of the present invention is selected from at least one of a type 1010 antioxidant or a type 168 antioxidant. In one embodiment, the anti-thermal oxidative aging agent in the water electret masterbatch of the present invention is selected from a compound of a type 1010 antioxidant and a type 168 antioxidant.
[0019] The water electret masterbatch of the present invention also includes 0.1 to 1 parts by weight of a toughening agent, preferably 0.3 parts by weight of a toughening agent. In some embodiments, the toughening agent in the water electret masterbatch of the present invention is selected from non-crystalline or low-crystalline alpha-olefin copolymers (POE). In one embodiment, the toughening agent in the water electret masterbatch of the present invention is selected from Mitsui Chemicals DF710. Because PP and POE have similar polarities, the olefin chains contained in the POE molecules are easily combined with the PP molecular chains, and the compatibility of the two is very good. The POE particles and the PP matrix can form a well-connected interface, effectively transferring the internal stress. With reference to the "cavitation theory" toughening, in the process of melt-blown fiber drawing, the material is subjected to external force, causing three-dimensional tensile stress of the surrounding matrix, thereby inducing shear yield, preventing the fiber cracks from further expanding, consuming a lot of energy, and improving the toughness of the material.
[0020] In certain embodiments of the present invention, the water electret masterbatch of the present invention comprises 67.7 parts by weight of polypropylene; 26.2 parts by weight of electret agent; 3 parts by weight of antistatic agent; 2 parts by weight of lubricant; 0.8 parts by weight of anti-thermal oxidative aging agent; and 0.3 parts by weight of toughening agent. The polypropylene, electret agent, antistatic agent, lubricant, anti-thermal oxidative aging agent and toughening agent of the present invention are the same as those described above and will not be repeated. In one embodiment, the water electret masterbatch of the present invention comprises 67.7 parts by weight of Basel 650X polypropylene; 26.2 parts by weight of electret agent, wherein the electret agent is selected from a compound of hindered amine polymer and fumed silica; 3 parts by weight of (N,N'-ethylenebisstearamide); 2 parts by weight of nano-grade zinc stearate; 0.8 parts by weight of a compound of model 1010 antioxidant and model 168 antioxidant; and 0.3 parts by weight of Mitsui Chemicals DF710.
[0021] The present invention also provides a meltblown cloth composition, comprising: a polypropylene meltblown material; and the above-mentioned water-electret masterbatch.
[0022] In certain embodiments of the present invention, the melt index of the polypropylene meltblown material of the present invention is 1450-1550g / 10min, preferably 1500g / 10min. In one embodiment, the melt index of the polypropylene meltblown material is 1560g / 10min. The water-electret masterbatch of the present invention is the same as described above and will not be repeated. In some embodiments, the weight ratio of the polypropylene meltblown material and the water-electret masterbatch is (95-97): (3-5). In one embodiment, the weight ratio of the polypropylene meltblown material and the water-electret masterbatch is 95.5:4.5. In one embodiment, the meltblown cloth composition of the present invention comprises 95wt% to 97wt% of polypropylene meltblown material and 3wt% to 5wt% of the above-mentioned water-electret masterbatch.
[0023] The present invention provides a method for preparing a meltblown cloth, comprising:
[0024] The melt-blown fabric composition is sequentially subjected to plasticizing extrusion, filtration, spinning, drawing, cooling, web forming, hydroentanglement and electret charging to obtain a melt-blown fabric.
[0025] The present invention uses the above-mentioned meltblown fabric composition as raw material, that is, uses polypropylene meltblown material and the water-electret masterbatch of the present invention as raw materials, and mixes the polypropylene meltblown material and the water-electret masterbatch of the present invention to obtain the above-mentioned meltblown fabric composition.
[0026] The present invention first plasticizes and extrude the above-mentioned meltblown fabric composition. Specifically, the present invention first mixes the polypropylene meltblown material and the above-mentioned water electret masterbatch to obtain the above-mentioned meltblown fabric composition, and then plasticizes and extrude the meltblown fabric composition; the temperature of the plasticizing and extruding is 200-250°C, preferably 225-235°C, and more preferably 230°C. In one embodiment, the present invention transports the above-mentioned meltblown fabric composition after mixing evenly to the extruder upper bin for plasticizing and extruding through a vacuum suction system. In some embodiments, the plasticizing and extruding of the present invention is carried out by a single screw extruder, and the temperature of the screw extruder is controlled to 225-235°C, and the heating area of the screw extruder is divided into six temperature zones from zone one to zone six, and the temperature zones are 185°C ± 1°C, 210 ± 1°C, 220 ± 1°C, 225 ± 1°C, 230 ± 1°C and 230 ± 1°C from zone one to zone six, respectively.
[0027] The present invention plasticizes and extrudes the above-mentioned meltblown cloth composition to obtain a molten raw material, and then filters the molten raw material. Specifically, the present invention filters the molten raw material with a composite filter. In one embodiment, the present invention filters the molten raw material with a double plunger filter. The temperature at the connection of the double plunger filter of the present invention is controlled to 225-235°C, preferably 230°C; the composite filter is a five-layer composite 600-mesh filter, and the mesh numbers of each layer are 200 mesh, 300 mesh, 600 mesh, 300 mesh and 200 mesh respectively.
[0028] The present invention filters the molten raw material and then spins the filtered molten raw material. Specifically, the present invention measures and discharges the filtered molten raw material to the hanger-type die spinneret die head for spinning. In some embodiments, the present invention uses a metering pump to meter the filtered molten raw material to the hanger-type die spinneret die head, and distributes it to the spinneret through the die head for spinning. The metering pump of the present invention is a gear metering pump, and the temperature of the connection is controlled to 225-235°C, preferably 230°C; the metering pump speed is controlled to 10-20r / min, preferably 15r / min. The temperature of the hanger-type die head of the present invention is controlled to 240-260°C, preferably 250°C. Specifically, the die head temperature setting increases from the middle to both sides of the hanger type in sequence, and the range is controlled to 240-260°C, preferably 250°C; the spinneret air gap requires 1.0mm, and the aperture is 0.25-0.30mm. In one embodiment, the metering pump of the present invention is a 100cc / r model metering pump.
[0029] The present invention spins the filtered molten raw material to obtain meltblown fibers, and then draws the meltblown fibers. Specifically, the present invention draws the meltblown fibers using high-pressure air. In some embodiments, the present invention generates a high-speed hot air flow through a screw air compressor and an electric heater, and draws the meltblown fibers under the generated high-speed hot air flow. The temperature of the high-speed hot air flow of the present invention is 250-270°C, and the air volume of the high-speed hot air flow is 20-30m 3 / min, the pressure of the high-speed hot air flow is 0.06-0.08MPa. In one embodiment, the temperature of the high-speed hot air flow is 265°C, and the air volume of the high-speed hot air flow is 26.5m 3 / min, and the pressure of the high-speed hot air flow is 0.067MPa. The present invention adjusts the various parameters of the high-speed hot air used in the drafting, and the specific high-speed hot air flow is used for drafting to obtain the linear density of the charge-storing basic fiber, so that the high filtration efficiency of the product can be guaranteed in the pure water electret process.
[0030] After the melt-blown fibers are stretched, the stretched melt-blown fibers are cooled. Specifically, the stretched melt-blown fibers are cooled by cold air and then formed in a flat web-forming machine. In one embodiment, after the melt-blown fibers are stretched, the hot air after stretching the fibers is discharged through the web curtain of the web-forming machine, and the stretched melt-blown fibers are cooled and formed by cold air in a flat web-forming machine using a side-blowing cooling device, wherein the cold air temperature is 20 to 25°C, and the cold air speed is 3m / s to 5m / s. In one embodiment, after the melt-blown fibers are stretched, a centrifugal suction fan is used to discharge the hot air after stretching the fibers through the web curtain of the web-forming machine at a speed of 1200r / min; the stretched melt-blown fibers are cooled and formed by cold air using a side-blowing cooling device, wherein the cold air temperature is 23.5°C, and the cold air speed is 3.7m / s.
[0031] The present invention cools the stretched melt-blown fibers and forms a web. Specifically, the present invention cools the stretched melt-blown fibers and forms a web using a web-forming machine; the web-forming machine receives the melt-blown fibers in the middle of the air inlet, and the air permeability of the net curtain is ≥13000m 3 / h. The web-to-web receiving distance (DCD) of the present invention is 20-25 cm; the web-to-web receiving distance specifically refers to the receiving distance from the spinneret to the web-forming machine. In one embodiment, the present invention forms the meltblown fiber web by a flat web suction web-forming machine, and the air permeability of the web curtain of the web-forming machine is 13000m 3 / h, and the receiving distance (DCD) is 23.5cm. The present invention adjusts the receiving distance from spinning to web formation; by controlling the receiving distance from spinning to web formation, the tightness of fiber overlap can be increased or decreased. This process has an impact on the filtration efficiency, air resistance and strength of the product, but the air resistance of the product fluctuates more. After there is a base amount of fiber, the filtration efficiency of the product is basically guaranteed, but if the DCD distance is too short, the fiber overlap or the cooling is too short and the adhesion occurs, the air resistance will increase significantly. If the DCD distance is too large, the fiber is not fully overlapped and the product strength is not high. Therefore, this adjustment should take into account various indicators.
[0032] The present invention forms a web of meltblown fibers and then performs hydroentanglement on them. Specifically, the present invention uses ultrapure water for hydroentanglement; the resistivity of the ultrapure water is above 16MΩ.cm; in one embodiment, the resistivity of the ultrapure water is 16MΩ.cm. The ultrapure water is obtained by treating desalted water in sequence using activated carbon, quartz sand, reverse osmosis membrane, and EDI (electrode ionization technology). In some embodiments, the main water pressure for hydroentanglement is 1.5MPa to 1.8MPa. In one embodiment, the main water pressure for hydroentanglement is 1.55MPa.
[0033] The present invention performs electret after hydroentanglement on the melt-blown fibers after forming a web. Specifically, the present invention performs suction penetration electret on the melt-blown fibers after hydroentanglement. In some embodiments, the present invention performs suction penetration electret on the melt-blown fibers after hydroentanglement through a water ring vacuum system. In one embodiment, the present invention uses two water ring vacuum pumps to perform friction electret on the melt-blown fibers after hydroentanglement, and the vacuum degree is -10kPa.
[0034] After the meltblown fibers after spunlace are electret, the present invention also includes drying, winding, and slitting the meltblown fibers after electret to obtain the meltblown cloth with high filtration efficiency and low air resistance described in the present invention. In one embodiment, the present invention uses an electrically heated hot air shower to dry the residual moisture of the meltblown fibers after electret, and after cooling in the winding area, it is wound and cut under low pressure to obtain a meltblown cloth with high filtration efficiency and low air resistance. The drying of the present invention is carried out at 80-90°C; the temperature of the winding area is less than 28°C; the winding pressure is less than 0.2MPa. In one embodiment, the present invention uses a single-roller friction automatic switching winding machine (model φ800×1600) to roll the cloth, and the winding speed is controlled to be 10-15m / min.
[0035] The preparation method of the melt-blown cloth provided by the present invention uses the melt-blown cloth composition of the present invention as a raw material, and sequentially plasticizes and extrudes, filters, spins, draws, cools, forms a web, spunlaces and electrets to obtain the melt-blown cloth. The production process provided by the present invention is simple, low-cost, pollution-free, and can operate stably for a long time.
[0036] The present invention provides a meltblown cloth, which is prepared by the above-mentioned preparation method of the meltblown cloth. The present invention also provides a mask, which comprises a filter layer and other layers arranged on both sides of the filter layer; the filter layer comprises the above-mentioned meltblown cloth. The meltblown cloth obtained by the present invention has the characteristics of high porosity, fiber diameter less than 5μm, high filtration efficiency and low resistance.
[0037] The present invention provides a water electret masterbatch, a meltblown fabric composition, a meltblown fabric and a preparation method thereof, and a mask. The present invention uses the above-mentioned customized organic water electret masterbatch and a polypropylene high molecular polymer as raw materials to prepare a meltblown fabric, and the two have good compatibility. The combination of the two can enable the meltblown nonwoven material to maintain excellent filtration performance. In the process of production, the customized organic water electret masterbatch is easy to incorporate and disperse evenly, which is beneficial to improve the uniformity of fiber diameter. The customized organic water electret masterbatch in the present invention is a hindered amine light stabilizer material that can capture free radicals, and is compounded with fumed silica. After the electret treatment, the electret charge storage performance is good, and the charge retention rate can reach more than 2 years, which improves the comprehensive filtration efficiency and thermal attenuation resistance of the meltblown fabric. Under the condition of the same fiber fineness and gram weight of the meltblown product, the product gas resistance of the meltblown fabric is reduced. Experiments show that the melt-blown cloth prepared by using the water-electret masterbatch and polypropylene melt-blown material as raw materials has a PFE particle filtration efficiency of more than 99%, an air resistance as low as 45 to 50 Pa, high strength of the melt-blown cloth, and stable product quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a production process flow chart of the high filtration efficiency and low air resistance melt-blown cloth for protective masks provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0039] The present invention discloses a water-electret masterbatch, a meltblown fabric composition, a meltblown fabric and a preparation method thereof, and a mask. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It is particularly important to point out that all similar substitutions and modifications are obvious to those skilled in the art, and they are all deemed to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications of this article without departing from the content, spirit and scope of the present invention to realize and apply the technology of the present invention.
[0040] The specific components of the water electret masterbatch used in the specific embodiment of the present invention include:
[0041] 67.7 wt% of polypropylene, the polypropylene selected from Basel 650X polypropylene;
[0042] 26.2 wt% of an electret, wherein the electret is selected from a compound of poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-[(2,2,6,6,-tetramethyl-piperidinyl)imino]-1,6-hexanediol[(2,2,6,6-tetramethyl-4-piperidinyl)imino]} and fumed nano-silica;
[0043] 3wt% of an antistatic agent, wherein the antistatic agent is selected from (N,N'-ethylenebisstearamide);
[0044] 2wt% of a lubricant, wherein the lubricant is selected from nano-grade zinc stearate;
[0045] 0.8 wt % of a heat-oxidative aging inhibitor, wherein the heat-oxidative aging inhibitor is selected from a compound of a type 1010 antioxidant and a type 168 antioxidant; and
[0046] 0.3 wt% of a toughening agent, wherein the toughening agent is selected from Mitsui Chemicals DF710.
[0047] The specific embodiment of the present invention adopts the above-mentioned water electret masterbatch to prepare the meltblown cloth, such as Figure 1 As shown, Figure 1 This is a production process flow chart of the high filtration efficiency and low air resistance meltblown cloth for protective masks provided in Example 1 of the present invention.
[0048] The present invention will be further described below in conjunction with embodiments:
[0049] Example 1
[0050] Step S1) The polypropylene melt-blown material with a melt flow rate of 1560g / 10min and the above-mentioned customized water electret masterbatch are mixed evenly in a mass ratio of 95.5:4.5 by using a feeding system, and the mixed raw materials are transported to the feeding bin of the screw extruder through a vacuum suction system. The screw extruder is operated, and the raw materials are melt-plasticized and extruded by a single screw. Among them, the temperature of the screw extruder is controlled at 235°C, and the temperature zones are 185°C, 210°C, 220°C, 225°C, 230°C and 230°C from zone 1 to zone 6, respectively.
[0051] Step S2) filtering the molten polypropylene meltblown melt through a double plunger filter; wherein the temperature at the connection of the double plunger filter is controlled to 230° C., and the filter used for changing the filter is a composite 5-layer 600-mesh filter (the mesh numbers of each layer are 200 / 300 / 600 / 300 / 200, respectively).
[0052] Step S3) After the molten polypropylene melt is filtered, it is metered and discharged at 15 r / min using a 100cc / r gear metering pump, and is distributed to the hanger-shaped die spinneret die through the die head for spraying; wherein the die head temperature is set to increase from the middle to both sides of the hanger shape in sequence, and the range is controlled at 250°C; the spinneret air gap is required to be 1.0 mm and the aperture is 0.30 mm.
[0053] Step S4) Fibers are stretched by high-pressure air, specifically by using a screw air compressor and an electric heater to stretch the ejected fluid under a high-speed hot air flow, the high-speed hot air temperature is 265°C, and the hot air volume is 26.5m 3 / min, pressure 0.067MPa.
[0054] Step S5) using a centrifugal suction fan at a speed of 1200 r / min to discharge the hot air after the drafting fiber through the mesh curtain of the web forming machine; using a side-blowing cooling device to cool the melt-blown fiber, the cold air temperature is 23.5° C., and the wind speed is 3.7 m / s;
[0055] Step S6) The melt-blown fibers are received and formed by a flat-net suction-type web-forming machine, the area where the web-forming machine receives the melt-blown fibers is in the middle of the air suction port, and the air permeability of the web curtain of the web-forming machine is 13000m 3 / h, receiving distance (DCD) 23.5cm.
[0056] Step S7) Use activated carbon, quartz sand, reverse osmosis membrane, and EDI to treat the desalted water in sequence to obtain pure water with a resistivity of ≥16MΩ.cm; use a high-pressure water pump to transport the prepared pure water to the fan-shaped nozzle, and the fan-shaped nozzle hydroentangles the meltblown cloth. The main water pressure for hydroentanglement is 1.55MPa, and the pure water on the upper part of the cloth surface is sucked by a double water ring vacuum pump at a vacuum degree of -10KPa, so that the pure water and the meltblown cloth friction generates an electric charge, and the hydroentanglement electret is completed to charge the meltblown fiber.
[0057] Step S8) Use an electric hot air shower oven to dry the residual moisture of the meltblown fiber after water-entangled electret charging, and the temperature is controlled at 83°C; use a single-roller friction automatic switching winder (model φ800×1600) to roll the meltblown fiber, the speed is controlled at 10-15m / min, the temperature of the winding area is less than 28°C, and the winding pressure is less than 0.2MPa.
[0058] Comparative Example 1
[0059] Ordinary electret masterbatch and melt-blown material are mixed in a mass ratio of 3:100, and then melt-blown and corona electret are used to obtain melt-blown cloth. Ordinary electret masterbatch is ES-001. The raw material ratio is as follows: 66 parts of PP resin with a melt index of 1500, 30 parts of magnesium stearate, 3.5 parts of Japanese Idemitsu S400 polypropylene, and 0.5 parts of B215 as an anti-thermal oxidation aging agent. The above raw material powders are put into a high-speed mixer, stirred at a low speed for 5 minutes to mix evenly, and then fed into an extruder for extrusion and granulation to obtain electret masterbatch particles.
[0060] Comparative Example 2
[0061] Meltblown cloth was prepared according to the method of Example 1, except that the electret masterbatch used was Tianfeng 2# water electret masterbatch, 70 parts of PP resin with a melt index of 1500, 3 parts of EBS, 2 parts of zinc stearate, 24 parts of 944 as electret agent, 0.5 parts of 1010 and 0.5 parts of 168 as anti-thermal oxidation aging agent. The above raw material powder was put into a high-speed mixer, stirred at a low speed for 5 minutes to mix evenly, and then fed into an extruder for extrusion and granulation to obtain electret masterbatch particles. The hindered amine copolymer (electret 944) in the electret agent was selected from poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-[(2,2,6,6,-tetramethyl-piperidinyl)imino]-1,6-hexanediol[(2,2,6,6-tetramethyl-4-piperidinyl)imino]}.
[0062] Comparative Example 3
[0063] Meltblown cloth was prepared according to the method of Example 1, except that the electret masterbatch used was Tianfeng 4# water electret masterbatch, 60 parts of PP resin with a melt index of 800, 10 parts of EBS, 2 parts of zinc stearate were added, 40 parts of 2020 were used as the electret agent, and 0.5 parts of 1010 and 0.5 parts of 168 were used as the anti-thermal oxidation aging agent. The above raw material powders were put into a high-speed mixer, stirred at a low speed for 5 minutes to mix evenly, and then fed into an extruder for extrusion and granulation to obtain electret masterbatch particles. (Electret agent 2020) The triazine copolymer in the electret agent is selected from the polymer of the reaction product of N, N-bis (2, 2, 6, 6-tetramethyl-4-piperidinyl) -1, 6-hexanediamine and 2, 4, 6-trichloro-1, 3, 5-triazine and N-butyl-1-butylamine and N-butyl-2, 2, 6, 6-tetramethyl-4-piperidinamine.
[0064] Comparative Example 4
[0065] Tianfeng 2# water-electret masterbatch was mixed with melt-blown material in a mass ratio of 3:100, and then melt-blown, and corona electret was used to obtain the melt-blown cloth.
[0066] Comparative Example 5
[0067] Tianfeng 4# water-electret masterbatch was mixed with melt-blown material in a mass ratio of 3:100, and then melt-blown, and corona electret was used to obtain the melt-blown cloth.
[0068] The embodiments of the present invention have achieved some positive effects in the downstream mask production process, and do have great advantages over the prior art. The melt-blown cloths of Example 1 and Comparative Examples 1 to 3 were melt-blown tests, and the effects are shown in Tables 1 to 3. Table 1 is a comparison data table of double-layer melt-blown cloth detection at 85 L / min of ordinary electret ES-001, Tianfeng 2# water electret, Tianfeng 4# water electret and the customized water electret masterbatch of the present invention, Table 2 is a comparison data table of double-layer melt-blown cloth detection at 95 L / min of Tianfeng 4# water electret masterbatch and the customized water electret masterbatch of the present invention, Table 3 is a comparison data table of double-layer melt-blown cloth detection at 85 L / min of electret masterbatch ES-001, Tianfeng 2# water electret masterbatch and Tianfeng 4# water electret masterbatch under corona electret process;
[0069] Table 1
[0070]
[0071] Table 2
[0072] Product Categories PFE filtration efficiency (%) Air resistance(Pa) <![CDATA[Grammage (g / m 2 )]]> Loading attenuation (%) Comparative Example 3 99~99.5 130~140 25±7% 10 Example 1 99~99.5 110~130 25±7% 2
[0073] Table 3
[0074]
[0075] As can be seen from the above table, the hindered amine polymer water electret masterbatch is used in the corona electret process to produce meltblown cloth. Under the same filtration efficiency, the product air resistance is not significantly improved, but the cost is increased; as can be seen from Table 1, the hindered polymer water electret masterbatch is used to produce products under the conditions of the water spunlace electret process. Under the same filtration efficiency, the product air resistance has been greatly reduced; as can be seen from Tables 2 and 3, the resistance of the meltblown cloth prepared by the water electret masterbatch combined with the production process of the present invention can be reduced by 40-50%, the PFE filtration efficiency reaches more than 99%, and the elongation is improved to a certain extent. The charge retention of the meltblown cloth with customized water electret masterbatch can reach more than 2 years without attenuation, and the product of this production process not only has high filtration efficiency, but also has low air resistance and high strength. Therefore, the present invention adopts the above-mentioned high filtration efficiency and low air resistance meltblown cloth process for protective masks, which can solve the problem of high inhalation resistance of protective masks.
[0076] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A water electret masterbatch, characterized in that: include: 60 to 80 parts by weight of polypropylene; 10 to 30 parts by weight of an electret agent, wherein the electret agent is selected from a compound of a hindered amine polymer and silicon dioxide; 1 to 5 parts by weight of an antistatic agent; 1 to 3 parts by weight of a lubricant; 0.25 to 1 parts by weight of a heat-oxidative aging inhibitor; 0.1 to 1 parts by weight of toughening agent.
2. The water electret masterbatch according to claim 1, characterized in that: The hindered amine copolymer is selected from poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-[(2,2,6,6,-tetramethyl-piperidinyl)imino]-1,6-hexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl)imino]}; The silicon dioxide is selected from fumed silicon dioxide.
3. The water electret masterbatch according to claim 1, characterized in that: The weight ratio of the hindered amine polymer to silicon dioxide is (3:1) to (7:1).
4. The water electret masterbatch according to claim 1, characterized in that: include: 67.7 parts by weight of polypropylene; 26.2 parts by weight of electret; 3 parts by weight of an antistatic agent; 2 parts by weight of a lubricant; 0.8 parts by weight of thermal oxidation aging inhibitor; 0.3 parts by weight of toughening agent.
5. A meltblown fabric composition, characterized in that: include: Polypropylene meltblown material; and The water-electret masterbatch according to any one of claims 1 to 4.
6. The meltblown fabric composition according to claim 5, characterized in that: The weight ratio of the polypropylene meltblown material to the water-electret masterbatch is (95-97): (3-5).
7. A method for preparing a meltblown cloth, characterized in that: include: The melt-blown fabric composition according to claim 5 or 6 is sequentially subjected to plasticizing extrusion, filtration, spinning, drawing, cooling, web forming, hydroentanglement and electret to obtain a melt-blown fabric.
8. The preparation method according to claim 7, characterized in that: The drawing is carried out under a high-speed hot air flow, the temperature of the high-speed hot air flow is 250°C to 270°C, and the air volume of the high-speed hot air flow is 20 to 30 m 3 / min; The receiving distance from spinning to web forming is 20cm to 25cm.
9. A meltblown cloth, characterized in that: The compound is prepared by the preparation method according to claim 7 or 8.
10. A mask, characterized in that: It includes a filter layer and other layers arranged on both sides of the filter layer; The filter layer comprises the meltblown cloth according to claim 9.