Diatomite-based moisture absorption and sweat releasing cloth and preparation method thereof

By adopting a combination of three-layer structure and hydrophobic nanoparticles in the moisture-absorbing fabric, the problem of blockage of the porous structure of diatomaceous earth is solved, achieving better moisture-absorbing and sweating performance and durability.

CN119019941APending Publication Date: 2024-11-26FUJIAN HUAFENG NEW MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411198126.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, the porous structure of diatomaceous earth is blocked by polymers, resulting in a degradation of moisture-absorbing and sweating properties.

Method used

Design of moisture-absorbing and sweating fabric with a three-layer structure, including a base fabric layer, an adhesive layer and a diatomaceous earth layer, which partially penetrates into the adhesive layer and adds hydrophobic nanoparticles to improve fluidity and dispersion. , the adhesive layer is evenly adhered and partially penetrated through the electrostatic spraying process.

Benefits of technology

It effectively maintains the porous structure of diatomaceous earth, improves the moisture-wicking effect and wash resistance of the fabric, and enhances the adhesion firmness and moisture-absorbing and breathable properties of diatomaceous earth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019941A_ABST
    Figure CN119019941A_ABST
Patent Text Reader

Abstract

The invention provides a moisture absorption and sweat releasing fabric based on diatomite and a preparation method thereof, and relates to the technical field of textiles. The moisture absorption and sweat releasing cloth sequentially comprises a basic cloth layer, an adhesive layer and a diatomite layer from bottom to top, and the diatomite layer partially permeates into the adhesive layer. Furthermore, the raw material components of the diatomite layer comprise diatomite and hydrophobic nanoparticles. The moisture-absorbing and sweat-releasing cloth can give full play to the moisture-absorbing and breathable performance of diatomite, and is good in durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of textiles and relates to a moisture-absorbing and perspiration-releasing fabric based on diatomaceous earth and a preparation method thereof. Background Art

[0002] Diatomaceous earth has a special porous structure and is often used to prepare moisture-absorbing and perspiration-releasing fabrics. At present, diatomaceous earth or modified diatomaceous earth is generally added to fabric materials, such as polyester, nylon, spandex, etc., to prepare composite materials, which are then woven into fibers; or diatomaceous earth or modified diatomaceous earth is dispersed in an emulsion, and then attached to the fiber or fabric surface by spraying, printing, etc. However, since the above-mentioned prior art directly disperses diatomaceous earth into a polymer (such as the main resin of a fabric material or an emulsion), the polymer will enter the porous structure of the diatomaceous earth, causing part or all of the porous structure to be blocked, affecting the effectiveness of the diatomaceous earth and also causing the moisture-absorbing and perspiration-releasing performance of the fabric to decrease.

[0003] In view of this, it is necessary to optimize and improve the existing technology. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a moisture absorption and perspiration-releasing fabric based on diatomaceous earth and a preparation method thereof.

[0005] The technical solution of the present invention is as follows:

[0006] A moisture-absorbing and perspiration-releasing fabric based on diatomaceous earth, comprising, from bottom to top, a base fabric layer, an adhesive layer and a diatomaceous earth layer;

[0007] The diatomaceous earth layer partially penetrates into the adhesive layer.

[0008] Preferably, the thickness of the adhesive layer is 0.02 mm-1 mm.

[0009] Preferably, the thickness of the diatomaceous earth layer is 1-100 μm.

[0010] Preferably, the raw material components of the diatomaceous earth layer include diatomaceous earth and hydrophobic nanoparticles.

[0011] More preferably, the weight ratio of the diatomaceous earth to the hydrophobic nanoparticles is 1:0.0005-0.005.

[0012] More preferably, the particle size of the diatomaceous earth is 200-12000 mesh.

[0013] More preferably, the average particle size of the hydrophobic nanoparticles is 5-100 nm.

[0014] A method for preparing the moisture wicking fabric according to any one of the above embodiments comprises applying an adhesive to the base fabric layer, applying the raw material components of the diatomaceous earth layer to the surface of the adhesive, and drying to obtain the moisture wicking fabric.

[0015] Preferably, the adhesive is selected from a water-based adhesive or an oil-based adhesive.

[0016] Preferably, the raw material components of the diatomaceous earth layer are applied to the surface of the adhesive by electrostatic spraying.

[0017] The beneficial effects of the present invention are:

[0018] (1) The present invention coats a thin layer of adhesive on a fabric layer, applies diatomaceous earth to the surface of the adhesive before the adhesive is cured, and then heats and cures the adhesive, so that a layer of diatomaceous earth is firmly adhered to the outer surface of the fabric, and the porous structure of the diatomaceous earth is basically not blocked, so that the effect of the diatomaceous earth can be fully exerted, thereby improving the moisture absorption and perspiration removal effect of the fabric.

[0019] (2) A small amount of hydrophobic nanoparticles is added to the diatomaceous earth of the present invention, which significantly improves the fluidity and dispersibility of the diatomaceous earth. Through the electrostatic spraying process, the diatomaceous earth can be more evenly adhered to the surface of the adhesive. Moreover, since the electrostatic spraying has a certain force, the diatomaceous earth can partially penetrate into the adhesive, thereby improving the adhesion firmness of the diatomaceous earth. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic structural diagram of the moisture wicking fabric of the present invention. DETAILED DESCRIPTION

[0021] The technical solution of the present invention is further illustrated and described below through specific implementation methods.

[0022] In order to solve the problem in the prior art that the porous structure of diatomaceous earth may be blocked, resulting in poor moisture absorption and perspiration removal effect of the fabric, on the one hand, the present invention provides a moisture absorption and perspiration removal fabric based on diatomaceous earth, comprising three layers, including, from bottom to top, a base fabric layer (1), an adhesive layer (2) and a diatomaceous earth layer (3);

[0023] The diatomaceous earth layer (3) partially penetrates into the adhesive layer (2).

[0024] In the present invention, the moisture wicking fabric comprises a base fabric layer, an adhesive layer and a diatomaceous earth layer, and the adhesive serves as an intermediate layer to adhere the diatomaceous earth layer to the base fabric layer. In the present invention, there is no particular limitation on the base fabric layer, and it can be a fabric material commonly used in textiles or a composite of various fabric materials, and the fabric material includes but is not limited to cotton, polyester, polypropylene, nylon, linen, silk, satin, nylon, etc.

[0025] The partial penetration of the diatomaceous earth layer into the adhesive layer means that there is no obvious interface between the diatomaceous earth layer and the adhesive layer, and part of the diatomaceous earth penetrates into the adhesive layer, which is conducive to improving the adhesion between the diatomaceous earth layer and the adhesive layer, and is not easy to fall off. After multiple washings, the diatomaceous earth layer can still adhere to the adhesive layer relatively firmly and has good wash resistance.

[0026] In a preferred embodiment of the present invention, the thickness of the adhesive layer (2) is 0.02mm-1mm. In the present invention, the thickness of the adhesive layer cannot be too thick, otherwise it will affect the feel and air permeability of the fabric. For example, the thickness of the adhesive layer can be any value among 0.02mm, 0.05mm, 0.08mm, 0.1mm, 0.12mm, 0.15mm, 0.18mm, 0.2mm, 0.23mm, 0.25mm, 0.3mm, 0.33mm, 0.35mm, 0.37mm, 0.4mm, 0.45mm, 0.5mm, 0.55mm, 0.6mm, 0.65mm, 0.7mm, 0.75mm, 0.8mm, 0.85mm, 0.9mm, 0.95mm, 1mm, etc., but not limited to the above-mentioned values. In a further preferred embodiment, the thickness of the adhesive layer can be 0.05-0.5mm.

[0027] In a preferred embodiment of the present invention, the thickness of the diatomaceous earth layer (3) is 1-100 μm. In the present invention, since the diatomaceous earth layer is adhered to the base fabric layer by the adhesive layer, the diatomaceous earth not adhered by the adhesive will fall off, and only the diatomaceous earth in contact with and bonded to the adhesive will form the diatomaceous earth layer, so the diatomaceous earth layer will not be very thick, and is basically not much different from the size of the diatomaceous earth particles. For example, the thickness of the diatomaceous earth layer can be any value of 1 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm, 100 μm, etc., but is not limited to the above-mentioned values.

[0028] In a preferred embodiment of the present invention, the raw material components of the diatomaceous earth layer (3) include diatomaceous earth and hydrophobic nanoparticles. When the untreated diatomaceous earth reaches the micron, submicron or nanometer level, it is easy to agglomerate due to the strong interaction between particles, resulting in poor fluidity and difficulty in dispersion. Therefore, the diatomaceous earth is not easy to apply to the surface of the adhesive, or part of the diatomaceous earth will be adsorbed on the diatomaceous earth layer due to the interaction between particles, but the adsorption force is very weak, and it is easy to fall off during subsequent processing or use, affecting the processing effect or use effect. If the diatomaceous earth is treated with hydrophobic treatment agents such as trimethylchlorosilane, hexamethyldisilazane, etc., the dispersibility and fluidity of the diatomaceous earth can be improved, but (1) the cost is greatly increased, and the cost of diatomaceous earth will increase several times or even higher; (2) it will affect the adhesion of the adhesive to it, resulting in a shorter service life of the diatomaceous earth layer; (3) the diatomaceous earth layer after hydrophobic treatment has good water repellency and poor water absorption, which will affect the moisture absorption and perspiration effect of the fabric. The present invention finds that adding hydrophobic nanoparticles to untreated diatomaceous earth (a mixture of diatomaceous earth and hydrophobic nanoparticles is a composite material) can significantly improve the fluidity and dispersibility of diatomaceous earth. Without substantially affecting the cost of diatomaceous earth, diatomaceous earth can be smoothly applied to the surface of the adhesive, and excess, unadhered diatomaceous earth can be removed by vibration or the like, and the moisture absorption and perspiration removal effect of diatomaceous earth will not be affected. There is no particular limitation on the mixing and dispersing method of diatomaceous earth and hydrophobic nanoparticles, and methods such as vibration dispersion by a vibrator or dispersion by a three-dimensional mixer can be used.

[0029] The fluidity of diatomite can be tested by using a vibrating screen. One test method is as follows: 100g of diatomite or composite material is placed on a 300-mesh screen and vibrated. The weight of the diatomite or composite material remaining on the screen is x, and the screening rate is (100-x) / 100×100%. The higher the screening rate, the better the fluidity of the diatomite or composite material. The screening rate of untreated diatomite is generally no more than 50%, while the screening rate of the composite material can reach 70% and above, and even 90%.

[0030] In a more preferred embodiment of the present invention, the weight ratio of diatomite to hydrophobic nanoparticles is 1:0.0005-0.005. In the present invention, adding a small amount of hydrophobic nanoparticles to diatomite can significantly improve the fluidity and dispersibility of diatomite. For example, the weight ratio of diatomite to hydrophobic nanoparticles can be any value in 1:0.0005, 1:0.001, 1:0.0012, 1:0.0015, 1:0.0018, 1:0.002, 1:0.0022, 1:0.0025, 1:0.0027, 1:0.003, 1:0.0033, 1:0.0035, 1:0.004, 1:0.0042, 1:0.0045, 1:0.005, etc., but is not limited to the above-mentioned values. However, the amount of hydrophobic nanoparticles added cannot be too much, for example, it cannot exceed 1% of the weight of the diatomaceous earth, otherwise the hydrophobicity of the hydrophobic nanoparticles will affect the hydrophilicity and moisture absorption and air permeability of the diatomaceous earth.

[0031] In a more preferred embodiment of the present invention, the particle size of diatomaceous earth is 200-12000 mesh. In the present invention, the particle size of diatomaceous earth cannot be too large, such as 100 mesh or 150 mesh. If it is too large, it will affect the comfort of wearing, the adhesion of diatomaceous earth will also be reduced, and the service life will be shortened. If the particle size of diatomaceous earth is too small, such as 15000 mesh or 20000 mesh, the arrangement of diatomaceous earth will be very dense and the thickness will be very thin, which will affect the moisture absorption and breathability performance. For example, the particle size of diatomaceous earth can be any value among 200 mesh, 500 mesh, 1000 mesh, 1200 mesh, 1500 mesh, 1800 mesh, 2000 mesh, 2500 mesh, 3000 mesh, 3500 mesh, 4000 mesh, 4500 mesh, 5000 mesh, 5500 mesh, 6000 mesh, 6500 mesh, 7000 mesh, 7500 mesh, 8000 mesh, 8500 mesh, 9000 mesh, 9500 mesh, 10000 mesh, 11000 mesh, 12000 mesh, etc., but is not limited to the above-mentioned values.

[0032] In a more preferred embodiment of the present invention, the average particle size of the hydrophobic nanoparticles is 5-100nm. For example, the average particle size of the hydrophobic nanoparticles can be any value of 5nm, 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, 85nm, 90nm, 95nm, 100nm, etc., but is not limited to the above-mentioned ones. The hydrophobic nanoparticles can be obtained by surface treatment of the nanoparticles with a hydrophobic treatment agent, which is a conventional technique in the art. The hydrophobic treatment agent is mainly an organic compound or an organic-inorganic hybrid compound with good hydrophobicity, such as stearyl alcohol, lauryl alcohol, hexamethyldisilazane, trimethylchlorosilane, trimethylmethoxysilane, octadecyldimethylchlorosilane, etc., and the organosilane compounds such as hexamethyldisilazane and trimethylchlorosilane are more commonly used in the industry, which have the characteristics of high reactivity and good hydrophobic effect. Nanoparticles can be inorganic nanoparticles, such as nano silicon dioxide, nano zirconium oxide, nano aluminum oxide, nano titanium dioxide, nano zinc oxide, nano calcium carbonate, nano kaolin, etc., or organic nanoparticles, such as nano polyethylene particles, nano polytetrafluoroethylene particles, etc. When organic nanoparticles are used, if the organic nanoparticles already show good hydrophobic properties, hydrophobic treatment is not required. The hydrophobicity of hydrophobic nanoparticles can be characterized by the methanol value, and the test method is as follows: add 50ml of clean water to a beaker, add 0.2g of hydrophobic nanoparticles, the hydrophobic nanoparticles float on the water surface, and under magnetic stirring, gradually add methanol until the hydrophobic nanoparticles are just completely dispersed in the water phase. At this time, the volume of methanol added is Aml, and the methanol value = A / (A+50)×100. Generally, after the nanoparticles are surface treated with a hydrophobic treatment agent, the methanol value of the hydrophobic nanoparticles is above 40%. The higher the methanol value, the better the hydrophobicity of the hydrophobic nanoparticles.

[0033] On the other hand, the present invention provides a method for preparing the moisture wicking fabric described in any of the above embodiments, wherein an adhesive is applied to a base fabric layer, and then the raw material components of the diatomaceous earth layer are applied to the surface of the adhesive, and dried to obtain the moisture wicking fabric. In the present invention, the method of applying the adhesive to the base fabric layer is not limited, and the more commonly used methods may be screen printing, spraying, brushing, rolling, etc.

[0034] In a preferred embodiment of the present invention, the adhesive is selected from a water-based adhesive or an oil-based adhesive. Both the water-based adhesive and the oil-based adhesive can be directly obtained from the market, such as PU667 from Nanjing Xinyi Synthetic Technology Co., Ltd., EP706K from Wacker, and the like.

[0035] In a more preferred embodiment of the present invention, the raw material components of the diatomaceous earth layer are applied to the surface of the adhesive by electrostatic spraying. The use of electrostatic spraying is conducive to the contact and penetration of the raw material components of the diatomaceous earth layer with the adhesive, improves the bonding strength between the diatomaceous earth layer and the adhesive, and improves the washability.

[0036] According to the method of the present invention, the moisture wicking fabric of the present invention can also contain diatomaceous earth layers on both sides of the fabric, that is, diatomaceous earth layer, adhesive layer, fabric layer, adhesive layer, diatomaceous earth layer in sequence, which can further improve the moisture wicking effect of the fabric. The preparation method can be performed on one side and then on the other side according to the same steps. The fabric has better moisture absorption and air permeability when both sides contain diatomaceous earth layers.

[0037] The technical solution of the present invention is further described and illustrated according to various embodiments below. Unless otherwise specified, the parts described in the following embodiments are parts by weight.

[0038] Example 1

[0039] 100 parts of untreated diatomaceous earth (8000 mesh) and 0.05 parts of hydrophobic nano-silica (average particle size 12 nm, surface hydrophobic treatment with hexamethyldisilazane, methanol value 58%) were added to a three-dimensional mixer, and rotated at 20 rpm for 5 minutes to obtain a composite material. The screening rate of the composite material on a 300-mesh sieve was 74%, and the screening rate of the untreated diatomaceous earth on a 300-mesh sieve was 45%.

[0040] The commercially available water-based adhesive PU667 was sprayed on one side of the cotton cloth with a thickness of about 0.2 mm, and then the above composite material was sprayed on the adhesive by electrostatic spraying, and the unadhered composite material was removed by vibration, and dried at 60°C for 3 hours to obtain a moisture-absorbing and perspiration-wicking fabric.

[0041] Example 2

[0042] The difference between this embodiment and embodiment 1 is that in embodiment 1, the hydrophobic nano-silicon dioxide is adjusted from 0.05 parts to 0.15 parts. The remaining steps remain unchanged. The screening rate of the test composite material on a 300-mesh sieve is 81%.

[0043] Example 3

[0044] The difference between this embodiment and embodiment 1 is that in embodiment 1, the hydrophobic nano-silicon dioxide is adjusted from 0.05 parts to 0.3 parts. The remaining steps remain unchanged. The screening rate of the test composite material on a 300-mesh sieve is 93%.

[0045] Example 4

[0046] The difference between this embodiment and embodiment 1 is that in embodiment 1, the hydrophobic nano-silicon dioxide is adjusted from 0.05 parts to 0.5 parts. The remaining steps remain unchanged. The screening rate of the test composite material on a 300-mesh sieve is 95%.

[0047] Example 5

[0048] The difference between this embodiment and embodiment 1 is that in embodiment 1, the composite material is replaced by an equal weight of untreated diatomaceous earth, and the untreated diatomaceous earth is directly sprayed on the adhesive. The other steps remain unchanged.

[0049] Example 6

[0050] The difference between this embodiment and embodiment 1 is that in embodiment 1, the hydrophobic nano-silicon dioxide is adjusted from 0.05 parts to 1 part. The other steps remain unchanged. The screening rate of the test composite material on a 300-mesh sieve is 97%.

[0051] Example 7

[0052] 100 parts of untreated diatomaceous earth (5000 mesh) and 0.2 parts of hydrophobic nano-alumina (average particle size 30 nm, surface hydrophobic treatment with trimethylchlorosilane, methanol value 61%) were added to a three-dimensional mixer, and rotated at 20 rpm for 8 minutes to obtain a composite material. The screening rate of the composite material on a 300 mesh sieve was 87%, and the screening rate of the untreated diatomaceous earth on a 300 mesh sieve was 47%.

[0053] The commercially available water-based adhesive PU667 was sprayed on one side of the cotton cloth with a thickness of about 0.1 mm, and then the above composite material was sprayed on the adhesive by electrostatic spraying, and the unadhered composite material was removed by vibration, and the fabric was dried at 60°C for 3 hours to obtain a moisture-absorbing and perspiration-wicking fabric.

[0054] Example 8

[0055] The difference between this embodiment and embodiment 7 is that after drying at 60° C. for 3 hours, the water-based adhesive PU667 and the composite material are sprayed on the other side of the cotton cloth according to the steps of embodiment 5. The other steps remain unchanged. That is, the diatomaceous earth layer is coated on both sides of the cotton cloth.

[0056] Example 9

[0057] The difference between this embodiment and embodiment 7 is that the hydrophobic nano-silica is replaced by an equal weight of hydrophobic kaolin (average particle size 75 nm, surface hydrophobic treatment with trimethylchlorosilane, methanol value 54%). The remaining steps remain unchanged.

[0058] Example 10

[0059] The difference between this embodiment and embodiment 7 is that the untreated diatomaceous earth is replaced by an equal weight of 1000 mesh untreated diatomaceous earth. The other steps remain unchanged. The screening rate of the test composite material on the 300 mesh sieve is 92%, and the screening rate of the untreated diatomaceous earth on the 300 mesh sieve is 50%.

[0060] Performance Testing

[0061] The drying speed, water absorption rate and drip diffusion time were tested according to the method of GB / T 21655.1-2023. The results are shown in Table 1. The faster the drying speed, the higher the water absorption rate and the shorter the drip diffusion time, the better the moisture absorption and air permeability.

[0062] Durability: After the moisture wicking fabric to be tested has been washed 20 times in a standard manner, the water absorption rate is tested according to the above scheme, and the water absorption retention rate is calculated. The higher the water absorption retention rate, the better the durability.

[0063] The results are shown in Table 1 below.

[0064] Table 1

[0065]

[0066] It can be seen from the data results in Table 1 that the moisture wicking fabric of the present invention has good hydrophilicity, good absorption and air permeability, and can achieve good moisture wicking effect.

[0067] As described above, the basic principles, main features and advantages of the present invention are shown and described. Those skilled in the art should understand that the present invention is not limited by the above embodiments, which are only preferred embodiments of the present invention and cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the scope of the present invention and the content of the specification should still be within the scope of the present invention. The scope of protection required by the present invention is defined by the attached claims and their equivalents.

Claims

1. A moisture wicking fabric based on diatomaceous earth, characterized in that: It includes a base fabric layer, an adhesive layer and a diatomaceous earth layer from bottom to top; The diatomaceous earth layer partially penetrates into the adhesive layer.

2. The moisture wicking fabric according to claim 1, characterized in that: The thickness of the adhesive layer is 0.02 mm-1 mm.

3. The moisture wicking fabric according to claim 1, characterized in that: The thickness of the diatomaceous earth layer is 1-100 μm.

4. The moisture wicking fabric according to claim 1, characterized in that: The raw material components of the diatomaceous earth layer include diatomaceous earth and hydrophobic nanoparticles.

5. The moisture wicking fabric according to claim 4, characterized in that: The weight ratio of the diatomaceous earth to the hydrophobic nanoparticles is 1:0.0005-0.

005.

6. The moisture wicking fabric according to claim 4, characterized in that: The particle size of the diatomaceous earth is 200-12000 meshes.

7. The moisture wicking fabric according to claim 4, characterized in that: The average particle size of the hydrophobic nanoparticles is 5-100 nm.

8. A method for preparing the moisture wicking fabric according to any one of claims 1 to 7, characterized in that: The adhesive is applied to the base fabric layer, and the raw material components of the diatomaceous earth layer are applied to the surface of the adhesive, and then dried to obtain the moisture wicking fabric.

9. The method for preparing a moisture wicking fabric according to claim 8, characterized in that: The adhesive is selected from a water-based adhesive or an oil-based adhesive.

10. The method for preparing a moisture wicking fabric according to claim 8, characterized in that: The raw material components of the diatomaceous earth layer are applied to the surface of the adhesive by electrostatic spraying.