Nano precipitated phase reinforced hydrogen embrittlement-resistant medium-entropy alloy and preparation method thereof

Through the nano-precipitation phase strengthening medium-entropy alloy process, arc smelting and homogenization treatment are used to form nano-scale L12 precipitation phase, and the hydrogen embrittlement problem of medium-entropy alloy is solved through the partial accumulation of B atoms, which significantly improves the strength of the material and anti-hydrogen embrittlement properties.

CN119020655AActive Publication Date: 2024-11-26UNIV OF SCI & TECH BEIJING
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411135474.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

Medium-entropy alloys are prone to hydrogen embrittlement problems during long-term use, resulting in degradation of material performance and limited application. It is difficult for the existing technology to effectively solve this bottleneck problem.

Method used

The hydrogen-embrittle medium-entropy alloy is strengthened with nano-precipitation phase. It is cold rolled and aging treatment after arc smelting and homogenization to form a nano-scale L12 precipitation phase with high dispersion distribution. Combined with the partial aggregate of trace B atoms, the alloy is enhanced. anti-hydrogen embrittlement properties.

Benefits of technology

It significantly improves the yield strength and ductility of medium-entropy alloys, and significantly reduces the hydrogen embrittlement sensitivity index, extends the service life of the material, and improves the anti-hydrogen embrittlement performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020655A_ABST
    Figure CN119020655A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of medium-entropy alloys, and particularly relates to a nano precipitated phase reinforced hydrogen embrittlement-resistant medium-entropy alloy and a preparation method thereof.The high-dispersion-distribution nano-scale L12 phase precipitated medium-entropy alloy is obtained in the modes of electric arc melting, homogenization treatment, cold rolling and aging treatment, and matching of the strength and toughness of the medium-entropy alloy is achieved; and the hydrogen embrittlement resistance of the material in the service process is greatly improved, and the method has profound significance in improving the comprehensive performance such as material strengthening and hydrogen embrittlement resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of medium-entropy alloys, and in particular to a nano-precipitation phase reinforced hydrogen embrittlement-resistant medium-entropy alloy and a preparation method thereof. Background Art

[0002] With the advancement of major industries such as aerospace, national defense and heavy industry, as well as the development of hydrogen energy, it is urgent to develop new alloy materials with high strength, high toughness, resistance to hydrogen embrittlement, and corrosion resistance. As people further deepen their research on medium-entropy alloys, their unique properties including high strength and high ductility have gradually attracted people's attention. However, for a long time, the hydrogen embrittlement problem has been a bottleneck problem restricting the industrial application of medium-entropy alloys, which often has disastrous consequences. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a nano-precipitation phase strengthened hydrogen embrittlement resistant medium entropy alloy and a preparation method thereof.

[0004] According to one aspect of the present invention, the present invention provides the following technical solution:

[0005] A nano-precipitation phase strengthened hydrogen embrittlement resistant medium entropy alloy comprises, by mass percentage: 33.30-34.30% Co; 33.20-34.20% Ni; 29.45-30.45% Cr; 1.30-1.90% Ti; 0.65-1.05% Al; 0.04-0.06% B; the remainder being inevitable impurities.

[0006] As a preferred solution of a nano-precipitation phase strengthening hydrogen embrittlement-resistant medium-entropy alloy described in the present invention, the microstructure of the medium-entropy alloy is an FCC solid solution structure composed of Co, Cr, Ni and a small amount of Al and Ti in an equiatomic ratio and a nano-scale L12 precipitation phase dispersed in the matrix. The three elements Co, Cr and Ni are the main elements constituting the medium-entropy alloy. They form a face-centered cubic (FCC) solid solution structure in an equiatomic ratio, thereby providing good plasticity and toughness; Al forms an L12-type nano-scale precipitation phase with other elements in the alloy, significantly improving the strength of the alloy; Ti can form a stable TiC with Al, which helps to fix C in the alloy and prevent the precipitation of carbides, thereby maintaining the uniformity of the alloy; trace amounts of B atoms tend to segregate at the grain boundaries, enhancing the cohesion of the grain boundaries, thereby improving the hydrogen embrittlement resistance of the alloy. In addition, the segregation of B can also reduce the diffusion rate of hydrogen at the grain boundaries, reduce the stress concentration of hydrogen at the grain boundaries, and thus reduce the nucleation and expansion of hydrogen-induced cracks.

[0007] As a preferred solution of the nano-precipitation phase strengthened hydrogen embrittlement resistant medium entropy alloy described in the present invention, wherein: the average size of the nano-scale L12 precipitate phase is 17.5-27.0 nm.

[0008] As a preferred embodiment of the nano-precipitation phase strengthened hydrogen embrittlement resistant medium entropy alloy described in the present invention, the yield strength of the nano-precipitation phase strengthened hydrogen embrittlement resistant medium entropy alloy is ≥780MPa, the ductility is ≥39.0%, the hydrogen embrittlement sensitivity index is ≤4.5% after 24 hours of hydrogen pre-charging, and the hydrogen embrittlement sensitivity index is ≤9.5% after 72 hours of hydrogen pre-charging.

[0009] According to another aspect of the present invention, the present invention provides the following technical solution:

[0010] A method for preparing a nano-precipitated phase-reinforced hydrogen embrittlement-resistant medium-entropy alloy comprises the following steps:

[0011] S1. Take raw materials according to the composition of the medium-entropy alloy, and obtain a medium-entropy alloy ingot by arc melting in an argon atmosphere;

[0012] S2, the ingot is homogenized to control the element distribution;

[0013] S3, the ingot is rolled by cold rolling process to obtain a plate;

[0014] S4. The plate is subjected to quenching and tempering heat treatment by means of solid solution treatment plus aging treatment to obtain a medium entropy alloy strengthened with nano-precipitation phase and resistant to hydrogen embrittlement.

[0015] As a preferred embodiment of the method for preparing a nano-precipitated phase-reinforced hydrogen embrittlement-resistant medium entropy alloy described in the present invention, in step S1, the ingot obtained by arc melting is turned over and re-melted at least 5 times to ensure uniform distribution of elements.

[0016] As a preferred embodiment of the method for preparing a nano-precipitation phase strengthened hydrogen embrittlement resistant medium entropy alloy described in the present invention, wherein: in the step S2, the homogenization treatment temperature is 1200±50°C, and the homogenization treatment time is 3±0.2h.

[0017] As a preferred embodiment of the method for preparing a nano-precipitation phase strengthened hydrogen embrittlement resistant medium entropy alloy according to the present invention, wherein: in the step S3, the rolling reduces the thickness of the blocky medium entropy alloy ingot by 50±5%.

[0018] As a preferred embodiment of the method for preparing a nano-precipitated phase-reinforced hydrogen embrittlement-resistant medium entropy alloy according to the present invention, step S4 comprises the following steps:

[0019] S41, heating the plate to 1000±50℃ and keeping it for 1±0.05h to achieve solid solution treatment, dissolving the second phase particles that may exist in the alloy, promoting the uniform distribution of elements and reducing the grain size;

[0020] S42, the plate after solution treatment is aged at 800±50℃ for 5±0.3h to ensure sufficient precipitation of L12 phase particles;

[0021] S43. The plate after aging treatment is water quenched to quickly cool it and fix the microstructure produced by the heat treatment to prevent phase change or particle coarsening during the cooling process.

[0022] The beneficial effects of the present invention are as follows:

[0023] The present invention proposes a nano-precipitation phase strengthened hydrogen embrittlement resistant medium-entropy alloy and a preparation method thereof, wherein a medium-entropy alloy with highly dispersed nano-scale L12 phase precipitation is obtained by arc melting and homogenization treatment plus cold rolling and aging treatment, so as to achieve strength-toughness matching of the medium-entropy alloy and greatly improve the hydrogen embrittlement resistance of the material during service, which has far-reaching significance for improving the comprehensive properties such as material strengthening and hydrogen embrittlement resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0025] Figure 1 The statistics and distribution of the dispersed L12 phase size of the samples of Example 1 and Comparative Example 1 of the present invention under a transmission electron microscope;

[0026] Figure 2 The mechanical properties diagram of the samples of Example 1 and Comparative Example 1 of the present invention;

[0027] Figure 3 It is the desorption peak (TDS) diagram of the samples of Example 1 and Comparative Example 1 of the present invention after hydrogenation.

[0028] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0029] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] The present invention proposes a nano-precipitated phase-reinforced hydrogen embrittlement-resistant medium-entropy alloy and a preparation method thereof. The introduction of precipitated phases is an effective method for preventing and controlling hydrogen embrittlement, and the academic community has achieved some results in the study of precipitated phases. As a precipitated phase, the L12 phase has a coherent interface with the matrix, which can effectively hinder the movement of dislocations, improve the yield strength of the alloy, and cause dislocations to accumulate during the tensile process, thereby improving the ultimate tensile strength of the alloy. In addition, the L12 phase can capture hydrogen atoms in the alloy matrix, thereby reducing the concentration of diffusible hydrogen in the alloy, which helps to reduce hydrogen-induced stress concentration and hydrogen embrittlement risks. Therefore, the L12 phase plays a key role in improving the performance of the medium-entropy alloy, not only improving the strength and toughness of the alloy, but also significantly improving its hydrogen embrittlement resistance, which is of great significance for the application of the alloy in harsh environments. The segregation of B atoms at the grain boundary changes the diffusion behavior and stress concentration of hydrogen, while the precipitation of the L12 phase directly reduces the risk of hydrogen embrittlement by capturing hydrogen atoms. The combination of the two provides the alloy with better hydrogen embrittlement resistance. Therefore, it is particularly important to design the process of nano-precipitated phase-reinforced hydrogen embrittlement-resistant medium-entropy alloy based on the above concept. Through arc melting and a series of homogenization treatments plus cold rolling and aging treatments, highly dispersed nano-scale L12 phase precipitation is obtained to achieve alloy strength and toughness matching and greatly improve the material's resistance to hydrogen embrittlement during service. This has far-reaching significance for improving comprehensive properties such as material strengthening and hydrogen embrittlement resistance.

[0031] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0032] Example 1

[0033] A method for preparing a nano-precipitated phase-reinforced hydrogen embrittlement-resistant medium-entropy alloy comprises the following steps:

[0034] S1. According to medium entropy alloy (CoCrNi) 96 Al 1.8 Ti 1.8 B 0.4 Composition (in mass percentage, including: Co33.87%; Ni 33.74%; Cr 29.88%; Ti 1.58%; Al 0.88%; B 0.05%, the balance being inevitable impurities) Raw materials are taken and a medium entropy alloy ingot is obtained by arc melting in an argon atmosphere; the ingot obtained by arc melting is turned over and re-melted 5 times to ensure uniform distribution of elements;

[0035] S2. The ingot is subjected to homogenization treatment to adjust the element distribution; the homogenization temperature is 1200°C and the homogenization time is 3h;

[0036] S3, the ingot is rolled by cold rolling process to obtain a plate; the rolling reduces the thickness of the blocky medium entropy alloy ingot by 50%;

[0037] S4. The plate is subjected to tempering heat treatment by solution treatment plus aging treatment. The plate is heated to 1000°C and kept for 1 hour to achieve solution treatment. The plate after solution treatment is aged at 800°C for 5 hours. The plate after aging treatment is water quenched to obtain a nano-precipitation phase-reinforced hydrogen embrittlement-resistant medium entropy alloy.

[0038] Comparative Example 1

[0039] The difference from Example 1 is that no aging treatment is performed in step S4.

[0040] Figure 1 A series of microscopic images show the microstructure of CoCrNi-based medium-entropy alloys under different treatment conditions:

[0041] Figure 1 A in the middle is a BF image: a bright field image under a transmission electron microscope, showing the microstructure of the sample of comparative example 1 (ATB-S);

[0042] Figure 1 Middle b is HRTEM image: High-resolution transmission electron microscope image, which further magnifies the details of the alloy of the comparative example 1 sample;

[0043] Figure 1 c in the figure is SAED: selected area electron diffraction pattern, used to determine crystal structure and orientation;

[0044] Figure 1 (d) is a HAADF image: a high-angle annular dark field image, which particularly shows the distribution of the alloy L12 particles of the sample of Example 1 (ATB-SA), and an illustration of the particle size distribution;

[0045] Figure 1 (e) STEM-EDS: Scanning transmission electron microscopy-energy dispersive X-ray spectroscopy, showing the distribution of elements in L12 particles and FCC matrix;

[0046] Figure 1 f in the figure is SAED: the selected area electron diffraction pattern of the sample in Example 1 is shown again, proving the existence of L12 particles;

[0047] Figure 1 Figure g is HRTEM: showing the high-resolution image of L12 particles in the alloy sample of Example 1;

[0048] Figure 1 Image h in the middle is the interface structure: it shows the interface between L12 particles and the FCC matrix, showing a completely coherent structure.

[0049] In the sample of Example 1, a large number of dispersed nanoscale L12 precipitates were observed by transmission electron microscopy (TEM). These L12 phases have a very fine and uniform size distribution, with an average particle size of 22.2±4.5nm. These particles are clearly visible in the high-angle annular dark field (HAADF) image, and the high-resolution transmission electron microscopy (HRTEM) image confirms that there is a completely coherent interface between them and the face-centered cubic (FCC) matrix. This coherent interface indicates that the lattice mismatch between the L12 particles and the matrix is ​​very small, which helps to improve the strength of the alloy without introducing additional stress concentration, thereby not reducing the toughness of the material.

[0050] Figure 2 The figure is a mechanical property diagram of the samples of Example 1 and Comparative Example 1, showing the comparison of mechanical properties between the sample of Example 1 and the sample of Comparative Example 1 (without aging treatment):

[0051] Figure 2 a in the figure is an engineering stress-strain curve: it shows the stress-strain behavior of the alloys of the comparative example 1 sample and the example 1 sample after hydrogen pre-charging without hydrogen and after 24h and 72h hydrogen pre-charging;

[0052] Figure 2 Figure b is the true stress-strain curve: it further shows the relationship between true stress and true strain under the same conditions;

[0053] Figure 2 Figure c is the strain hardening rate curve: it shows the change in strain hardening rate of the two alloys during the stretching process.

[0054] The sample of Example 1 exhibits a significantly improved yield strength of about 780.8 MPa, which is much higher than the yield strength of the sample of Comparative Example 1 (about 386.5 MPa), and the ductility of the sample of Example 1 is 39.5%, while the ductility of the sample of Comparative Example 1 is 60.7%, and the ductility has only decreased by 35.9%. This significant strengthening effect is attributed to the dispersion strengthening effect of L12 particles. It is worth noting that although the strength of the sample of Example 1 is improved, its hydrogen embrittlement sensitivity index (IHE) does not increase, which is contrary to the trend that strength improvement is usually accompanied by increased hydrogen embrittlement sensitivity in conventional materials. This result shows that the introduction of L12 particles through optimized aging treatment can improve the strength of the alloy without sacrificing hydrogen embrittlement resistance.

[0055] Figure 3 The desorption peak (TDS) diagram of the samples of Example 1 and Comparative Example 1 after hydrogen charging is shown, showing the hydrogen desorption behavior of the samples of Example 1 and Comparative Example 1 after hydrogen pre-charging treatment:

[0056] Figure 3Figure a is a TDS curve: it shows the TDS analysis results of the alloys of the comparative example 1 sample and the example 1 sample after 72 hours of hydrogen pre-charging, using a heating rate of 100°C / h;

[0057] Figure 3 Figure b is the decomposition and fitting of the TDS spectrum of the sample in Example 1: The TDS spectrum of the sample alloy in Example 1 was decomposed to identify the hydrogen release peaks at different temperatures, which helps to understand the hydrogen capture capabilities of different trap sites.

[0058] After 72 hours of hydrogen pre-charging, the hydrogen capture capacity of the sample in Example 1 is 18.5 ppm, which is much lower than 28.8 ppm of the sample in Comparative Example 1. A high-temperature desorption peak related to L12 particles appears at 191°C, and the hydrogen diffusion rate in the material decreases, indicating that the L12 particles effectively capture hydrogen, reduce the diffusion of hydrogen in the alloy, and reduce the risk of hydrogen embrittlement.

[0059] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A nano-precipitate phase strengthened hydrogen embrittlement resistant medium entropy alloy, characterized in that: Calculated by mass percentage, it includes: Co 33.30-34.30%; Ni 33.20-34.20%; Cr 29.45-30.45%; Ti 1.30-1.90%; Al 0.65-1.05%; B 0.04-0.06%, and the balance is inevitable impurities.

2. The nano-precipitation phase strengthened hydrogen embrittlement resistant medium entropy alloy according to claim 1, characterized in that: The microstructure of the medium-entropy alloy is an FCC solid solution structure composed of Co, Cr, Ni in equiatomic ratios and a small amount of Al and Ti, and a nanoscale L12 precipitate phase dispersed in the matrix.

3. The nano-precipitation phase strengthened hydrogen embrittlement resistant medium entropy alloy according to claim 1, characterized in that: The average size of the nanoscale L12 precipitate phase is 17.5-27.0 nm.

4. The nano-precipitation phase strengthened hydrogen embrittlement resistant medium entropy alloy according to claim 1, characterized in that: The yield strength of the nano-precipitation phase strengthened hydrogen embrittlement resistant medium entropy alloy is ≥780MPa, the ductility is ≥39.0%, the hydrogen embrittlement sensitivity index is ≤4.5% after 24 hours of hydrogen pre-charging, and the hydrogen embrittlement sensitivity index is ≤9.5% after 72 hours of hydrogen pre-charging.

5. A method for preparing a nano-precipitate phase-reinforced hydrogen embrittlement-resistant medium entropy alloy according to any one of claims 1 to 4, characterized in that: The steps include: S1. Take raw materials according to the composition of the medium-entropy alloy, and obtain a medium-entropy alloy ingot by arc melting in an argon atmosphere; S2, the ingot is homogenized to adjust the element distribution; S3, the ingot is rolled by cold rolling process to obtain a plate; S4. The plate is subjected to quenching and tempering heat treatment by means of solid solution treatment plus aging treatment to obtain a nano-precipitation phase-reinforced hydrogen embrittlement-resistant medium entropy alloy.

6. The method for preparing a nano-precipitated phase-reinforced hydrogen embrittlement-resistant medium entropy alloy according to claim 5, characterized in that: In the step S1, the ingot obtained by arc melting is turned over and remelted at least 5 times to ensure uniform distribution of elements.

7. The method for preparing a nano-precipitated phase-reinforced hydrogen embrittlement-resistant medium entropy alloy according to claim 5, characterized in that: In the step S2, the homogenization temperature is 1200±50° C., and the homogenization time is 3.0±0.2 h.

8. The method for preparing a nano-precipitated phase-reinforced hydrogen embrittlement-resistant medium entropy alloy according to claim 5, characterized in that: In the step S3, the rolling reduces the thickness of the massive medium entropy alloy ingot by 50±5%.

9. The method for preparing a nano-precipitated phase-reinforced hydrogen embrittlement-resistant medium entropy alloy according to claim 5, characterized in that: The step S4 comprises the following steps: S41, heating the plate to 1000±50℃ and keeping it at that temperature for 1±0.05h to achieve solution treatment; S42, the plate after solution treatment is subjected to aging treatment at 800±50℃ for 5±0.3h; S43. The plate after aging treatment is water quenched to obtain a nano-precipitate phase-reinforced hydrogen embrittlement-resistant medium entropy alloy.

Citation Information

Patent Citations

  • High-toughness medium entropy high temperature alloy and preparing method thereof

    CN111500917A

  • Coherent nanophase-reinforced medium-entropy alloy with excellent thermal stability and preparation method of coherent nanophase-reinforced medium-entropy alloy

    CN114807718A

  • Medium-entropy alloy and preparation method and application thereof

    CN115725887A

  • High-entropy alloy with high strength at room temperature and high temperature as well as preparation method and application of high-entropy alloy

    CN116574953A

  • Preparation method of high-strength hydrogen-damage-resistant medium-entropy alloy, medium-entropy alloy and application of medium-entropy alloy

    CN117144167A