Low-temperature high-toughness drill rod joint and preparation method thereof
By using specific chemical composition and processes in drill pipe joints, the problems of drill pipe joint performance and quality control in low temperature environments of -40℃ are solved, and the effects of high yield strength and low-temperature impact toughness are achieved, improving the safety of drill pipe joints performance and performance.
Patent Information
- Application Number
- CN202310587233.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-23
AI Technical Summary
The existing drill pipe joints have difficulty in performance and quality control in low temperature environments of -40℃, and there is no upper limit requirement for tensile strength, which poses safety hazards.
Drill pipe joint materials with specific chemical composition ratios, including microalloyed elements such as C, Si, Mn, Cr, Ni, Mo, Nb, Ti, B, Al, Ca, etc., through steelmaking, continuous casting, perforation hot continuous rolling , die forging and heat treatment processes to prepare drill pipe joints with high yield strength and low temperature impact toughness.
It realizes the high strength and toughness performance of drill pipe joints in an environment of -40℃, meets the safety requirements in extremely low temperature environments, and improves the performance and quality control of drill pipe joints.
Smart Images

Figure CN119020677A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of drill rod materials, in particular to a low-temperature high-toughness drill rod joint and a preparation method thereof. Background Art
[0002] The winter ambient temperature of oil fields in cold regions is as low as -40℃. Winter operations require low-temperature toughness of drill pipes to meet the needs of safe production. Drill pipes are usually connected by friction welding of pipe bodies and joints. Drill pipe joints are an important part of drill pipes. Extreme low-temperature oil and gas production conditions place higher requirements on the strength, low-temperature toughness and safety and reliability of drill pipe joints.
[0003] At present, ISO, API and my country's national standards only put forward requirements for the toughness of drill pipes at -20℃, and domestic and foreign drill pipe manufacturers mainly produce drill pipes that can meet the -20℃ low temperature working environment. The relevant patents also mainly involve drill pipes of various steel grades used in -20℃ low temperature working environments. In addition, in the relevant standards, the yield strength range of drill pipe joints is too large, and there is no upper limit requirement for tensile strength, which brings difficulties to the performance and quality control of drill pipe joints and drill pipes, and will bring safety hazards in use. Summary of the invention
[0004] The object of the present invention is to provide a method for overcoming the problems of performance and quality control of drill pipe joints in a low temperature environment of -40°C in the prior art.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A low-temperature high-toughness drill pipe joint, the chemical composition of the joint is, by mass percentage, C: 0.37%-0.42%, Si: 0.20%-0.35%, Mn: 1.15%-1.25%, P≤0.015%, S≤0.005%, Cr: 0.95%-1.15%, Ni: 1.05%-1.25%, Mo: 0.20%-0.30%, Nb: 0.03%-0.05%, Ti: 0.01%-0.03%, B: 0.0005%-0.0010%, Al: 0.005%-0.010%, Ca: 0.005%-0.010%, O≤0.002%, H≤0.00015%, N≤0.003%, and the balance is Fe and unavoidable impurities.
[0007] Preferably, the room temperature yield strength of the drill pipe joint is 827-965MPa, the tensile strength is 965-1103MPa, and the elongation is ≥15%; the longitudinal Charpy impact toughness at -20°C is ≥100J, and the transverse Charpy impact toughness is ≥85J; the longitudinal Charpy impact toughness at -40°C is ≥90J, and the transverse Charpy impact toughness is ≥75J.
[0008] A method for preparing a low-temperature high-toughness drill pipe joint, based on the above joint, comprises the following steps:
[0009] S1: Steelmaking is performed according to the proportion of ingredients to obtain molten steel;
[0010] S2: Casting the molten steel into a rod-shaped continuous casting billet;
[0011] S3: Punching and hot rolling the continuous casting billet to obtain a thick-walled tube;
[0012] S4: performing die forging treatment on the thick-walled pipe to obtain a drill pipe joint blank;
[0013] S5: rough machining and heat treatment of the drill pipe joint blank to obtain a preliminary drill pipe joint;
[0014] S6: Finish and thread the preliminary drill pipe joint to obtain the drill pipe joint, and weld a wear-resistant belt on the outer diameter of the final drill pipe joint.
[0015] Preferably, when casting the molten steel into a rod-shaped continuous casting billet, electromagnetic stirring and soft reduction technology are used to control the segregation in the continuous casting billet.
[0016] Preferably, the piercing and hot rolling are specifically as follows: the continuous casting billet is heated in an annular heating furnace with a heating furnace temperature of 1150°C to 1200°C for 90 to 120 minutes, hot pierced at 1050°C to 1150°C, hot rolled at 950°C to 1150°C, then cooled to form a thick-walled tube, and the thick-walled tube is sawed.
[0017] Preferably, the die forging is specifically to heat the thick-walled tube to 1150°C-1200°C, keep it warm for 60-90 minutes, perform rough forging at 1120°C-1170°C, perform fine forging at 830°C-880°C, control the forging ratio to be ≥3, and air-cool after forging to obtain a drill pipe joint blank.
[0018] Preferably, the rough machining and heat treatment are specifically as follows: rough machining the forged drill pipe joint blank, leaving a machining allowance of 1 to 3 mm, and then heat treating it, using a heat treatment process of heating in a protective atmosphere furnace, quenching + high temperature tempering to obtain a preliminary drill pipe joint.
[0019] Preferably, the heat treatment process of quenching + high temperature tempering is specifically as follows: the quenching heating temperature is controlled at 850°C to 860°C, the holding time is 40 to 60 minutes, and then quenching is performed. The quenching cooling medium is PAG quenching liquid, and the quenching liquid temperature is controlled at 20°C to 40°C to ensure that all martensitic structures are basically obtained after quenching. The tempering temperature is controlled at 600°C to 620°C, the tempering time is 90 to 120 minutes, and tempered troostite is obtained with a grain size of 8 to 9, and water cooling is performed after tempering.
[0020] Preferably, the method comprises performing non-destructive testing on the preliminary drill pipe joint after water cooling.
[0021] Compared with the prior art, the present invention has the following beneficial effects: the present invention provides a low-temperature high-toughness drill pipe joint, wherein C is controlled within the range of 0.37% to 0.42% to ensure the hardenability, strength and toughness of the steel, Mn is controlled within the range of 1.15% to 1.25%, Cr is controlled within the range of 0.95% to 1.15%, Ni is controlled within the range of 1.05% to 1.25%, all of which are used to improve the hardenability of the steel, Mo is controlled within the range of 0.20% to 0.30%, which is used to improve the hardenability of the steel to improve the strength and tempering stability, Nb is controlled within the range of 0.03% to 0.05%, Ti is controlled within the range of 0.01% to 0.03%, B is controlled within the range of 1.15% to 1.25%, Cr is controlled within the range of 0.95% to 1.15%, Ni is controlled within the range of 1.05% to 1.25%, all of which are used to improve the hardenability of the steel, Mo is controlled within the range of 0.20% to 0.30%, which is used to improve the hardenability of the steel to improve the strength and tempering stability, Nb is controlled within the range of 0.03% to 0.05%, Ti is controlled within the range of 0.01% to 0.03%, and In the range of 0.0005% to 0.0010%, the strength and toughness of steel are improved. Al is controlled in the range of 0.005% to 0.010%, and it forms oxides with oxygen to play a deoxidation role. It forms nitrides with nitrogen to partially eliminate the adverse effects of N, and at the same time plays a role in refining grains, improving strength and toughness. Ca is controlled in the range of 0.005% to 0.010%, which improves the properties and morphology of inclusions, thereby improving the toughness of steel. Nb is added to steel to form NbC and NbN with C and N in steel, and Ti is added to steel to form TiC and TiN with C and N in steel, which have the effect of hindering the growth of austenite grains and refining grains, thereby improving strength and toughness. Such material ratio greatly improves the performance and quality of drill pipe joints.
[0022] At the same time, the present invention provides a method for preparing a low-temperature high-toughness drill pipe joint. Through multiple steps, the preparation of the drill pipe joint is completed to meet the use requirements in a -40°C environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The present invention is a flow chart of a method for preparing a low-temperature high-toughness drill pipe joint. DETAILED DESCRIPTION
[0024] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0025] In order to overcome the shortcomings or deficiencies of existing drill pipe joint steel design and its production and manufacturing technology, a low-temperature high-toughness drill pipe joint with a yield strength of 827-965MPa and a -40℃ Charpy impact toughness ≥90J and a preparation method thereof are provided.
[0026] In order to meet the comprehensive requirements of drill pipe joint strength, plasticity, low-temperature toughness, welding applicability, etc., its chemical composition and preparation process must be reasonably designed.
[0027] In terms of composition design, the present invention intends to use C, Mn, Cr, Ni, Mo, B, V, Ti microalloying, control harmful elements such as P, S, O, H, N in steel, use Al and Si for full deoxidation, and perform Ca treatment on the molten steel. The functions and content ranges of the main elements are as follows:
[0028] C: It is a strengthening element in steel, but too low carbon content is not conducive to improving the hardenability of steel and the strength of steel; too high carbon content is not conducive to the toughness of steel. It should be controlled within the range of 0.37% to 0.42%.
[0029] Si: It is a common element in steel and is controlled within the range of 0.20% to 0.35%.
[0030] Mn: Mainly used to improve the hardenability of steel, thereby increasing strength. Controlled within the range of 1.15% to 1.25%.
[0031] Cr: Mainly used to improve the hardenability of steel, thereby increasing strength. Controlled within the range of 0.95% to 1.15%.
[0032] Ni: Mainly used to improve the hardenability of steel, thereby increasing strength. Controlled within the range of 1.05% to 1.25%.
[0033] Mo: Mainly used to improve the hardenability of steel to increase strength and tempering stability. Controlled within the range of 0.20% to 0.30%.
[0034] Nb: Added into steel to form NbC and NbN with C and N in steel, it has the function of hindering the growth of austenite grains and refining grains, thereby improving strength and toughness. Controlled within the range of 0.03% to 0.05%.
[0035] Ti: added to steel to form TiC and TiN with C and N in steel, which has the effect of hindering the growth of austenite grains and refining grains, thereby improving strength and toughness. Controlled within the range of 0.01% to 0.03%.
[0036] B: Adding it to steel can significantly improve the hardenability of the steel and thus increase the strength of the steel, but too high a content will cause boron embrittlement. Control it within the range of 0.0005% to 0.0010%.
[0037] Al: It is an important deoxidizer. It forms oxides with oxygen to deoxidize, and forms nitrides with nitrogen to partially eliminate the adverse effects of N. It also refines grains and improves strength and toughness. The content is controlled within the range of 0.005% to 0.010%.
[0038] Ca: It can improve the properties and morphology of inclusions, thereby increasing the toughness of steel. It should be controlled within the range of 0.005% to 0.010%.
[0039] P: Harmful element, mainly affects the plasticity and toughness of steel. Control P≤0.015%.
[0040] S: Harmful element, mainly affects the plasticity, toughness and corrosion resistance of steel. Control S≤0.005%.
[0041] O: Harmful element, mainly affects the plasticity, toughness and corrosion resistance of steel. Control O≤0.002%.
[0042] H: Harmful element, mainly affects the plasticity and toughness of steel. Control H≤0.00015%.
[0043] N: Harmful element, mainly affects the plasticity and toughness of steel. Control N≤0.003%.
[0044] In summary, the chemical composition of the drill pipe joint is by mass percentage: C: 0.37% ~ 0.42%, Si: 0.20% ~ 0.35%, Mn: 1.15% ~ 1.25%, P ≤ 0.015%, S ≤ 0.005%, Cr: 0.95% ~ 1.15%, Ni: 1.05% ~ 1.25%, Mo: 0.20% ~ 0.30%, Nb: 0.03% ~ 0.05%, Ti: 0.01% ~ 0.03%, B: 0.0005% ~ 0.0010%, Al: 0.005% ~ 0.010%, Ca: 0.005% ~ 0.010%, O ≤ 0.002%, H ≤ 0.00015%, N ≤ 0.003%, the balance is Fe and unavoidable impurities.
[0045] In terms of the preparation process of drill pipe joints, the main processes are steelmaking (including refining outside the furnace, vacuum degassing), continuous casting, hot rolling in the austenite zone, die forging, quenching and tempering heat treatment, etc., so that the material can obtain a fine and uniform tempered sorbite microstructure to achieve a reasonable match between the strength and plastic toughness of the drill pipe joints.
[0046] Preparation process of low temperature and high toughness petroleum drill pipe joint:
[0047] ① Steelmaking: batching, electric furnace or oxygen-blown converter steelmaking, refining outside the furnace and vacuum degassing to obtain the above chemical composition, feeding Si-Ca wire to modify the inclusions in the steel.
[0048] ②Continuous casting: The molten steel is cast into rod-shaped continuous casting billets. During the continuous casting process, electromagnetic stirring and light pressure reduction technology are used to control the segregation in the continuous casting billets.
[0049] ③Piercing and hot rolling: Heat the continuous casting billet in a ring-shaped heating furnace at a temperature of 1150°C to 1200°C for 90 to 120 minutes, hot pierce at 1050°C to 1150°C, hot roll at 950°C to 1150°C, and then cool to make a thick-walled tube, which is sawn to a suitable length.
[0050] ④ Die forging: Heat the thick-walled tubular raw material to 1150℃~1200℃, keep warm for 60~90 minutes, rough forge at 1120℃~1170℃, fine forge at 830℃~880℃, control the forging ratio ≥3, and air cool after forging.
[0051] ⑤ Rough machining and heat treatment: Rough machining of the forged drill pipe joint blank is carried out in accordance with national standards, with a machining allowance of 1 to 3 mm, and then heat treatment is carried out. A heat treatment process of heating in a protective atmosphere furnace (to prevent decarburization), quenching + high-temperature tempering is adopted. The quenching heating temperature is controlled at 850℃~860℃, the holding time is 40 to 60 minutes, and then quenching is performed. The quenching cooling medium is PAG quenching liquid, and the quenching liquid temperature is controlled at 20℃~40℃ to ensure that all martensitic structures are basically obtained after quenching; the tempering temperature is controlled at 600℃~620℃, and the tempering time is 90 to 120 minutes to obtain fine and uniform tempered troostite with a grain size of 8 to 9. After tempering, water cooling is performed to avoid possible temper brittleness. Non-destructive testing is then performed.
[0052] ⑥ Finishing and thread processing: According to standards and user requirements, the drill pipe joints are finished, API standard threads or special threads are processed, and magnetic particle inspection is performed on the threads.
[0053] The present invention has the following performance characteristics: the low-temperature high-toughness drill pipe joint material of the present invention has excellent comprehensive performance after appropriate preparation process, room temperature yield strength of 827-965MPa, tensile strength of 965-1103MPa, elongation ≥15%; -20℃ longitudinal Charpy impact toughness ≥100J, transverse Charpy impact toughness ≥85J; -40℃ longitudinal Charpy impact toughness ≥90J, transverse Charpy impact toughness ≥75J. It can meet the requirements of extreme low temperature environment for the safety of oil drill pipe joints.
[0054] Example 1
[0055] The chemical composition of the low-temperature and high-toughness petroleum drill pipe joint material provided by the embodiment of the present invention is C: 0.42%, Si: 0.35%, Mn: 1.25%, P: 0.010%, S: 0.003%, Cr: 1.15%, Mo: 0.3%, Ni: 1.25%, Nb: 0.039%, Ti: 0.021%, B: 0.001%, Ca: 0.005%, Al0.007%, O: 0.002%, H: 0.00015%, N: 0.003%, and the balance is Fe and unavoidable impurities.
[0056] The embodiment of the present invention also provides a method for preparing a low-temperature high-toughness drill pipe joint, comprising the following steps:
[0057] ① Steelmaking: batching, electric furnace steelmaking, refining outside the furnace and vacuum degassing to obtain the above chemical composition, and modify the inclusions in the steel with Si-Ca wire.
[0058] ②Continuous casting: The molten steel is cast into rod-shaped continuous casting billets. During the continuous casting process, electromagnetic stirring and light pressure reduction technology are used to control the segregation in the continuous casting billets.
[0059] ③Piercing and hot rolling: Heat the continuous casting billet in a ring-shaped heating furnace with a heating furnace temperature of 1150°C and a heating time of 120 minutes. Hot piercing is performed at 1150°C, hot rolling is performed at 1150°C, and then cooling is performed to form a thick-walled tube, which is sawn to a suitable length.
[0060] ④ Die forging: Heat the thick-walled tubular raw material to 1200℃, keep it warm for 90 minutes, rough forge at 1170℃, fine forge at 880℃, control the forging ratio to 3, and air cool after forging.
[0061] ⑤ Rough machining and heat treatment: Rough machining is performed on the forged drill pipe joint blank, leaving a machining allowance of 1mm, and then heat treatment is performed. A heat treatment process of heating in a protective atmosphere furnace (to prevent decarburization), quenching + high-temperature tempering is used. The quenching heating temperature is 860°C, the holding time is 60 minutes, and then quenching is performed. The quenching cooling medium is PAG quenching liquid. The quenching liquid temperature is controlled to be 40°C, and the time from the quenching heating temperature to the quenching medium is 5s to ensure that all martensitic structures are basically obtained after quenching; the tempering temperature is 620°C, and the tempering time is 90 minutes to obtain fine and uniform tempered troostite, with a grain size of 9. After tempering, water cooling is performed to avoid possible temper brittleness. Nondestructive testing is then performed.
[0062] ⑥ Finishing and thread processing: According to standards and user requirements, the drill pipe joints are finished, API standard threads or special threads are processed, and magnetic particle inspection is performed on the threads.
[0063] The performance of the oil drill pipe joint prepared according to the above composition and process: room temperature yield strength 943MPa, tensile strength greater than 1069MPa, elongation 25%; -20℃ longitudinal Charpy impact toughness 136J, transverse Charpy impact toughness 116J; -40℃ longitudinal Charpy impact toughness 125J, transverse Charpy impact toughness 106J. It has the characteristics of high strength and high and low temperature toughness, and can meet the safety requirements of oil drill pipe joints in -40℃ low temperature environment.
[0064] Example 2
[0065] The chemical composition of the low-temperature and high-toughness petroleum drill pipe joint material provided in Example 2 of the present invention is C: 0.41%, Si: 0.20%, Mn: 1.15%, P: 0.011%, S: 0.002%, Cr: 0.97%, Mo: 0.2%, Ni: 1.05%, Nb: 0.030%, Ti: 0.030%, B: 0.005%, Ca: 0.007%, Al0.008%, O: 0.001%, H: 0.00015%, N: 0.003%, and the remainder is Fe and unavoidable impurities.
[0066] Embodiment 2 of the present invention also provides a method for preparing a low-temperature high-toughness drill pipe joint, comprising the following steps:
[0067] ① Steelmaking: batching, oxygen-blown converter steelmaking, refining outside the furnace and vacuum degassing to obtain the above chemical composition, and modify the inclusions in the steel to Si-Ca wire.
[0068] ②Continuous casting: The molten steel is cast into rod-shaped continuous casting billets. During the continuous casting process, electromagnetic stirring and light pressure reduction technology are used to control the segregation in the continuous casting billets.
[0069] ③Piercing and hot rolling: Heat the continuous casting billet in a ring-shaped heating furnace at a temperature of 1200°C for 100 minutes, perform hot piercing at 1100°C, perform hot rolling at 1050°C, and then cool it to form a thick-walled tube, which is then sawn to a suitable length.
[0070] ④ Die forging: Heat the thick-walled tubular raw material to 1175℃, keep it warm for 70 minutes, rough forge at 1140℃, fine forge at 850℃, control the forging ratio to 4, and air cool after forging.
[0071] ⑤ Rough machining and heat treatment: Rough machining is performed on the forged drill pipe joint blank, leaving a machining allowance of 2mm, and then heat treatment is performed. A heat treatment process of heating in a protective atmosphere furnace, quenching + high-temperature tempering is used. The quenching heating temperature is 854°C, the holding time is 50 minutes, and then quenching is performed. The quenching cooling medium is PAG quenching liquid. The quenching liquid temperature is controlled to be 30°C, and the time from the quenching heating temperature to the quenching medium is 3s to ensure that all martensitic structures are basically obtained after quenching; the tempering temperature is 610°C, and the tempering time is 110 minutes to obtain fine and uniform tempered troostite, with a grain size of 8. After tempering, water cooling is performed to avoid possible temper brittleness. Nondestructive testing is then performed.
[0072] ⑥ Finishing and thread processing: According to standards and user requirements, the drill pipe joints are finished, API standard threads or special threads are processed, and magnetic particle inspection is performed on the threads.
[0073] The performance of the oil drill pipe joint prepared according to the above composition and process is as follows: room temperature yield strength 923MPa, tensile strength greater than 1048MPa, elongation 24%; -20℃ longitudinal Charpy impact toughness 129J, transverse Charpy impact toughness 110J; -40℃ longitudinal Charpy impact toughness 118J, transverse Charpy impact toughness 100J. It has the characteristics of high strength and high and low temperature toughness, and can meet the requirements of -40℃ low temperature environment for the safety of oil drill pipe joints.
[0074] Example 3
[0075] The chemical composition of the low-temperature and high-toughness petroleum drill pipe joint material provided in Example 3 of the present invention is C: 0.38%, Si: 0.29%, Mn: 1.19%, P: 0.013%, S: 0.002%, Cr: 1.10%, Mo: 0.24%, Ni: 1.11%, Nb: 0.034%, Ti: 0.016%, B: 0.006%, Ca: 0.006%, Al0.005%, O: 0.002%, H: 0.0001%, N: 0.002%, and the remainder is Fe and unavoidable impurities.
[0076] Embodiment 3 of the present invention also provides a method for preparing a low-temperature high-toughness drill pipe joint, comprising the following steps:
[0077] ① Steelmaking: batching, electric furnace steelmaking, refining outside the furnace and vacuum degassing to obtain the above chemical composition, and modify the inclusions in the steel with Si-Ca wire.
[0078] ②Continuous casting: The molten steel is cast into rod-shaped continuous casting billets. During the continuous casting process, electromagnetic stirring and light pressure reduction technology are used to control the segregation in the continuous casting billets.
[0079] ③Piercing and hot rolling: Heat the continuous casting billet in a ring-shaped heating furnace at a temperature of 1200°C for 90 minutes, hot pierce at 1050°C, hot roll at 950°C, and then cool to make a thick-walled tube, which is sawn to a suitable length.
[0080] ④ Die forging: Heat the thick-walled tubular raw material to 1150℃, keep it warm for 60 minutes, rough forge at 1120℃, fine forge at 830℃, control the forging ratio to 4, and air cool after forging.
[0081] ⑤ Rough machining and heat treatment: Rough machining is performed on the forged drill pipe joint blank, leaving a machining allowance of 3mm, and then heat treatment is performed. A heat treatment process of heating in a protective atmosphere furnace, quenching + high-temperature tempering is used. The quenching heating temperature is 850°C, the holding time is 50 minutes, and then quenching is performed. The quenching cooling medium is PAG quenching liquid. The quenching liquid temperature is controlled to be 40°C, and the time from the quenching heating temperature to the quenching medium is 4s to ensure that all martensitic structures are basically obtained after quenching; the tempering temperature is 600°C, and the tempering time is 90 minutes to obtain fine and uniform tempered troostite, with a grain size of 9. After tempering, water cooling is performed to avoid possible temper brittleness. Nondestructive testing is then performed.
[0082] ⑥ Finishing and thread processing: According to standards and user requirements, the drill pipe joints are finished, API standard threads or special threads are processed, and magnetic particle inspection is performed on the threads.
[0083] The performance of the oil drill pipe joint prepared according to the above composition and process is as follows: room temperature yield strength 928MPa, tensile strength greater than 1054MPa, elongation 24%; -20℃ longitudinal Charpy impact toughness 127J, transverse Charpy impact toughness 108J; -40℃ longitudinal Charpy impact toughness 117J, transverse Charpy impact toughness 99J. It has the characteristics of high strength and high and low temperature toughness, and can meet the requirements of -40℃ low temperature environment for the safety of oil drill pipe joints.
[0084] Example 4
[0085] The chemical composition of the low-temperature and high-toughness petroleum drill pipe joint material provided in Example 3 of the present invention is C: 0.37%, Si: 0.24%, Mn: 1.23%, P: 0.011%, S: 0.003%, Cr: 1.01%, Mo: 0.28%, Ni: 1.16%, Nb: 0.05%, Ti: 0.010%, B: 0.009%, Ca: 0.010%, Al0.009%, O: 0.003%, H: 0.0001%, N: 0.002%, and the remainder is Fe and unavoidable impurities.
[0086] Embodiment 4 of the present invention also provides a method for preparing a low-temperature high-toughness drill pipe joint, comprising the following steps:
[0087] ① Steelmaking: batching, oxygen-blown converter steelmaking, refining outside the furnace and vacuum degassing to obtain the above chemical composition, and modify the inclusions in the steel to Si-Ca wire.
[0088] ②Continuous casting: The molten steel is cast into rod-shaped continuous casting billets. During the continuous casting process, electromagnetic stirring and light pressure reduction technology are used to control the segregation in the continuous casting billets.
[0089] ③Piercing and hot rolling: Heat the continuous casting billet in a ring-shaped heating furnace with a heating furnace temperature of 1150°C and a heating time of 120 minutes. Hot piercing is performed at 1150°C, hot rolling is performed at 1150°C, and then cooling is performed to form a thick-walled tube, which is sawn to a suitable length.
[0090] ④ Die forging: Heat the thick-walled tubular raw material to 1200℃, keep it warm for 90 minutes, rough forge at 1170℃, fine forge at 880℃, control the forging ratio to 3, and air cool after forging.
[0091] ⑤ Rough machining and heat treatment: Rough machining is performed on the forged drill pipe joint blank, leaving a machining allowance of 3mm, and then heat treatment is performed. A heat treatment process of heating in a protective atmosphere furnace, quenching + high-temperature tempering is used. The quenching heating temperature is 860°C, the holding time is 60 minutes, and then quenching is performed. The quenching cooling medium is PAG quenching liquid. The quenching liquid temperature is controlled to be 40°C, and the time from the quenching heating temperature to the quenching medium is 5s to ensure that all martensitic structures are basically obtained after quenching; the tempering temperature is 620°C, and the tempering time is 120 minutes to obtain fine and uniform tempered troostite, with a grain size of 8. After tempering, water cooling is performed to avoid possible temper brittleness. Nondestructive testing is then performed.
[0092] ⑥ Finishing and thread processing: According to standards and user requirements, the drill pipe joints are finished, API standard threads or special threads are processed, and magnetic particle inspection is performed on the threads.
[0093] The performance of the oil drill pipe joint prepared according to the above composition and process is as follows: room temperature yield strength 916MPa, tensile strength greater than 1042MPa, elongation 25%; -20℃ longitudinal Charpy impact toughness 132J, transverse Charpy impact toughness 112J; -40℃ longitudinal Charpy impact toughness 123J, transverse Charpy impact toughness 105J. It has the characteristics of high strength and high and low temperature toughness, and can meet the requirements of -40℃ low temperature environment for the safety of oil drill pipe joints.
[0094] Example 5
[0095] The chemical composition of the low-temperature and high-toughness petroleum drill pipe joint material provided in Example 5 of the present invention is C: 0.40%, Si: 0.27%, Mn: 1.21%, P: 0.010%, S: 0.005%, Cr: 1.04%, Mo: 0.2:5%, Ni: 1.19%, Nb: 0.046%, Ti: 0.024%, B: 0.0008%, Ca: 0.008%, Al0.010%, O: 0.002%, H: 0.0001%, N: 0.002%, and the remainder is Fe and unavoidable impurities.
[0096] Embodiment 5 of the present invention also provides a method for preparing a low-temperature high-toughness drill pipe joint, comprising the following steps:
[0097] ① Steelmaking: batching, electric furnace steelmaking, refining outside the furnace and vacuum degassing to obtain the above chemical composition, and modify the inclusions in the steel with Si-Ca wire.
[0098] ②Continuous casting: The molten steel is cast into rod-shaped continuous casting billets. During the continuous casting process, electromagnetic stirring and light pressure reduction technology are used to control the segregation in the continuous casting billets.
[0099] ③Piercing and hot rolling: Heat the continuous casting billet in a ring-shaped heating furnace with a heating furnace temperature of 1150°C and a heating time of 120 minutes. Hot piercing is performed at 1150°C, hot rolling is performed at 1150°C, and then cooling is performed to form a thick-walled tube, which is sawn to a suitable length.
[0100] ④ Die forging: Heat the thick-walled tubular raw material to 1200℃, keep it warm for 90 minutes, rough forge at 1170℃, fine forge at 880℃, control the forging ratio to 3, and air cool after forging.
[0101] ⑤ Rough machining and heat treatment: Rough machining is performed on the forged drill pipe joint blank, leaving a machining allowance of 3mm, and then heat treatment is performed. A heat treatment process of heating in a protective atmosphere furnace, quenching + high-temperature tempering is used. The quenching heating temperature is 860°C, the holding time is 40 minutes, and then quenching is performed. The quenching cooling medium is PAG quenching liquid. The quenching liquid temperature is controlled to be 40°C, and the time from the quenching heating temperature to the quenching medium is 5s to ensure that all martensitic structures are basically obtained after quenching; the tempering temperature is 620°C, and the tempering time is 120 minutes to obtain fine and uniform tempered troostite, with a grain size of 8. After tempering, water cooling is performed to avoid possible temper brittleness. Nondestructive testing is then performed.
[0102] ⑥ Finishing and thread processing: According to standards and user requirements, the drill pipe joints are finished, API standard threads or special threads are processed, and magnetic particle inspection is performed on the threads.
[0103] The performance of the oil drill pipe joint prepared according to the above composition and process: room temperature yield strength 908MPa, tensile strength greater than 1033MPa, elongation 25%; -20℃ longitudinal Charpy impact toughness 136J, transverse Charpy impact toughness 116J; -40℃ longitudinal Charpy impact toughness 125J, transverse Charpy impact toughness 106J. It has the characteristics of high strength and high and low temperature toughness, and can meet the requirements of -40℃ low temperature environment for the safety of oil drill pipe joints.
[0104] Example 6
[0105] The chemical composition of the low-temperature and high-toughness petroleum drill pipe joint material provided in Example 6 of the present invention is C: 0.39%, Si: 0.33%, Mn: 1.20%, P: 0.015%, S: 0.002%, Cr: 0.95%, Mo: 0.26%, Ni: 1.14%, Nb: 0.040%, Ti: 0.020%, B: 0.0007%, Ca: 0.009%, Al: 0.006%, O: 0.002%, H: 0.0001%, N: 0.002%, and the remainder is Fe and unavoidable impurities.
[0106] Embodiment 6 of the present invention also provides a method for preparing a low-temperature high-toughness drill pipe joint, comprising the following steps:
[0107] ① Steelmaking: batching, oxygen-blown converter steelmaking, refining outside the furnace and vacuum degassing to obtain the above chemical composition, and modify the inclusions in the steel to Si-Ca wire.
[0108] ②Continuous casting: The molten steel is cast into rod-shaped continuous casting billets. During the continuous casting process, electromagnetic stirring and light pressure reduction technology are used to control the segregation in the continuous casting billets.
[0109] ③Piercing and hot rolling: Heat the continuous casting billet in a ring-shaped heating furnace with a heating furnace temperature of 1150°C and a heating time of 120 minutes. Hot piercing is performed at 1150°C, hot rolling is performed at 1150°C, and then cooling is performed to form a thick-walled tube, which is sawn to a suitable length.
[0110] ④ Die forging: Heat the thick-walled tubular raw material to 1200℃, keep it warm for 90 minutes, rough forge at 1170℃, fine forge at 880℃, control the forging ratio to 3, and air cool after forging.
[0111] ⑤ Rough machining and heat treatment: Rough machining is performed on the forged drill pipe joint blank, leaving a machining allowance of 3mm, and then heat treatment is performed. A heat treatment process of heating in a protective atmosphere furnace, quenching + high-temperature tempering is used. The quenching heating temperature is 860°C, the holding time is 60 minutes, and then quenching is performed. The quenching cooling medium is PAG quenching liquid. The quenching liquid temperature is controlled to be 40°C, and the time from the quenching heating temperature to the quenching medium is 5s to ensure that all martensitic structures are basically obtained after quenching; the tempering temperature is 620°C, and the tempering time is 90 minutes to obtain fine and uniform tempered troostite, with a grain size of 9. After tempering, water cooling is performed to avoid possible temper brittleness. Nondestructive testing is then performed.
[0112] ⑥ Finishing and thread processing: According to standards and user requirements, the drill pipe joints are finished, API standard threads or special threads are processed, and magnetic particle inspection is performed on the threads.
[0113] The performance of the oil drill pipe joint prepared according to the above composition and process: room temperature yield strength 943MPa, tensile strength greater than 1069MPa, elongation 23%; -20℃ longitudinal Charpy impact toughness 119J, transverse Charpy impact toughness 101J; -40℃ longitudinal Charpy impact toughness 109J, transverse Charpy impact toughness 93J. It has the characteristics of high strength and high and low temperature toughness, and can meet the safety requirements of oil drill pipe joints in -40℃ low temperature environment.
[0114] Although the embodiments of the present invention are described above in conjunction with the accompanying drawings, the present invention is not limited to the above-mentioned specific embodiments and application fields, and the above-mentioned specific embodiments are only illustrative and instructive, rather than restrictive. Under the guidance of the specification, a person skilled in the art can also make many forms without departing from the scope of protection of the claims of the present invention, all of which belong to the scope of protection of the present invention.
Claims
1. A low temperature and high toughness drill pipe joint, It is characterized in that The chemical composition of the joint is, in percentage by mass, C: 0.37% to 0.42%, Si: 0.20% to 0.35%, Mn: 1.15% to 1.25%, P≤0.015%, S≤0.005%, Cr: 0.95% to 1.15%, Ni: 1.05% to 1.25%, Mo: 0.20% to 0.30%, Nb: 0.03% to 0.05%, Ti: 0.01% to 0.03%, B: 0.0005% to 0.0010%, Al: 0.005% to 0.010%, Ca: 0.005% to 0.010%, O≤0.002%, H≤0.00015%, N≤0.003%, and the balance is Fe and unavoidable impurities.
2. A low temperature and high toughness drill pipe joint according to claim 1, It is characterized in that The room temperature yield strength of the drill pipe joint is 827~965MPa, the tensile strength is 965~1103MPa, and the elongation is ≥15%; the longitudinal Charpy impact toughness at -20℃ is ≥100J, and the transverse Charpy impact toughness is ≥85J; the longitudinal Charpy impact toughness at -40℃ is ≥90J, and the transverse Charpy impact toughness is ≥75J.
3. A method for preparing a low-temperature high-toughness drill pipe joint, based on the low-temperature high-toughness drill pipe joint according to any one of claims 1-2 It is characterized in that The following steps are involved: S1: Steelmaking is performed according to the proportion of ingredients to obtain molten steel; S2: Casting the molten steel into a rod-shaped continuous casting billet; S3: Punching and hot rolling the continuous casting billet to obtain a thick-walled tube; S4: performing die forging treatment on the thick-walled pipe to obtain a drill pipe joint blank; S5: rough machining and heat treatment of the drill pipe joint blank to obtain a preliminary drill pipe joint; S6: Finish and thread the preliminary drill pipe joint to obtain the drill pipe joint, and weld a wear-resistant belt on the outer diameter of the final drill pipe joint.
4. The method for preparing a low-temperature high-toughness drill pipe joint according to claim 3, It is characterized in that When the molten steel is cast into a rod-shaped continuous casting billet, electromagnetic stirring and soft pressure reduction technology are used to control the segregation in the continuous casting billet.
5. The method for preparing a low-temperature high-toughness drill pipe joint according to claim 3, It is characterized in that The piercing and hot rolling are specifically as follows: heating the continuous casting billet in an annular heating furnace with a heating furnace temperature of 1150°C to 1200°C for 90 to 120 minutes, hot piercing at 1050°C to 1150°C, hot rolling at 950°C to 1150°C, and then cooling to form a thick-walled tube, and sawing the thick-walled tube.
6. The method for preparing a low-temperature high-toughness drill pipe joint according to claim 3, It is characterized in that The die forging is specifically as follows: heating the thick wall pipe to 1150°C-1200°C, keeping the temperature for 60-90 minutes, rough forging at 1120°C-1170°C, fine forging at 830°C-880°C, controlling the forging ratio to be ≥3, air cooling after forging, and obtaining the drill pipe joint blank.
7. The method for preparing a low-temperature high-toughness drill pipe joint according to claim 3, It is characterized in that The rough machining and heat treatment are specifically as follows: rough machining is performed on the forged drill pipe joint blank, leaving a machining allowance of 1 to 3 mm, and then heat treatment is performed, using a protective atmosphere furnace heating, quenching + high temperature tempering heat treatment process to obtain a preliminary drill pipe joint.
8. The method for preparing a low-temperature high-toughness drill pipe joint according to claim 7, It is characterized in that The heat treatment process of quenching + high temperature tempering is specifically as follows: the quenching heating temperature is controlled at 850°C to 860°C, the holding time is 40 to 60 minutes, and then quenching is performed. The quenching cooling medium is PAG quenching liquid, and the quenching liquid temperature is controlled at 20°C to 40°C to ensure that basically all martensitic structures are obtained after quenching. The tempering temperature is controlled at 600°C to 620°C, the tempering time is 90 to 120 minutes, and tempered troostite is obtained with a grain size of 8 to 9. Water cooling is performed after tempering.
9. The method for preparing a low-temperature high-toughness drill pipe joint according to claim 8, It is characterized in that Includes non-destructive testing of preliminary drill pipe joints after water cooling.
Citation Information
Patent Citations
Automobile high-strength electric resistance welded steel pipe with excellent low-temperature impact property and method of manufacturing the same
CN101514433A
High-strength high-toughness petroleum drill pipe and production method thereof
CN103789685A
Manufacturing method of pipe for 110ksi steel level sulfide stress corrosion resisting drill rod connector
CN109868413A
Production of thick walled ultra high tension steel
JP1984129724A
Low alloy steel
US20040187971A1