Method for plating aluminum oxide film and solar cell
By inserting ozone and nitrogen into the atomic layer deposition machine to purify the surface of the silicon wafer, remove dust and generate an alumina film, it solves the problem of EL black spots caused by dust during silicon wafer transportation, and improves the solar cell Electrical performance and production line yield.
Patent Information
- Application Number
- CN202310601768.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-26
AI Technical Summary
During the manufacturing process of solar cells, when the silicon wafer is transported to the deposition aluminum oxide film process or the ALD machine to detect leakage, dust drops in the air or machine to cause the generation of EL black spots, affecting the yield of production lines.
Ozone is introduced into the chamber of the atomic layer deposition machine to purge the surface of the silicon wafer to remove dust, and an alumina film is generated on the surface of the silicon oxide film. The cleanliness of the chamber is further improved through the first nitrogen gas flow and avoid dust Attached.
Effectively remove dust on the surface of the silicon wafer, improve the situation of black spots in EL, improve the electrical performance and production line yield of solar cells, and the process is simple and cost-saving.
Smart Images

Figure CN119028805A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of photovoltaic technology, in particular to a method for plating an aluminum oxide film and a solar cell. Background Art
[0002] With the development of the photovoltaic industry and the continuous innovation of photovoltaic technology, in the manufacturing process of solar cells, the aluminum oxide film deposition process of the coating process has been gradually separated. The existing aluminum oxide film deposition process usually uses an atomic layer deposition (ALD) machine to deposit the aluminum oxide film. The tooling of the ALD machine is an aluminum boat. The silicon wafer is placed in the aluminum boat, and the aluminum boat carries the silicon wafer into the chamber of the ALD machine.
[0003] After the previous process of depositing aluminum oxide film is completed, when the silicon wafer is transported to the ALD machine of the aluminum oxide film deposition process, and when the ALD machine is leak-checking, dust in the air or in the ALD machine falls onto the surface of the silicon wafer, causing EL (Electro Luminescence) black spots, which affects the production line yield.
[0004] In the prior art, the generation of EL black spots and black dots is generally reduced by improving the cleanliness of the tooling or fixtures. Although this method can reduce the generation of EL black spots and black dots caused by the dirtiness of the tooling or fixtures, it cannot improve the situation in which dust in the air or in the ALD machine falls onto the surface of the silicon wafer during the process of transporting the silicon wafer to the ALD machine for depositing the aluminum oxide film, and during the leak detection of the ALD machine, causing the generation of EL black spots and black dots. Summary of the invention
[0005] The present invention provides a method for coating an aluminum oxide film and a solar cell, aiming to solve the problem in the prior art that during the aluminum oxide film deposition process, dust in the air or in the ALD machine falls onto the surface of the silicon wafer during the aluminum oxide film deposition process, causing EL black spots and black dots to be generated, thereby affecting the production line yield.
[0006] A first aspect of the present invention provides a method for coating an aluminum oxide film, comprising:
[0007] A silicon wafer is placed in a chamber of an atomic layer deposition machine, and after leak detection of the atomic layer deposition machine, ozone is introduced to purge the surface of the silicon wafer and form a silicon oxide film on the surface of the silicon wafer; a first nitrogen gas is introduced to purge the chamber; and an aluminum oxide film is formed on the surface of the silicon oxide film.
[0008] In the present invention, a silicon wafer is placed in the chamber of an atomic layer deposition machine, and after leak detection of the atomic layer deposition machine, ozone is introduced to purge the surface of the silicon wafer to purge and remove dust on the surface of the silicon wafer. The dust on the surface of the silicon wafer includes dust that falls from the air to the surface of the silicon wafer during transportation from the previous process to the process of depositing an aluminum oxide film, or dust that falls from the chamber of the atomic layer deposition machine to the surface of the silicon wafer when leak detection of the atomic layer deposition machine is performed. The dust mainly includes: silicon fragments and powder, dust in the air, and aluminum oxide powder remaining in the chamber of the ALD machine. During the purge of the surface of the silicon wafer, the silicon fragments and powder are oxidized into silicon oxide particles and are removed by ozone purge. Organic matter in the dust in the air undergoes a pyrolysis reaction at high temperature to produce granular carbonaceous matter, which is removed by ozone purge. Other substances other than organic matter in the dust in the air are removed by ozone purge. The aluminum oxide powder remaining in the chamber of the ALD machine is removed by ozone purge, and no film layer is formed on the surface of the silicon wafer. Ozone reacts with silicon wafers to form a silicon oxide film on the surface of the silicon wafer, which can better passivate the silicon wafer. The introduction of ozone is also used to purge other locations in the chamber other than the surface of the silicon wafer to remove dust in the chamber and improve the cleanliness of the chamber. Ozone is a commonly used reaction gas for generating aluminum oxide films. Existing ALD machines can usually be introduced with ozone. The introduction of ozone does not require additional modifications to the ALD machine, which is simple in process and saves costs. The first nitrogen gas is introduced to purge the chamber, which can remove the granular carbonaceous substances produced by the pyrolysis reaction of organic matter in the dust remaining in the chamber after the introduction of ozone, the silicon oxide particles generated after the oxidation of silicon fragments and powder, and the residual dust, further improving the cleanliness of the chamber. In addition, nitrogen has a high degree of chemical stability, is difficult to participate in chemical reactions, and will not react with silicon wafers or dust to avoid adverse effects. Nitrogen is commonly used as a carrier gas or cleaning gas for generating aluminum oxide film. Existing ALD machines can usually be fed with nitrogen. No additional modification of the ALD machine is required for the nitrogen. The process is simple and cost-effective. Then, an aluminum oxide film is generated on the surface of the silicon oxide film. Since the dust on the surface of the silicon wafer has been removed more thoroughly in the previous process, the present invention can improve the EL black spots caused by dust falling on the surface of the silicon wafer during the aluminum oxide film deposition process, thereby avoiding affecting the production line yield.
[0009] Optionally, the flow rate of the ozone is 1000 standard milliliters per minute to 2000 standard milliliters per minute.
[0010] Optionally, the time for introducing ozone is 50 seconds to 150 seconds.
[0011] Optionally, the silicon oxide film has a thickness of 1 nanometer to 3 nanometers.
[0012] Optionally, the flow rate of the first nitrogen gas is 2000 standard milliliters per minute to 5000 standard milliliters per minute, and the time for the first nitrogen gas to be introduced is 10 seconds to 30 seconds.
[0013] Optionally, after placing the silicon wafer into a chamber of an atomic layer deposition machine, the method further comprises:
[0014] A second nitrogen gas flow is performed to purge the chamber.
[0015] Optionally, the flow rate of the second nitrogen gas is 2000 standard milliliters per minute to 10000 standard milliliters per minute, and the time for the second nitrogen gas to be introduced is 20 seconds to 60 seconds.
[0016] Optionally, the step of forming an aluminum oxide film on the surface of the silicon oxide film includes:
[0017] The first step is to introduce trimethylaluminum;
[0018] In the second step, nitrogen is introduced to purge the trimethylaluminum;
[0019] The third step is to introduce ozone;
[0020] The fourth step is to introduce nitrogen to purge the ozone;
[0021] Steps 1 to 4 form a cycle;
[0022] After the one cycle, a third nitrogen gas is introduced to purge the surface of the silicon wafer.
[0023] A second aspect of the present invention provides a solar cell, comprising: a silicon wafer, a silicon oxide film located on the surface of the silicon wafer, and an aluminum oxide film located on the surface of the silicon oxide film, wherein the silicon oxide film and the aluminum oxide film are both prepared by the method for coating aluminum oxide film as described in the first aspect.
[0024] Optionally, the solar cell includes a passivated emitter and back cell technology cell, a shingled solar cell, a tunneling oxide layer passivated contact cell, and a back electrode contact silicon solar cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments of the present invention will be briefly introduced below. Obviously, the accompanying drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.
[0026] Figure 1 A flowchart showing a method for coating an aluminum oxide film according to an embodiment of the present invention is shown;
[0027] Figure 2 A flow chart showing the steps of another method for coating an aluminum oxide film in an embodiment of the present invention is shown. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] The embodiment of the present invention provides a method for coating an aluminum oxide film, referring to Figure 1 , Figure 1 A flowchart of a method for coating an aluminum oxide film in an embodiment of the present invention is shown, and the method comprises:
[0030] Step 101, placing a silicon wafer into a chamber of an atomic layer deposition machine, after leak testing the atomic layer deposition machine, introducing ozone to purge the surface of the silicon wafer and forming a silicon oxide film on the surface of the silicon wafer.
[0031] Put the silicon wafer into the chamber of the atomic layer deposition machine. Specifically, the silicon wafer can be put into an aluminum boat, and then the aluminum boat is placed on a carrier that carries the aluminum boat, and the carrier that carries the aluminum boat enters the chamber of the ALD machine. Perform a leak check on the atomic layer deposition machine to ensure the normal progress of the aluminum oxide film deposition process. Introduce ozone to purge the surface of the silicon wafer to purge and remove the dust on the surface of the silicon wafer. The dust mainly includes: silicon fragments and powder, dust in the air, and aluminum oxide powder remaining in the chamber of the ALD machine. During the purge of the surface of the silicon wafer, the silicon fragments and powder are oxidized into silicon oxide particles and are removed by ozone purge. The organic matter in the dust in the air undergoes a pyrolysis reaction at high temperature to produce granular carbonaceous substances, which are removed by ozone purge. Other substances other than organic matter in the dust in the air are removed by ozone purge. The aluminum oxide powder remaining in the chamber of the ALD machine is removed by ozone purge, and no film layer is formed on the surface of the silicon wafer. Ozone reacts with the silicon wafer to form a silicon oxide film on the surface of the silicon wafer, which can better passivate the silicon wafer. The surface of the silicon wafer can be the light-facing side of the silicon wafer and / or the backlight side. It should be noted that before the silicon wafer is placed in the chamber of the atomic layer deposition machine, if there is a silicon oxide film or other film on the surface of the silicon wafer, ozone is introduced to purge the surface of the silicon wafer, that is, to purge the silicon oxide film or other film on the surface of the silicon wafer, and a silicon oxide film is generated on the surface of the silicon wafer, that is, a silicon oxide film is generated on the silicon oxide film or other film on the surface of the silicon wafer. For example, in the case of preparing passivated emitter and rear cell technology (Passivated Emitter and Rear Cell, PERC) batteries, the aluminum oxide film deposition process is to generate an aluminum oxide film on the backlight side of the silicon wafer, and the previous process of the aluminum oxide film deposition process is an oxidation process, in which a silicon oxide film is generated on the backlight side of the silicon wafer. In this case, ozone is introduced to purge the surface of the silicon wafer, that is, to purge the silicon oxide film on the backlight side of the silicon wafer, and a silicon oxide film is generated on the silicon oxide film on the backlight side of the silicon wafer. The ozone is also used to purge other locations in the chamber other than the silicon wafer surface to remove dust in the chamber and improve the cleanliness of the chamber. Ozone is a commonly used reaction gas for generating aluminum oxide film. Existing ALD machines can usually be fed with ozone. The introduction of ozone does not require additional modification of the ALD machine, and the process is simple and cost-saving.
[0032] Step 102, introducing a first nitrogen gas to purge the chamber.
[0033] The first nitrogen gas is introduced to purge the chamber, which can remove the particulate carbonaceous materials produced by the pyrolysis reaction of organic matter in the dust remaining in the chamber after the ozone is introduced, the silicon oxide particles generated after the oxidation of silicon fragments and powders, and the residual dust, further improving the cleanliness of the chamber. Nitrogen has the advantages of being cheap and not generating pollutants. In addition, nitrogen has high chemical stability, is difficult to participate in chemical reactions, and will not react with silicon wafers or dust to avoid adverse effects. In addition, nitrogen is a commonly used carrying gas or cleaning gas for generating aluminum oxide films. Existing ALD machines can usually be supplied with nitrogen. The introduction of nitrogen does not require additional modifications to the ALD machine, and the process is simple and cost-saving.
[0034] Step 103: forming an aluminum oxide film on the surface of the silicon oxide film.
[0035] An aluminum oxide film is formed on the surface of the silicon oxide film. Specifically, a reaction gas for forming an aluminum oxide film is introduced to form the aluminum oxide film. For example, trimethylaluminum and ozone may be introduced.
[0036] The inventors have discovered that in the prior art, the generation of EL black spots and black dots is generally reduced by improving the cleanliness of the tooling or fixtures. Although this method can reduce the generation of EL black spots and black dots caused by the dirtiness of the tooling or fixtures, it cannot improve the situation in which dust in the air or in the ALD machine falls onto the surface of the silicon wafer during the process of transporting the silicon wafer to the ALD machine for depositing the aluminum oxide film, and during the leak detection of the ALD machine, causing the generation of EL black spots and black dots.
[0037] In response to the above-mentioned technical problems, in an embodiment of the present invention, the inventor creatively added a step of introducing ozone, placing a silicon wafer into the chamber of an atomic layer deposition machine, and after leak testing the atomic layer deposition machine, introducing ozone to purge the surface of the silicon wafer to remove dust on the surface of the silicon wafer. The dust on the surface of the silicon wafer includes dust that falls from the air to the surface of the silicon wafer during transportation from the previous process to the process of depositing an aluminum oxide film, or dust that falls from the chamber of the atomic layer deposition machine to the surface of the silicon wafer when the atomic layer deposition machine is leak tested. The dust mainly includes: silicon fragments and powder, dust in the air, and aluminum oxide powder remaining in the chamber of the ALD machine. During the purging process of the silicon wafer surface, the silicon fragments and powder are oxidized into silicon oxide particles, which are purged and removed by ozone. The organic matter in the dust in the air undergoes pyrolysis reaction at high temperature to produce granular carbonaceous substances, which are purged and removed by ozone. Other substances other than organic matter in the dust in the air are purged and removed by ozone. The aluminum oxide powder remaining in the ALD machine chamber is purged and removed by ozone, and no film layer is formed on the surface of the silicon wafer. Ozone reacts with the silicon wafer to form a silicon oxide film on the surface of the silicon wafer, which can better passivate the silicon wafer. The introduction of ozone is also used to purge other locations in the chamber other than the silicon wafer surface to remove dust in the chamber and improve the cleanliness of the chamber. Ozone is a commonly used reaction gas for generating aluminum oxide films. Existing ALD machines can usually be introduced with ozone. The introduction of ozone does not require additional modifications to the ALD machine, and the process is simple and cost-saving. The first nitrogen gas is introduced to purge the chamber, which can remove the granular carbonaceous materials produced by the pyrolysis reaction of organic matter in the dust remaining in the chamber after the ozone is introduced, the silicon oxide particles generated after the oxidation of silicon fragments and powders, and the residual dust, and further improve the cleanliness of the chamber. In addition, nitrogen has a high chemical stability, is difficult to participate in chemical reactions, and will not react with silicon wafers or dust to avoid adverse effects. Nitrogen is a commonly used carrier gas or cleaning gas for generating aluminum oxide film. Existing ALD machines can usually be introduced with nitrogen. The introduction of nitrogen does not require additional modification of the ALD machine, and the process is simple and cost-saving. Then, an aluminum oxide film is generated on the surface of the silicon oxide film. Since the dust on the surface of the silicon wafer has been removed more thoroughly in the aforementioned process, the present invention can improve the situation of EL black spots caused by dust falling on the surface of the silicon wafer during the process of depositing the aluminum oxide film, and avoid affecting the yield of the production line.
[0038] Optionally, the flow rate of ozone is 1000 standard milliliters per minute to 2000 standard milliliters per minute. For example, the flow rate of ozone can be 1000 sccm (standard cubic centimeter per minute), or 1200 sccm, or 1400 sccm, or 1600 sccm, or 1800 sccm, or 2000 sccm. The flow rate of ozone is 1000 standard milliliters per minute to 2000 standard milliliters per minute, which can avoid a small flow rate, which will cause a poor purging effect on the dust falling on the surface of the silicon wafer, and at the same time, avoid a large flow rate, which will cause a thick silicon oxide film and affect the thickness of the solar cell.
[0039] Optionally, the time for passing ozone is 50 seconds to 150 seconds. For example, the time for passing ozone can be 50 seconds (seconds), or 70 seconds, or 90 seconds, or 110 seconds, or 130 seconds, or 140 seconds, or 150 seconds. The time for passing ozone is 50 seconds to 150 seconds, which can avoid the time being too short, which will cause a poor purging effect on the dust falling on the surface of the silicon wafer, and at the same time, avoid the time being too long, which will cause the silicon oxide film to be thicker and affect the thickness of the solar cell. In addition, avoid the time being too long, which will extend the process time and cause waste of production capacity.
[0040] Optionally, the thickness of the silicon oxide film is 1 nanometer to 3 nanometers. For example, the thickness of the silicon oxide film can be 1 nm (nanometer), or 1.4 nm, or 1.5 nm, or 2 nm, or 2.5 nm, or 3 nm. The thickness of the silicon oxide film is 1 nanometer to 3 nanometers, which has a good passivation effect on the silicon wafer, and at the same time, avoids the silicon oxide film being too thick, which affects the thickness of the solar cell.
[0041] Optionally, the flow rate of the first nitrogen gas is 2000 standard milliliters per minute to 5000 standard milliliters per minute, and the time for the first nitrogen gas to be introduced is 10 seconds to 30 seconds. For example, the flow rate of the first nitrogen gas can be 2000sccm, or 2500sccm, or 3000sccm, or 3500sccm, or 4000sccm, or 5000sccm, and the flow rate of the first nitrogen gas is 2000 standard milliliters per minute to 5000 standard milliliters per minute, which can avoid the flow rate of the first nitrogen gas being too small, resulting in a poor purging effect, and at the same time, avoid too large a flow rate, resulting in a waste of nitrogen; for example, the time for the first nitrogen gas to be introduced can be 10s, or 14s, or 15s, or 20s, or 25s, or 30s, and the time for the first nitrogen gas to be introduced is 10 seconds to 30 seconds, which can avoid the time of the first nitrogen gas being too short, resulting in a poor purging effect, and at the same time, avoid too long a time, resulting in a waste of nitrogen, and in addition, avoid too long a time, prolong the process time, and cause waste of production capacity.
[0042] Optionally, after placing the silicon wafer into the chamber of the atomic layer deposition machine, the method further includes: introducing a second nitrogen gas to purge the chamber, thereby reducing the amount of dust in the chamber of the atomic layer deposition machine and improving the cleanliness of the chamber of the atomic layer deposition machine.
[0043] Optionally, the flow rate of the second nitrogen gas is 2000 standard milliliters per minute to 10000 standard milliliters per minute, and the time for the second nitrogen gas to be introduced is 20 seconds to 60 seconds. For example, the flow rate of the second nitrogen gas can be 2000sccm, or 4000sccm, or 5000sccm, or 6000sccm, or 8000sccm, or 10000sccm, and the flow rate of the second nitrogen gas is 2000 standard milliliters per minute to 10000 standard milliliters per minute, which can avoid the flow rate of the second nitrogen gas being too small, resulting in incomplete purging of the atomic layer deposition machine chamber, and at the same time, avoid too large a flow rate, resulting in waste of nitrogen; for example, the time for the second nitrogen gas to be introduced can be 20s, or 25s, or 30s, or 40s, or 50s, or 60s, and the time for the second nitrogen gas to be introduced is 20 seconds to 60 seconds, which can avoid the time of the second nitrogen gas being too short, resulting in incomplete purging of the atomic layer deposition machine chamber, and at the same time, avoid too long time, resulting in waste of nitrogen, and also avoid too long time, extending the process time, and causing waste of production capacity.
[0044] Optionally, an aluminum oxide film is generated on the surface of the silicon oxide film, including: a first step, introducing trimethylaluminum; a second step, introducing nitrogen to purge the trimethylaluminum; a third step, introducing ozone; a fourth step, introducing nitrogen to purge the ozone; the first step to the fourth step form a cycle; after one cycle, a third step of introducing nitrogen to purge the surface of the silicon wafer.
[0045] After one cycle, the third nitrogen gas is introduced to purge the surface of the silicon wafer. The purge can be performed after each cycle of depositing the aluminum oxide film to prevent dust in the atomic layer deposition machine chamber from adhering to the silicon wafer, which can effectively reduce the generation of EL black spots.
[0046] Optionally, after the aluminum oxide film is formed on the surface of the silicon oxide film, the exhaust gas is cleaned and discharged, and then nitrogen is introduced to purge the chamber to ensure that there is no dust attached to the surface of the silicon wafer when it leaves the chamber, thereby improving the cleanliness of the silicon wafer surface.
[0047] An embodiment of the present invention also provides a solar cell, comprising: a silicon wafer, a silicon oxide film located on the surface of the silicon wafer, and an aluminum oxide film located on the surface of the silicon oxide film, wherein the silicon oxide film and the aluminum oxide film are both prepared by the above-mentioned aluminum oxide film coating method.
[0048] Both the silicon oxide film and the aluminum oxide film are prepared by the above-mentioned method of coating the aluminum oxide film. Since the process in the above-mentioned method of coating the aluminum oxide film has already removed the dust on the surface of the silicon wafer more thoroughly, the present invention can improve the situation of EL black spots caused by dust falling onto the surface of the silicon wafer during the process of depositing the aluminum oxide film, thereby improving the electrical performance of the solar cell and avoiding affecting the production line yield.
[0049] Optionally, the solar cell includes a passivated emitter and back cell technology cell, a shingled solar cell, a tunnel oxide passivated contact cell, and a back electrode contact silicon solar cell. PERC cells, shingled solar cells, tunnel oxide passivated contact (TOPCon) cells, and interdigitated back contact (IBC) silicon solar cells are widely used. The silicon oxide film and aluminum oxide film of these solar cells are prepared by the above-mentioned aluminum oxide film coating method, which can improve their electrical performance. Optionally, when preparing a PERC cell, the backlight surface of the silicon wafer is purged, and a silicon oxide film is generated on the backlight surface of the silicon wafer; a first nitrogen gas is introduced to purge the chamber; and an aluminum oxide film is generated on the surface of the silicon oxide film. In addition, when preparing PERC cells, the previous process of depositing the aluminum oxide film is an oxidation process. Generally, a tubular machine is used to oxidize the backlight side of the silicon wafer. That is to say, when preparing PERC cells, the backlight side of the silicon wafer is purged, and the surface of the silicon oxide film generated on the backlight side of the silicon wafer in the oxidation process is purged. When preparing PERC cells, a silicon oxide film is generated on the backlight side of the silicon wafer. The silicon oxide film is generated on the surface of the silicon oxide film generated on the backlight side of the silicon wafer in the oxidation process.
[0050] The present invention will be further explained below in conjunction with specific embodiments. Figure 2 , Figure 2 A flowchart of another method for coating an aluminum oxide film in an embodiment of the present invention is shown, which specifically includes the following steps:
[0051] Step 1: Automatically load the wafers. After the previous process, the silicon wafers that have reached the aluminum oxide film deposition process are inserted into the aluminum boat in a double-insertion manner with the light side facing each other. Then, the aluminum boat is placed on a carrier that supports the aluminum boat. After completion, proceed to step 2.
[0052] Step 2: Back pressure in the chamber, introduce N 2 (nitrogen), N 2 The flow rate is 10000sccm, and N 2 The time is 90s, the chamber returns to normal atmospheric pressure, the chamber is opened, and the carrier carrying the aluminum boat enters the chamber. After completion, proceed to step 3.
[0053] Step 3, the machine is heated and starts to heat up. The temperature is set to 190°C (degrees Celsius). After reaching the set temperature, the temperature is kept constant for 300s. Then, the process ends and the process goes to step 4.
[0054] Step 4: Start the main pumping and introduce the second nitrogen to purge the chamber. 2 The flow rate is 5000sccm, and N 2 The time is 60s. After purging, the chamber pressure is pumped down to 0.002 Torr for leak detection, and then the process goes to step 5.
[0055] Step 5: After leak testing the atomic layer deposition machine, introduce O 3 (Ozone), O 3 The flow rate is 2000sccm, and O 3 The time is 60s, the surface of the silicon wafer is purged, and a silicon oxide film is formed on the surface of the silicon wafer; after the end, the first nitrogen gas is introduced to purge the chamber, N 2 The flow rate is 5000sccm, and N 2 The time is 10s, and after that, go to step 6.
[0056] Step 6, the flow rate of TMA (trimethylaluminum) is 3000sccm, O 3 The flow rate is 6000sccm, the temperature is controlled at 190℃, and the pressure is set to 0.002Torr. In the first step, trimethylaluminum is introduced for 4s; in the second step, nitrogen is introduced to purge trimethylaluminum for 4s to stabilize the gas distribution in the chamber; in the third step, ozone is introduced for 6s; in the fourth step, nitrogen is introduced to purge ozone for 4s to stabilize the gas distribution in the chamber; from the first step to the fourth step, a cycle is formed, and the cycle time is 18s. The number of cycles is set to 18. In the second and fourth steps, N 2 The flow rate is 5000sccm. After one cycle, the third nitrogen gas is introduced to purge the surface of the silicon wafer. 2 The flow rate is 1000sccm, and N 2 The time is 5s, that is, N is passed at the end of each cycle. 2 Perform the purge and proceed to step 7 when finished.
[0057] Step 7: Set the pressure to 0 mTorr (mTorr), clean the exhaust gas, and then introduce N 2 , N 2 The flow rate is 5000sccm, and N 2 The time is 30s, and cleaning is performed before exiting the cavity to remove the residual dust on the aluminum boat and proceed to step 8.
[0058] Step 8: Back pressure in the chamber, introduce N 2, N 2 The flow rate is 10000sccm, and N 2 The time is 90s, the chamber returns to normal atmospheric pressure, the chamber is opened, and the carrier carrying the aluminum boat is taken out of the chamber. After completion, enter step 9.
[0059] Step 9, cooling down, the cooling time is 100s, then the robot grabs the aluminum boat and puts it into the unloading station for unloading.
[0060] In step 2, N 2 The flow rate can be 10000 sccm to 20000 sccm. For example, N 2 The flow rate of N can be 10000 sccm, or 12000 sccm, or 14000 sccm, or 16000 sccm, or 18000 sccm, or 20000 sccm. 2 The time can be 60s to 90s. For example, N 2 The time can be 60s, or 65s, or 70s, or 75s, or 80s, or 90s.
[0061] In step 3, the constant temperature time can be 200s to 300s, for example, the constant temperature time can be 200s, or 220s, or 240s, or 260s, or 280s, or 300s. In step 3, the constant temperature is performed to keep the temperature constant, which can ensure that the chamber temperature is evenly distributed, and the chamber temperature and the aluminum boat and silicon wafer at different positions are heated to the same temperature to ensure the deposition rate, so that O 3 React completely with TMA to avoid the situation where the temperature of the aluminum boat and silicon wafer at different positions is different. The temperature is different and the gas reacts differently in the same time. The excess gas reacts into alumina powder instead of being deposited on the aluminum boat and silicon wafer.
[0062] In step 4, N 2 The flow rate can be 2000 sccm to 10000 sccm, for example, N 2 The flow rate of N can be 2000sccm, 4000sccm, 5000sccm, 6000sccm, 8000sccm, or 10000sccm. 2 The time can be 20s to 60s. For example, N 2 The time may be 20s, 25s, 30s, 35s, 50s, or 60s. After the purge, the chamber pressure may be pumped down to 0.002 Torr to 0.005 Torr for leak detection. For example, the pressure may be pumped down to 0.002 Torr, 0.003 Torr, 0.0035 Torr, 0.004 Torr, 0.0045 Torr, or 0.005 Torr.
[0063] In step 6, the temperature can be controlled at 190° C. to 210° C., for example, the temperature can be controlled at 190° C., or 195° C., or 200° C., or 205° C., or 208° C., or 210° C. The pressure can be set to 0.002 Torr to 0.005 Torr, for example, the pressure can be set to 0.002 Torr, or 0.003 Torr, or 0.0035 Torr, or 0.004 Torr, or 0.0045 Torr, or 0.005 Torr. In the second and fourth steps, N 2 The flow rate can be 5000 sccm to 10000 sccm. For example, in the second and fourth steps, N 2 The flow rate can be 5000sccm, or 6000sccm, or 7000sccm, or 8000sccm, or 9000sccm, or 10000sccm. 2 The flow rate is larger and can carry TMA, O 3 Diffusion in the furnace allows the gas to react completely, avoiding excess gas reaction to generate alumina powder, rather than being deposited on the aluminum boat or silicon wafer. The flow rate of the third nitrogen gas can be 1000 sccm to 2000 sccm, for example, the flow rate of the third nitrogen gas can be 1000 sccm, or 1200 sccm, or 1400 sccm, or 1600 sccm, or 1800 sccm, or 2000 sccm. The time for the third nitrogen gas to be introduced can be 3s to 6s, for example, the time for the third nitrogen gas to be introduced can be 3s, or 4s, or 4.5s, or 5s, or 5.5s, or 6s.
[0064] In step 7, N 2 The flow rate can be 2000 sccm to 5000 sccm, for example, N 2 The flow rate can be 2000sccm, or 2500sccm, or 3000sccm, or 3500sccm, or 4000sccm, or 5000sccm. 2 The time can be 20s to 60s. For example, N 2 The time can be 20s, or 25s, or 30s, or 35s, or 50s, or 60s.
[0065] In step 8, N 2 The flow rate can be 10000 sccm to 20000 sccm. For example, N 2 The flow rate of N can be 10000 sccm, or 12000 sccm, or 14000 sccm, or 16000 sccm, or 18000 sccm, or 20000 sccm. 2The time can be 60s to 90s. For example, N 2 The time can be 60s, or 65s, or 70s, or 75s, or 80s, or 90s.
[0066] The silicon wafers were subjected to the processes before the aluminum oxide film deposition process under the same conditions, and then divided into two groups. The first group adopted the above-mentioned aluminum oxide film coating method to perform the aluminum oxide film deposition process on the silicon wafers, and then performed the processes after the aluminum oxide film deposition process to prepare solar cells as Example 1; the second group referred to the above-mentioned aluminum oxide film coating method, except that the above-mentioned step 5 was not performed, and step 6 was directly performed after the above-mentioned step 4. The other steps and parameters were the same, the aluminum oxide film deposition process was performed on the silicon wafers, and then the processes after the aluminum oxide film deposition process were performed under the same conditions as in Example 1 to prepare solar cells as Comparative Example 1.
[0067] The solar cells prepared in the comparative example 1 and the example 1 were subjected to electrical performance test and EL test under the same test conditions. The test results are shown in Table 1 and Table 2.
[0068] Table 1 Electrical performance test results of comparative example 1 and embodiment 1
[0069] Group count Eta(%) Isc(A) Uoc(V) FF(%) Rs(Ω) Rsh(Ω) Irev1(A) Example 1 3200 23.325 13.548 0.695 81.78 0.0014 401 0.192 Comparative Example 1 3200 23.21 13.538 0.694 81.558 0.0014 434 0.165
[0070] In Table 1, the count refers to the number of tested solar cells, Eta refers to the photoelectric conversion efficiency, Isc refers to the short-circuit current, Uoc refers to the open-circuit voltage, FF refers to the fill factor, Rs refers to the series resistance, Rsh refers to the parallel resistance, and Irev1 refers to the reverse current when the voltage is -10V (volts). Each electrical performance value is obtained by taking the average value of all solar cells in each group.
[0071] As can be seen from Table 1, the photoelectric conversion efficiency of Example 1 is improved compared with Comparative Example 1. This shows that the photoelectric conversion efficiency can be improved by using the method for coating an aluminum oxide film in the embodiment of the present invention. The method for coating an aluminum oxide film in the embodiment of the present invention adds a step of introducing ozone, introducing ozone, blowing the surface of the silicon wafer to remove dust on the surface of the silicon wafer, and forming a silicon oxide film on the surface of the silicon wafer, which can better passivate the silicon wafer, thereby improving the photoelectric conversion efficiency of the solar cell.
[0072] Table 2 EL test results of comparative example 1 and embodiment 1
[0073] Group count The ratio of black spots The proportion of dirt The ratio of winding plating Example 1 3200 0.19% 0.08% 0.00% Comparative Example 1 3200 0.37% 0.26% 0.05%
[0074] The counts in Table 2 refer to the number of solar cells tested. The main EL test failures include black spots, dirt, and plating bypass. Black spots are mainly caused by dust or liquid on the silicon wafer, which appear black with obvious dots in the center during the EL test. Dirt is the blackening of irregular EL areas. Plating bypass is the black edges caused by contamination of the edge of the silicon wafer during the EL test. The percentage values in Table 2 (retain two decimal places) are the proportions of the number of solar cells with these three EL test failures to the number of solar cells tested.
[0075] As can be seen from Table 2, compared with Comparative Example 1, the proportion of black spots and black dots in Example 1 is reduced, the proportion of dirt is reduced, and the proportion of bypass plating is reduced. This shows that the method for plating aluminum oxide film in the embodiment of the present invention can improve the situation of EL black spots and black dots caused by dust falling on the surface of the silicon wafer during the process of depositing aluminum oxide film, and at the same time, the proportion of bypass plating and dirt is also reduced. The method for plating aluminum oxide film in the embodiment of the present invention adds the step of introducing ozone, introducing ozone, blowing the surface of the silicon wafer to blow away the dust on the surface of the silicon wafer, and introducing the first nitrogen gas to blow the chamber, which can further improve the cleanliness of the chamber. Since the dust on the surface of the silicon wafer has been removed more thoroughly in the aforementioned process, the method for plating aluminum oxide film in the embodiment of the present invention can improve the situation of EL black spots and black dots caused by dust falling on the surface of the silicon wafer during the process of depositing aluminum oxide film. At the same time, since the dust of the ALD machine is reduced, the cleanliness of the ALD machine is improved, which can improve the bypass plating caused by silicon wafer edge contamination and improve the EL dirt.
[0076] It should be noted that the aforementioned aluminum oxide film coating method and solar cell, the relevant parts of the two can be referenced to each other, and can achieve the same or similar effects.
[0077] It should be noted that, for the method embodiments, for the sake of simplicity of description, they are all expressed as a series of action combinations, but those skilled in the art should be aware that the embodiments of the present application are not limited by the described order of actions, because according to the embodiments of the present application, certain steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also be aware that the embodiments described in the specification are all preferred embodiments, and the actions involved are not necessarily required by the embodiments of the present application.
[0078] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.
[0079] It should be noted that, in this document, the terms "first", "second", etc. in the specification and claims are used to distinguish similar objects, rather than to describe a specific order or sequence. Moreover, the objects distinguished by "first", "second", etc. are usually of the same type, and the number of objects is not limited. For example, the second object can be one.
[0080] Through the description of the above implementation methods, those skilled in the art can clearly understand that the above-mentioned embodiment methods can be implemented by means of software plus a necessary general hardware platform, and of course by hardware, but in many cases the former is a better implementation method. Based on such an understanding, the technical solution of the present invention, or the part that contributes to the prior art, can be embodied in the form of a software product, which is stored in a storage medium (such as ROM / RAM, a magnetic disk, or an optical disk), and includes a number of instructions for enabling a terminal (which can be a mobile phone, a computer, a server, an air conditioner, or a network device, etc.) to execute the methods described in each embodiment of the present invention.
[0081] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation modes, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.
Claims
1. A method for coating an aluminum oxide film, characterized in that: include: Putting a silicon wafer into a chamber of an atomic layer deposition machine, after leak testing the atomic layer deposition machine, introducing ozone to purge the surface of the silicon wafer and forming a silicon oxide film on the surface of the silicon wafer; A first nitrogen gas is introduced to purge the chamber; An aluminum oxide film is formed on the surface of the silicon oxide film.
2. The method for coating an aluminum oxide film according to claim 1, characterized in that: The flow rate of the ozone is 1000 standard milliliters per minute to 2000 standard milliliters per minute.
3. The method for coating an aluminum oxide film according to claim 1, characterized in that: The time of introducing ozone is 50 seconds to 150 seconds.
4. The method for coating an aluminum oxide film according to claim 1, characterized in that: The silicon oxide film has a thickness of 1 nanometer to 3 nanometers.
5. The method for coating an aluminum oxide film according to claim 1, characterized in that: The flow rate of the first nitrogen gas is 2000 standard milliliters per minute to 5000 standard milliliters per minute, and the time for the first nitrogen gas to be introduced is 10 seconds to 30 seconds.
6. The method for coating an aluminum oxide film according to any one of claims 1 to 5, characterized in that: After placing the silicon wafer into the chamber of the atomic layer deposition machine, the method further comprises: A second nitrogen gas flow is performed to purge the chamber.
7. The method for coating an aluminum oxide film according to claim 6, characterized in that: The flow rate of the second nitrogen gas is 2000 standard milliliters per minute to 10000 standard milliliters per minute, and the time for the second nitrogen gas to be introduced is 20 seconds to 60 seconds.
8. The method for coating an aluminum oxide film according to any one of claims 1 to 5, characterized in that: The step of generating an aluminum oxide film on the surface of the silicon oxide film comprises: The first step is to introduce trimethylaluminum; In the second step, nitrogen is introduced to purge the trimethylaluminum; The third step is to introduce ozone; The fourth step is to introduce nitrogen to purge the ozone; Steps 1 to 4 form a cycle; After the one cycle, a third nitrogen gas is introduced to purge the surface of the silicon wafer.
9. A solar cell, characterized in that: include: A silicon wafer, a silicon oxide film located on the surface of the silicon wafer, and an aluminum oxide film located on the surface of the silicon oxide film, wherein the silicon oxide film and the aluminum oxide film are both prepared by the method for coating aluminum oxide film according to any one of claims 1 to 8.
10. The solar cell according to claim 9, characterized in that: The solar cells include passivated emitter and back cell technology cells, shingled solar cells, tunnel oxide layer passivated contact cells, and back electrode contact silicon solar cells.
Citation Information
Cited By
Preparation process of aluminum oxide film-containing battery piece and UV (ultraviolet) solar battery of aluminum oxide film-containing battery piece
CN120060826A