Three-dimensional assembly method using sacrificial layer to assist debonding

By preparing a sacrificial layer that is easy to remove in the non-bonding zone of the three-dimensional flexible electronic device, and using a temporary substrate to assist in the debonding, the problem of difficulty in debonding in the non-bonding zone in the prior art is solved, and high reliability and low cost are achieved 3D assembly, suitable for the assembly of complex structures.

CN119031688APending Publication Date: 2024-11-26TSINGHUA UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411117400.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-05-31
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the existing three-dimensional flexible electronic device assembly methods, the non-bonding zone is difficult to debond according to design requirements, resulting in assembly failure. The existing auxiliary debonding method increases process complexity and production costs, making it difficult to achieve accurate controllable complex structures. design.

Method used

Using the method of assisted debonding of the sacrificial layer, the sacrificial layer that is easy to remove is prepared in the non-bonding area of ​​the precursor and transfer it to the temporary substrate, and then attach the precursor to the assembled substrate to remove the temporary substrate and the sacrificial layer to achieve Reliable debonding of the precursor and the assembled substrate.

Benefits of technology

Reliable debonding of non-bonding zones in three-dimensional assembly is achieved, reducing process complexity and production costs, avoiding the impact of additional appendages on the molded structure, and improving the designability and reliability of the assembly technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119031688A_ABST
    Figure CN119031688A_ABST
Patent Text Reader

Abstract

The invention provides a three-dimensional assembly method for assisting debonding by using a sacrificial layer. The three-dimensional assembly method comprises the following steps: S1, preparing the sacrificial layer on a precursor; s2, transferring the precursor with the sacrificial layer to a temporary substrate; s3, attaching the precursor with the sacrificial layer to an assembly substrate by means of the temporary substrate; and S4, removing the temporary substrate and the sacrificial layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of flexible electronic technology, and in particular to a three-dimensional assembly method using a sacrificial layer to assist in debonding. Background Art

[0002] In recent years, flexible electronic technology has rapidly developed into a frontier research direction, and many types of flexible electronic device products have emerged on the market, such as flexible displays, electronic skin, and wearable electronic products. Three-dimensional flexible electronic devices often have advantages such as more deformation modes, greater stretchability, and richer spatial configurations. They are a type of flexible electronic device with broad application prospects.

[0003] In order to designably assemble traditional planar two-dimensional electronic devices into the required three-dimensional configuration, a commonly used method is a three-dimensional assembly method based on mechanical guidance. This method has become an important method for assembling and forming three-dimensional flexible electronic devices. The typical process flow of this method is: 1. Obtain a patterned two-dimensional precursor structure by micromachining, laser cutting and other methods. 2. Deposit silica at a specific position of the precursor (i.e., the bonding point position). 3. Transfer the two-dimensional precursor to a water-soluble tape, and at the same time quantitatively pre-stretch an elastic substrate on the loading table, and activate the surfaces of both by ultraviolet treatment and other methods. 4. Transfer the two-dimensional precursor to the pre-stretched elastic substrate to ensure that the surfaces of the two activated substrates are tightly attached together, and heat the overall structure to form a strong covalent bond between the silica on the structure and the elastic substrate. 5. Remove the water-soluble tape with flowing deionized water. 6. Gradually release the pre-stretching strain of the elastic substrate, thereby deforming the two-dimensional precursor and forming a three-dimensional flexible structure.

[0004] In the above-mentioned prior art solution, since the two-dimensional precursor is selectively bonded to the surface of the elastic substrate only at the bonding point, the two-dimensional precursor structure will bend and deform under the action of compressive strain, and finally form a three-dimensional structure. This method can integrate discrete flexible components of different types and independently prepared on a large scale to form a spatially ordered functional system. It has unique advantages such as compatibility with planar micromachining technology, wide application of material systems, and large-scale efficient production. The above solution has been widely used in flexible photodetection devices, flexible wearable sensors, and curved conformal three-dimensional structures.

[0005] As the types of materials and structural forms used in three-dimensional flexible electronic device systems become more and more complex and diverse, the reliability of flexible electronic device assembly methods also needs to be further improved. In the above-mentioned traditional three-dimensional assembly method, silicon dioxide is deposited in the bonding area of ​​the precursor and connected to the elastic substrate to form a strong interface with a firm bond. The remaining area of ​​the precursor (non-bonding area) should theoretically form a weak interface that is easy to detach with the elastic substrate (strong interface and weak interface are theoretical areas between the precursor and the assembly substrate that are distinguished by the size of the adhesive force, rather than the area division of the precursor or the assembly substrate itself). However, the area where the precursor should theoretically form a weak interface is generally not specially treated, and it is easy to form an uncontrollable strong bond between this area and the assembly substrate, so that part of the non-bonding point area on the structure may also be adhered to the surface of the elastic substrate together, resulting in the precursor may not be correctly assembled into the designed three-dimensional structure. In order to solve this problem, it is necessary to optimize the regulation ability of the weak interface so that the non-bonding area of ​​the precursor can be reliably separated from the elastic substrate, and to achieve accurate design and control of patterning of the non-bonding area, thereby improving the designability and reliability of the three-dimensional assembly technology.

[0006] The existing methods for improving the debonding of weak interfaces in three-dimensional assembly methods generally involve applying external auxiliary forces, such as adding auxiliary supports and applying non-contact electromagnetic forces. Figure 7 As shown, the method of adding an auxiliary support structure is to arrange an auxiliary support 70 under the non-bonding area of ​​the precursor (target structure) to be assembled to assist in the assembly of the three-dimensional flexible electronic device, that is, to form a three-dimensional structure 60. The precursor and the auxiliary support 70 are assembled at the same time. The auxiliary support 70 can form a three-dimensional structure and generate a certain upward support force on the precursor, helping the non-bonding area of ​​the precursor to separate from the surface of the assembly substrate 50. Figure 8 As shown, the method of applying non-contact electromagnetic force is to additionally make circuits, electrodes, magnetic particles, etc. on the precursor to form an electrical performance layer 80, and then apply non-contact electromagnetic force to the electrical performance layer 80 through external equipment such as high-voltage power supply and strong magnets to help the precursor to separate from the assembly substrate 50 in the non-adhesive area.

[0007] The above existing methods will significantly increase the process complexity and production cost of three-dimensional flexible electronic devices, and will also impose many restrictions on their material system and process flow, making it difficult to form a precise and controllable design for weak interfaces of complex structures. At the same time, the above methods will add additional appendages to the formed three-dimensional flexible structure, and an additional step is required to remove the appendages after completing the three-dimensional assembly step, which may have an adverse effect on the properties of the formed three-dimensional structure.

[0008] Specifically, if Figure 7The method of adding auxiliary support shown in the figure requires the additional preparation of another auxiliary support structure, which increases the complexity of the process steps and production costs of the three-dimensional flexible electronic device production. Since the precursor structure and the auxiliary support structure are independent of each other, after the auxiliary support structure is first transferred to the substrate, the precursor structure may not be effectively aligned with the auxiliary support structure during transfer, thereby failing to achieve accurate weak interface regulation. At the same time, the auxiliary support structure is mostly a strip structure, which can generally only assist a relatively simple precursor structure to complete three-dimensional assembly, and it is difficult to assist in debonding a precursor structure with multiple bonding points or internal bonding points. The auxiliary support structure is often assembled in different directions of the target structure, and the elastic substrate needs to be pre-stretched in one more dimension, which will increase the complexity of the assembly process. The auxiliary support structure needs to be removed after the assembly is completed, otherwise it will affect the configuration and performance of the target three-dimensional structure, and it is difficult to selectively separate the bonding area of ​​the auxiliary support structure, and the subsequent process of removing the auxiliary support structure may also cause damage to the target three-dimensional structure.

[0009] For methods of applying non-contact electromagnetic force, such as applying electrostatic force, magnetic field force and other external forces to assist in detachment on the precursor structure, it is necessary to add additional electrical appendages such as circuits, electrodes, and magnetic particles to the precursor structure, and complex external equipment conditions are required during three-dimensional assembly. For methods of electrostatic force-assisted debonding, it is necessary to make additional electrodes on the precursor structure, and apply a high voltage through a high-voltage power supply on the side of the substrate that is not connected to the precursor. For methods of magnetic field force-assisted debonding, it is necessary to make a current path or attach magnetic particles on the precursor structure, and to apply a strong magnetic field as an aid, which increases the complexity of the system and the production cost and also makes the production process dangerous. Similarly, this type of method of applying non-contact electromagnetic force also has the problem of needing to remove appendages, otherwise it will have a significant impact on the properties of the target three-dimensional structure, especially the electrical properties. Summary of the invention

[0010] This application is made in view of the above-mentioned state of the prior art. The purpose of this application is to provide a three-dimensional assembly method using a sacrificial layer to assist debonding, which can use the sacrificial layer to achieve reliable debonding between the non-bonding area of ​​the precursor and the assembly substrate.

[0011] The present application provides a three-dimensional assembly method using a sacrificial layer to assist debonding, which comprises:

[0012] S1: preparing a sacrificial layer on the precursor;

[0013] S2: transferring the precursor with the sacrificial layer to a temporary substrate;

[0014] S3: attaching the precursor having the sacrificial layer to an assembly substrate by means of the temporary substrate;

[0015] S4: removing the temporary substrate and the sacrificial layer.

[0016] In at least one possible implementation, before step S3, silicon dioxide is deposited on the precursor.

[0017] In at least one possible embodiment, before step S3, the assembled substrate is subjected to a pre-stretching treatment.

[0018] In step S3, the silicon dioxide deposited by the precursor is attached to the assembly substrate,

[0019] After removing the temporary substrate and the sacrificial layer, the precursor and the assembly substrate are spaced apart or not attached to each other as a whole, and the pre-stretching strain of the assembly substrate is released, so that the precursor is deformed.

[0020] In at least one possible embodiment, the material of the precursor is one or more of a polymer, a metal, a semiconductor, a conductor and a composite material.

[0021] In at least one possible implementation, the material of the sacrificial layer is one or more of ultraviolet photoresist, polymethyl methacrylate and copper.

[0022] In at least one possible embodiment, the material of the temporary substrate is one or more of polydimethylsiloxane, a thermal release tape, and a water-soluble tape;

[0023] The material of the assembly substrate is one or more of polydimethylsiloxane and silicone.

[0024] In at least one possible implementation, in step S1, the method for preparing the sacrificial layer includes one or more of the following methods:

[0025] a: selectively exposing and developing the material for preparing the sacrificial layer through a photolithography mask to prepare the sacrificial layer;

[0026] b: removing part of the material for preparing the sacrificial layer by dry etching under the protection of a hard mask to obtain the sacrificial layer;

[0027] c: Preparation of sacrificial layer by selective deposition through hard mask.

[0028] In at least one possible embodiment, in step S2, the method of transferring the precursor to the temporary substrate is one or more of a secondary transfer method, a liquid-assisted transfer method, and an electrostatic-assisted transfer method.

[0029] In at least one possible embodiment, in step S3, before attaching the precursor having the sacrificial layer to the assembly substrate, the precursor and / or the assembly substrate is subjected to surface activation treatment, and the surface activation treatment method is one or more of ultraviolet light irradiation treatment, corona treatment, and reactive ion etching.

[0030] In at least one possible implementation, in step S4, the method of removing the sacrificial layer is one or more of a solvent method, an atmosphere method, and an irradiation method.

[0031] The three-dimensional assembly method using a sacrificial layer to assist in debonding provided in the present application can solve or alleviate the problem of assembly failure caused by the difficulty in debonding the non-bonding area as designed during the implementation of the traditional three-dimensional structure assembly method by setting an easily removable sacrificial layer in the non-bonding area on the precursor. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a flowchart of a three-dimensional assembly method according to one embodiment of the present application.

[0033] Figure 2 A schematic diagram of the structure of a precursor provided with a sacrificial layer and silicon dioxide according to one embodiment of the present application.

[0034] Figure 3 It is a schematic diagram of the structure of connecting a precursor to a temporary substrate according to one embodiment of the present application.

[0035] Figure 4 It is a schematic diagram of the structure of a precursor connection assembly substrate according to one embodiment of the present application.

[0036] Figure 5 This is a schematic diagram of the structure of the precursor after removing the sacrificial layer and connecting the assembly substrate according to one embodiment of the present application.

[0037] Figure 6 It is a schematic structural diagram of a three-dimensional structural product according to one embodiment of the present application.

[0038] Figure 7 It is a schematic structural diagram of a three-dimensional structural product of the first example in the prior art.

[0039] Figure 8 It is a schematic structural diagram of a second example of a three-dimensional structural product in the prior art.

[0040] Description of Reference Numerals

[0041] 10 Precursors

[0042] 20 Sacrificial Layer

[0043] 30 Silica

[0044] 40 Temporary base

[0045] 50 Assemble the base

[0046] 60 Three-dimensional structure

[0047] 70 Auxiliary support

[0048] 80 Electrical performance layer DETAILED DESCRIPTION

[0049] The exemplary embodiments of the present application are described below with reference to the accompanying drawings. It should be understood that these specific descriptions are only used to teach those skilled in the art how to implement the present application, and are not intended to exhaust all possible methods of the present application, nor to limit the scope of the present application.

[0050] The embodiments of the present application provide a three-dimensional assembly method using a sacrificial layer to assist debonding (hereinafter, sometimes referred to as "assembly method"). Figure 1 As shown, the assembly method may include the following steps: a. preparing a two-dimensional precursor structure; b. preparing a sacrificial layer on the precursor; c. transferring the precursor to a temporary substrate; d. attaching the precursor to an assembly substrate; e. removing the temporary substrate and the sacrificial layer; f. completing mechanically guided three-dimensional assembly.

[0051] Specifically, the assembly method can first design and prepare the two-dimensional precursor 10 according to the requirements, and the preparation method of the two-dimensional precursor 10 is not particularly limited. Figure 2 and Figure 3 As shown, a sacrificial layer 20 is prepared on the non-bonding area of ​​the prepared precursor 10 (target structure), and the non-bonding area of ​​the precursor 10 can form a weak interface area that is easy to separate with the assembly substrate 50. Silicon dioxide 30 can also be deposited on the bonding area of ​​the precursor 10, and the silicon dioxide 30 can form a strong interface area that is tightly connected with the assembly substrate 50. The non-bonding area and the bonding area can be divided into areas on the same surface of the precursor 10, that is, the sacrificial layer 20 and the silicon dioxide 30 can be set on the same surface of the precursor 10 according to design requirements. The precursor 10 is transferred to the temporary substrate 40, as shown in FIG. Figure 3 As shown, the side of the precursor 10 that is not provided with the sacrificial layer 20 and the silicon dioxide 30 can be connected (attached / transferred) to the temporary substrate 40. The temporary substrate 40 can be made of a material that is easy to peel off or remove. Figure 4As shown, the surface of the precursor 10 (especially the side provided with the sacrificial layer 20 and the silicon dioxide 30) can be activated and then attached to the pre-stretched assembly substrate 50. The silicon dioxide in the bonding area of ​​the precursor 10 and the assembly substrate 50 can be attached to form a strong interface area, and the sacrificial layer in the non-bonding area of ​​the precursor 10 and the assembly substrate 50 can be close to or attached to form a weak interface area. Figure 5 As shown, after the precursor 10 is connected to the assembly substrate 50, the temporary substrate 40 can be removed, and the sacrificial layer 20 can be removed by a reagent method or an atmosphere method, so that the structure of the precursor 10 in the weak interface area and the assembly substrate 50 are physically separated. Then, the conventional mechanical guided three-dimensional assembly steps can be continued, such as Figure 6 As shown, mechanically guided three-dimensional assembly can make the two-dimensional precursor 10 form a three-dimensional structure 60, and then form three-dimensional flexible electronic devices and other products. After the three-dimensional structure 60 formed by the above assembly method is prepared, no additional steps of removing the appendages are required to obtain a complete three-dimensional structure 60.

[0052] It can be understood that there is no strict limitation on the preparation order of the sacrificial layer 20 and the silicon dioxide 30 , as long as the sacrificial layer 20 and the silicon dioxide 30 are formed separately before the precursor 10 is attached to the assembly substrate 50 .

[0053] Optionally, the types of structural materials of the two-dimensional precursor 10 applicable to the present embodiment are not limited. For example, the precursor 10 can be various thin film structures flatly attached to a hard substrate (such as a silicon wafer, a glass wafer, etc.), including polymers (such as polyimide, SU-8 epoxy resin, etc.), metals (such as gold, titanium, etc.), semiconductor materials (such as silicon, germanium, etc.), conductor materials (such as indium tin oxide / ITO, silver paste, etc.) and composite materials of the above materials.

[0054] Optionally, the material type of the sacrificial layer 20 disposed on the precursor 10 applicable to the present embodiment is not limited. Exemplarily, the sacrificial layer 20 may be a material that is easy to prepare and / or remove, such as ultraviolet photoresist, polymethyl methacrylate (PMMA), copper, etc.

[0055] Optionally, the method for accurately determining the sacrificial layer area on the surface of the precursor 10 applicable to the present embodiment is not limited. For example, the position of the sacrificial layer area can be determined by selective exposure and development through a photolithography mask (particularly suitable for sacrificial layer materials such as ultraviolet photoresist); excess sacrificial layer material can be removed by dry etching under the protection of a hard mask while retaining the sacrificial layer material at the required position (particularly suitable for sacrificial layer materials such as polymethyl methacrylate / PMMA); the sacrificial layer material can be selectively deposited at the required position through a hard mask (particularly suitable for sacrificial layer materials such as copper).

[0056] Optionally, the temporary substrate 40 applicable to the present embodiment can be a releasable temporary pickup substrate. The type of the temporary substrate 40 is not limited. For example, the material of the temporary substrate 40 can be a material that is easy to peel off, such as polydimethylsiloxane (PDMS), a thermal release tape, or a material that is easy to dissolve and remove, such as a water-soluble tape.

[0057] Optionally, the method for transferring the precursor 10 to the temporary substrate 40 applicable to the present embodiment is not limited. For example, the transfer method may be a double transfer method based on different transfer stamps, or a liquid-assisted transfer method, an electrostatic-assisted transfer method, etc. The purpose of transferring the precursor 10 is to allow the precursor 10 to be picked up by the temporary substrate 40 while the other surface thereof provided with the sacrificial layer 20 and the silicon dioxide 30 faces outward so as to be attached to the assembly substrate 50.

[0058] Optionally, the method for activating the surface of the precursor 10 provided with the silicon dioxide 30 and / or the surface of the assembly substrate applicable to the present embodiment is not limited, and the surface activation method may be ultraviolet light irradiation treatment, corona treatment, reactive ion etching bombardment of the surface, etc. The purpose of the surface activation is to open the surface chemical bonds between the silicon dioxide 30 deposited on the structure of the precursor 10 and the assembly substrate 50, so that a strong chemical bond connection can be formed after the two are attached.

[0059] Optionally, the material type of the assembly substrate 50 applicable to this embodiment is not limited, and can be polydimethylsiloxane (PDMS), silicone (especially Ecoflex TM 、Dragon skin TM Series silica gel) and so on.

[0060] Optionally, the method for removing the sacrificial layer 20 applicable to the present embodiment is not limited, and the sacrificial layer can be removed by using reagents such as acetone, N-methylpyrrolidone (NMP), and acidic oxidizing solution; the sacrificial layer can be removed by using a gas atmosphere such as oxygen or chlorine; or the sacrificial layer can be removed by using optical methods such as ultraviolet irradiation and laser irradiation. Decomposing and removing the sacrificial layer can physically separate the precursor 10 in the weak interface region from the adjacent surface of the assembly substrate 50, thereby significantly reducing the adhesion force in the weak interface region and achieving reliable debonding between the precursor and the assembly substrate in the non-bonding area.

[0061] An example of the present embodiment is given below and the technical solution of the present application is further described in detail in conjunction with the accompanying drawings. It should be noted that the following examples are intended to facilitate the understanding of the technical solution of the present application and do not have any limiting effect on it.

[0062] 1. As Figure 2As shown, a strip-shaped two-dimensional precursor structure is prepared by micromachining with a silicon wafer as the hard substrate of the precursor. Silicon dioxide is selectively deposited in the bonding area (strong interface area) through a hard mask, and a 1.5 μm thick AZ5214 photoresist is spin-coated on the surface of the two-dimensional precursor structure. The precursor is then placed on a hot plate at 110°C (degrees Celsius) for 60 seconds, and then the mask is aligned with the precursor structure on the photolithography machine, and a 200W / cm 2 (Watts per square centimeter) of ultraviolet light exposure, shaking in a 2.38% concentration of tetramethylammonium hydroxide solution for 120 seconds and then washing, ultimately a sacrificial layer made of photoresist can be formed in the non-bonding area of ​​the precursor.

[0063] It can be understood that the precursor in this embodiment adopts a strip structure, but the specific structure of the precursor is not limited thereto, and the implementation methods of the present application are applicable to precursors of any complex structure.

[0064] Preferably, in this embodiment, the sacrificial layer is made of AZ5214 photoresist material, and the sacrificial layer is prepared by spin coating AZ5214 photoresist and then removing excess photoresist material through a photolithography process, but the material and preparation method of the sacrificial layer are not limited thereto.

[0065] 2. If Figure 3 As shown, the precursor structure was picked up with a polydimethylsiloxane (PDMS) stamp and transferred to a water-soluble tape as a temporary substrate.

[0066] Preferably, the temporary substrate of this embodiment is made of water-soluble tape, but the material of the temporary substrate is not limited thereto.

[0067] 3. Such as Figure 4 As shown, prepare a piece of Ecoflex with a thickness of about 1mm TM 00-50 model silicone is used as the assembly substrate, and the assembly substrate is pre-stretched 40% on a small loading platform. The surfaces of the pre-stretched assembly substrate and the precursor are corona treated for 10s to activate the surfaces of the silicone assembly substrate and the silica. Subsequently, the surface of the precursor provided with silica is closely fitted to the surface of the assembly substrate, and placed in a 100°C oven for heating treatment for 10 minutes to complete the bonding connection between the assembly substrate and the silica.

[0068] Preferably, the assembly substrate in this embodiment is Ecoflex TM Silicone from 00-50, but not limited to.

[0069] Preferably, the tensile strain of the assembly substrate in this embodiment is selected to be 40%, but is not limited thereto.

[0070] Preferably, the surface activation method of the assembly substrate and silicon dioxide in this embodiment is a corona treatment method, but is not limited thereto.

[0071] 4. Such as Figure 5 As shown, deionized water is used to dissolve and remove the temporary substrate made of the water-soluble tape material, and then acetone is added dropwise to dissolve the sacrificial layer made of the AZ5214 photoresist material.

[0072] Preferably, in this embodiment, acetone is used to dissolve and remove the sacrificial layer, but the invention is not limited thereto.

[0073] 5. As Figure 6 As shown, the pre-stretching strain of the assembly substrate is slowly released, so that the precursor structure undergoes out-of-plane buckling under the action of the compressive strain and is assembled into the designed three-dimensional structure 60. Figure 6 , Figure 7 and Figure 8 As shown, the strip-shaped three-dimensional structure produced by the assembly method provided by the present application does not have any additional appendages compared to the same three-dimensional structure assembled by the aforementioned prior art method, that is, no additional process of removing the appendages is required, which can effectively reduce the impact on the quality of the three-dimensional structure.

[0074] The above embodiments provide a detailed description of the technical solutions and beneficial effects of the present application. It should be understood that the above description is only a specific embodiment of the present application and is not intended to limit the present application. Any modifications and improvements made within the scope of the principles of the present application should be included in the protection scope of the present application.

[0075] This application proposes to use a designable sacrificial layer to regulate the weak interface area in the three-dimensional assembly technology, which can achieve low-cost, large-scale, and high-reliability debonding of the target structure in the weak interface area. Compared with traditional auxiliary debonding methods such as using external structures or external forces, this solution has many advantages in production cost and product quality.

[0076] The technical solution of the present application can prepare the sacrificial layer with high precision, designability and selectivity through standard micro-machining technology, and decouple the preparation of the sacrificial layer from the preparation and assembly process of the precursor structure. The addition of two process steps, namely, preparing the sacrificial layer and removing the sacrificial layer, will not affect the process steps such as the processing and assembly of the precursor, and will not cause cross-influence between the overall process steps and the final structural performance.

[0077] The technical solution of the present application can arrange sacrificial layers at different positions of the precursor by appropriately designing the mask to meet the pattern requirements of different weak interface areas.

[0078] The technical solution of the present application can remove the sacrificial layer through a solution or atmosphere, so that the precursor structure in the weak interface area and the assembly substrate can be physically separated, thereby greatly reducing the interfacial energy and achieving highly reliable debonding of the weak interface, and the final formed three-dimensional structure has no redundant appendages.

[0079] The technical solution of the present application can be applied to the assembly of various flexible material components, such as polymers, metals, semiconductors and other commonly used materials in the flexible electronics field.

[0080] The following briefly describes some of the beneficial effects of the above-mentioned embodiments of the present application.

[0081] (1) The existing methods for assisting the debonding of weak interfaces in the assembly process of three-dimensional flexible electronic devices generally involve applying external auxiliary forces, such as adding auxiliary support structures, applying non-contact electromagnetic forces, etc. Such existing technologies will significantly increase process complexity and production costs, and have many restrictions on material types and process systems, and do not have the ability to accurately control the weak interfaces of complex structures. In the existing technology, additional appendages will be added to the formed three-dimensional structure, and additional steps are required to remove the appendages after completing the three-dimensional assembly steps, which may have an impact on the properties of the formed three-dimensional structure.

[0082] The technical solution of the present application at least partially solves the above problems. By directly preparing a designable sacrificial layer on the precursor structure, there is no need to prepare another complete auxiliary support structure, and there is no need to make complex structures such as interlayers, circuits, electrodes, magnetic particles, etc. on the target structure, so that high-reliability weak interface assisted debonding in the three-dimensional assembly process can be achieved. This assembly method can prepare the sacrificial layer after the precursor structure is fully prepared, which realizes the decoupling of the process flow and minimizes the complexity of the process steps and production costs. This assembly method can accurately determine the area of ​​the sacrificial layer by means of photolithography alignment, etc., and can achieve accurate and controllable weak interface regulation, which can be applicable to structures with complex appearance features and multiple bonding points. The sacrificial layer in this assembly method can be completely removed after the assembly is completed, and will not affect the configuration and performance of the target three-dimensional structure, etc., and can avoid damage to the target three-dimensional structure that may be caused during the removal of the appendages.

[0083] (2) Compared with the traditional three-dimensional assembly weak interface assisted debonding method, the three-dimensional assembly method using sacrificial layer assisted debonding provided by the embodiment of the present application adopts the method of adding a designable sacrificial layer, which can achieve low-cost, high-precision, large-volume, and high-reliability weak interface regulation, and can significantly improve the success rate of three-dimensional assembly technology in practical applications. The three-dimensional flexible electronic device products produced by this assembly method are at least partially superior to traditional methods in terms of accuracy, speed, component damage rate, etc. At the same time, the principle is simple, the repeatability is high, and the cost is low, which can meet the needs of industrial production and has a greater market prospect.

[0084] It is understood that in the present application, when the number of parts or components is not particularly limited, the number may be one or more, and the multiple here means two or more. For the case where the number of parts or components shown in the drawings and / or described in the specification is a specific number such as two, three, four, etc., the specific number is usually exemplary and not restrictive, and it can be understood as multiple, that is, two or more, but this does not mean that the present application excludes the case of one.

[0085] It should be understood that the above embodiments are merely exemplary and are not intended to limit the present application. Those skilled in the art may make various modifications and changes to the above embodiments under the guidance of the present application without departing from the scope of the present application.

Claims

1. A three-dimensional assembly method using a sacrificial layer to assist debonding, It is characterized in that include: S1: preparing a sacrificial layer (20) on a precursor (10); S2: transferring the precursor (10) having the sacrificial layer (20) to a temporary substrate (40); S3: attaching the precursor (10) having the sacrificial layer (20) to an assembly substrate (50) by means of the temporary substrate (40); S4: removing the temporary substrate (40) and the sacrificial layer (20).

2. The three-dimensional assembly method using a sacrificial layer to assist debonding according to claim 1, It is characterized in that Before step S3, silicon dioxide (30) is deposited on the precursor (10).

3. The three-dimensional assembly method using a sacrificial layer to assist debonding according to claim 2, It is characterized in that Before step S3, the assembled substrate (50) is subjected to a pre-stretching treatment. In step S3, the silicon dioxide (30) deposited from the precursor (10) is attached to the assembly substrate (50). After removing the temporary substrate (40) and the sacrificial layer (20), the precursor (10) and the assembly substrate (50) are spaced apart or not attached to each other as a whole, and the pre-stretching strain of the assembly substrate (50) is released, so that the precursor (10) is deformed.

4. The three-dimensional assembly method using a sacrificial layer to assist debonding according to claim 1, It is characterized in that The material of the precursor (10) is one or more of a polymer, a metal, a semiconductor, a conductor and a composite material.

5. The three-dimensional assembly method using a sacrificial layer to assist debonding according to claim 1, It is characterized in that The material of the sacrificial layer (20) is one or more of ultraviolet photoresist, polymethyl methacrylate and copper.

6. The three-dimensional assembly method using a sacrificial layer to assist debonding according to claim 1, It is characterized in that The material of the temporary substrate (40) is one or more of polydimethylsiloxane, a thermal release tape and a water-soluble tape; The material of the assembly substrate (50) is one or more of polydimethylsiloxane and silicone.

7. The three-dimensional assembly method using a sacrificial layer to assist debonding according to claim 1, It is characterized in that In step S1, the method for preparing the sacrificial layer (20) includes one or more of the following methods: a: selectively exposing and developing the material for preparing the sacrificial layer (20) through a photolithography mask to prepare the sacrificial layer (20); b: removing part of the material for preparing the sacrificial layer (20) by dry etching under the protection of a hard mask to obtain the sacrificial layer (20); c: Prepare a sacrificial layer (20) by selective deposition through a hard mask.

8. The three-dimensional assembly method using a sacrificial layer to assist debonding according to claim 1, It is characterized in that In step S2, the method of transferring the precursor (10) to the temporary substrate (40) is one or more of a secondary transfer method, a liquid-assisted transfer method, and an electrostatic-assisted transfer method.

9. The three-dimensional assembly method using a sacrificial layer to assist debonding according to claim 1, It is characterized in that In step S3, before attaching the precursor (10) having the sacrificial layer (20) to the assembly substrate (50), the precursor (10) and / or the assembly substrate (50) are subjected to surface activation treatment, and the surface activation treatment method is one or more of ultraviolet light irradiation treatment, corona treatment, and reactive ion etching.

10. The three-dimensional assembly method using a sacrificial layer to assist debonding according to claim 1, It is characterized in that In step S4, the method of removing the sacrificial layer (20) is one or more of a solvent method, an atmosphere method, and an irradiation method.