Easily recyclable absorbent article, and method for manufacturing regenerated raw material, fiber, and fiber product
By melt-kneading and pelletizing the thermoplastic resin in the outer packaging part of the absorbent article, the problem of overall recycling of the outer packaging part in the prior art is solved, and efficient production of recycled raw materials and fibers is achieved. It is suitable for A variety of industrial and daily necessities.
Patent Information
- Application Number
- CN202380031259.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-06
- Filing Date
- 2023-04-05
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art has failed to effectively realize the overall recycling of the outer packaging part of the absorbent article, and recirculates only by incineration or separation of the film, and lacks a complete recycling method for the outer packaging part.
By all the main components in the outer packaging portion of the absorbent article include thermoplastic resin, and by melt-kneading and pelletizing treatment, renewable raw materials or fibers are generated, and the thermoplastic polyurethane elastic wire and hot melt adhesive are treated. The melt viscosity variation coefficient is controlled to be less than 0.5 to realize the overall recycling of the outer packaging part.
The overall recycling of the outer packaging part of the absorbent article is realized, and high-quality recycled raw materials and fibers are generated, which improves the recycling efficiency and productivity of recycled raw materials. It is suitable for a variety of industrial and daily necessities.
Smart Images

Figure CN119031896A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to easily recyclable absorbent articles, and methods for producing recycled raw materials, fibers and fiber products. Background Art
[0002] Conventionally, there is known a technique for recycling used absorbent articles.
[0003] The following patent document 1 discloses a method for efficiently producing recycled pulp that can be recycled into sanitary products and has ash content and antibacterial properties that meet sanitary product standards from used sanitary products, which method is characterized in that it includes: immersing used sanitary products or pulp fibers in an aqueous solution containing ozone, an ozone treatment step for decomposing highly absorbent polymers in the used sanitary products or attached to the pulp fibers, and treating the used sanitary products or pulp fibers with a cationic antibacterial agent before, simultaneously with, or after the ozone treatment step.
[0004] In addition, Patent Document 2 discloses a method for manufacturing a recycled product by collecting the constituent components of used absorbent articles according to their characteristics and recycling them according to their characteristics, as a method for manufacturing a recycled product. The method comprises the following steps: a material separation step of separating a plurality of used absorbent articles into at least a plurality of films and absorbent body materials; a film separation step of separating the separated plurality of films into a plurality of recycling films according to the filler content; and a pellet forming step of forming a plurality of recycled resin pellets corresponding to the filler content using the separated plurality of recycling films.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2016-79525
[0008] Patent Document 2: Japanese Patent Application Publication No. 2018-171780 Summary of the invention
[0009] Problem that the invention aims to solve
[0010] In recent years, it is desired to reduce carbon dioxide and garbage generated in the treatment of waste of absorbent articles, and to add value to the waste by recycling the waste. Absorbent articles are generally composed of an inner packaging part including a surface sheet and an absorbent body, and an outer packaging part including a back sheet and pleats. The mass of the outer packaging part accounts for a large proportion of about 30% of the mass of the entire absorbent article, so it is desired to recycle the outer packaging part.
[0011] However, Patent Document 1 only discloses a method of recovering heat by incinerating the outer packaging as solid fuel (RPF), and does not disclose a technique for recycling the outer packaging.
[0012] Patent Document 2 discloses a method of separating and recycling only a film that is a part of an outer packaging part from among the components of the absorbent material, but does not disclose a technique of recycling the entire outer packaging part without separating it.
[0013] As described above, an absorbent article in which the entire outer cover can be easily recycled or a method for recycling the entire outer cover has not been known so far.
[0014] In view of the problems of the above-mentioned prior art, the problem to be solved by the present invention is to provide an absorbent article whose outer packaging portion can be easily recycled as a whole, a method for producing recycled raw materials or fibers from the absorbent article, and a method for producing fiber products from the fibers.
[0015] Solutions for solving problems
[0016] The present inventors unexpectedly found that the above-mentioned problems can be solved by making all the main members included in the outer packaging of an absorbent article contain a thermoplastic resin, thereby completing the present invention.
[0017] That is, the present invention is as follows.
[0018] [1] An easily recyclable absorbent article, characterized in that it is an absorbent article comprising an inner wrapper and an outer wrapper, wherein the inner wrapper comprises a surface sheet and an absorbent body, and the outer wrapper constitutes a portion other than the inner wrapper and comprises a back sheet and gathers,
[0019] The back sheet comprises a sheet material containing a thermoplastic resin, and
[0020] The pleats include thermoplastic stretch yarns.
[0021] [2] The easily recyclable absorbent article according to [1] above, wherein the outflow start temperature of the thermoplastic elastic yarn is 160° C. or higher and 220° C. or lower.
[0022] [3] The easily recyclable absorbent article according to [1] or [2] above, wherein the thermoplastic elastic yarn is a thermoplastic polyurethane yarn.
[0023] [4] The easily recyclable absorbent article according to any one of [1] to [3] above, wherein the outer packaging portion contains a hot-melt adhesive.
[0024] [5] The easily recyclable absorbent article according to any one of [1] to [4] above, wherein the outer packaging portion includes a thermoplastic film.
[0025] [6] The easily recyclable absorbent article according to any one of [1] to [5], wherein the coefficient of variation of the melt viscosity of the outer packaging part obtained by the following steps is 0.5 or less.
[0026] The outer packaging portion is melt-kneaded to obtain pellets;
[0027] The pellets were placed in the oven of a capillary rheometer set to 230°C for 30 minutes;
[0028] The melt viscosity was measured at a shear rate of 1857 / sec while maintaining the temperature at 230°C.
[0029] The coefficient of variation of the melt viscosity in any 3 minutes from 8 minutes after the start of the measurement to the end of the measurement was calculated.
[0030] [7] An easily recyclable absorbent article according to any one of the above [1] to [6], wherein, with respect to the aforementioned outer packaging portion, the maximum value of the melt viscosity at 200 to 220°C obtained by melt-kneading the outer packaging portion using a flow tester under the conditions of an extrusion load of 49N, a starting temperature of 120°C, and a temperature increase of 3°C / min is divided by the maximum value of the melt viscosity at 200 to 220°C obtained by melt-kneading only the back sheet of the aforementioned outer packaging portion using the same method, and the value is less than 5.0.
[0031] [8] A method for producing a recycled raw material, comprising the following steps:
[0032] (1) a step of melt-kneading at least the outer packaging portion separated from the easily recyclable absorbent article according to any one of [1] to [7] above; and
[0033] (2) A step of pelletizing the product of the above step (1).
[0034] [9] The production method according to [8] above, wherein in the step (1), a raw material is further added.
[0035]
[10] The production method according to [9] above, wherein in the step (1), virgin raw material is added in an amount of 1 to 95% by mass relative to the recycled raw material.
[0036]
[11] A method for producing a recycled raw material, comprising the following steps:
[0037] (i) a step of separating at least the outer packaging portion from the easily recyclable absorbent article according to any one of [1] to [7] above;
[0038] (ii) a step of melt-kneading at least the outer packaging portion separated in the above step (i); and
[0039] (iii) A step of pelletizing the product of the above step (ii).
[0040]
[12] The production method according to [8] above, wherein in the step (ii), a raw material is further added.
[0041]
[13] The production method according to
[12] , wherein in the step (ii), virgin raw material is added in an amount of 1 to 95% by mass relative to the recycled raw material.
[0042]
[14] A method for producing fibers, comprising the step of fiberizing a recycled raw material produced by the production method described in any one of [8] to
[13] .
[0043]
[15] A method for producing a fiber product, comprising: a step of producing the fiber product using the fiber produced by the production method described in
[14] above.
[0044]
[16] A method for producing a fiber, comprising the following steps:
[0045] (A) a step of melt-kneading at least the outer packaging portion separated from the easily recyclable absorbent article according to any one of [1] to [7] above; and
[0046] (B) A step of melt-spinning the product of the above step (A).
[0047]
[17] The production method according to the above
[16] , wherein a raw material is further added in the above step (B).
[0048]
[18] The production method according to
[17] above, wherein in the step (B), virgin raw materials are added in an amount of 1 to 95% by mass relative to the recycled raw materials.
[0049]
[19] A method for producing a fiber, comprising the following steps:
[0050] (a) a step of separating at least the outer packaging portion from the easily recyclable absorbent article according to any one of [1] to [7] above;
[0051] (b) a step of melt-kneading at least the outer packaging portion separated in the above step (a); and
[0052] (c) A step of melt-spinning the product of the step (b).
[0053]
[20] The production method according to the above
[19] , wherein a raw material is further added in the above step (b).
[0054]
[21] The production method according to
[20] , wherein in the step (b), virgin raw materials are added in an amount of 1 to 95% by mass relative to the recycled raw materials.
[0055] Effects of the Invention
[0056] According to the present invention, it is possible to provide an absorbent article in which the entire outer packaging portion can be easily recycled, a method for producing recycled raw materials or fibers from the absorbent article, and a method for producing fiber products from the fibers. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1 This is a diagram showing a configuration example of an easily recyclable absorbent article according to the present embodiment. DETAILED DESCRIPTION
[0058] Hereinafter, embodiments of the present invention will be described in detail. In addition, the present invention is not limited to the following embodiments, and can be implemented in various modifications within the scope of the gist thereof.
[0059] In this specification, "thermoplastic" means that it can be melted by heating at a decomposition temperature or lower, exhibits plastic flow while in a molten state, and has a reversible property of solidifying by cooling.
[0060] In this specification, "recycling" means: reusing products no longer needed in daily life or items derived from industrial activities as resources or recovering / regenerating them for effective use, and refers to material recycling or chemical recycling. For example, recycled raw materials are obtained from used sanitary materials or sanitary materials that failed to meet quality standards during manufacturing.
[0061] One embodiment of the present invention is an easily recyclable absorbent article (hereinafter also referred to as "absorbent article"), characterized in that it is an absorbent article including an inner packaging part and an outer packaging part, the inner packaging part including a surface sheet and an absorbent body, and the outer packaging part constituting a portion other than the inner packaging part and including a back sheet and pleats. The back sheet includes a sheet material containing a thermoplastic resin, and the pleats include thermoplastic elastic yarns.
[0062] The absorbent article of this embodiment is mainly used to absorb and retain body fluids discharged from the body, such as urine, menstrual blood, vaginal discharge, etc. The absorbent article includes, for example, disposable diapers, sanitary napkins, incontinence pads, panty liners, etc., but is not limited to them and widely includes articles for absorbing liquids discharged from the human body.
[0063] The inner wrapping part is a part constituting the wearer side of the absorbent article, and includes a surface sheet and an absorbent body. For the purpose of leakage prevention, the inner wrapping part may include three-dimensional gathers.
[0064] The top sheet is a liquid-permeable sheet that is first received by the absorbent article to receive excreted body fluids, and a conventionally known sheet material such as a spunbonded nonwoven fabric is used.
[0065] The absorbent is a part that absorbs and retains body fluids excreted from the body, and is disposed between the top sheet and the back sheet. The absorbent can be made of conventionally known materials, and typically includes pulp fibers, super absorbent polymers (SAP), and absorbent paper.
[0066] The outer packaging part is a part other than the inner packaging part, and includes a back sheet and pleats. The absorbent article of this embodiment is characterized in that the back sheet includes a sheet material containing a thermoplastic resin, and the pleats include thermoplastic elastic yarns. That is, the absorbent article of this embodiment is characterized in that all the main components included in the outer packaging part include thermoplastic resins. According to this feature, the outer packaging part can be formed into recycled raw materials and fibers by thermoforming the entire part, thereby forming an absorbent article that is easy to recycle.
[0067] The back sheet is a liquid-impermeable sheet for preventing leakage of body fluids retained in the absorbent, and includes a sheet material containing a thermoplastic resin. The back sheet includes sheet materials such as nonwoven fabrics, synthetic resin films, or composite sheets of nonwoven fabrics and synthetic resin films. The sheet material included in the back sheet may include polyolefin resins such as polyethylene and polypropylene, polyamide resins such as 6-nylon and 6,6-nylon, polyester resins such as polyethylene terephthalate (PET) and polybutylene terephthalate (PBT), etc., preferably including polyolefin resins.
[0068] The back sheet may contain an inorganic filler, a pigment, etc. Examples of the inorganic filler contained in the back sheet include calcium carbonate, calcium oxide, zeolite, amorphous aluminosilicate, clay, synthetic silica, titanium oxide, aluminum oxide, barium sulfate, aluminum sulfate, magnesium hydroxide, etc. Among them, calcium carbonate, zeolite, amorphous aluminosilicate, barium sulfate, synthetic silica, and magnesium hydroxide are preferred, and calcium carbonate and barium sulfate are particularly preferred.
[0069] From the viewpoint of ejection stability during melt kneading, the particle size of the inorganic filler is preferably 0.1 μm or more and 30 μm or less, more preferably 1 μm or more and 20 μm or less, and further preferably 3 μm or more and 10 μm or less.
[0070] From the viewpoint of ejection stability when the molten polymer after melt kneading is ejected, the content of the inorganic filler is preferably 20% by mass or less, more preferably 15% by mass or less, further preferably 10% by mass or less, and most preferably 5% by mass or less relative to the mass of the outer packaging portion.
[0071] In the sheet material contained in the back sheet, from the viewpoint of ejection stability when the molten polymer after melt kneading is ejected, the content of the thermoplastic resin with an outflow start temperature of 230°C or above is preferably 30% by mass or less, more preferably 20% by mass or less, further preferably 10% by mass or less, and most preferably 5% by mass or less relative to the mass of the outer packaging portion.
[0072] The gathers are stretchable members having a plurality of pleats, which expand and contract in at least one direction and are arranged at the waist or thigh of the absorbent article. The gathers can be formed by joining a thermoplastic elastic yarn to a part of the back sheet, or by joining a thermoplastic elastic yarn to a sheet material different from the back sheet, and as the different sheet material, a sheet material containing the same thermoplastic resin as the back sheet can be used.
[0073] The thermoplastic elastic yarn contained in the gathers is a thermoplastic and stretchable yarn. As the thermoplastic elastic yarn, for example, an elastic yarn containing a thermoplastic elastomer of a styrene system, an olefin system, a polyester system, and a polyurethane system can be used, preferably an elastic yarn containing a thermoplastic elastomer of a polyurethane system (hereinafter also referred to as "thermoplastic polyurethane elastic yarn").
[0074] The outflow start temperature of the thermoplastic elastic yarn is preferably 160°C or higher, 170°C or higher, or 180°C or higher, and preferably 220°C or lower, 215°C or lower, or 210°C or lower. If the outflow start temperature is 160°C or higher, the heat resistance is sufficiently high, and the yarn is less likely to break due to heat such as when applying a hot-melt adhesive in the manufacturing process of the absorbent article. On the other hand, if the outflow start temperature is 220°C or lower, melting at an excessively high temperature is not required during recycling, and thus thermal decomposition of the polyurethane is less likely to occur. The outflow start temperature is set to the following temperature: using Shimadzu flow tester CFT-500D (manufactured by Shimadzu Corporation), under the conditions of a sample weight of 1.5 g, a die (nozzle) diameter of 0.5 mm, and a thickness of 1.0 mm, an extrusion load of 49 N is applied, and after preheating at an initial set temperature of 120°C for 240 seconds, the temperature is uniformly increased at a rate of 3°C / min. The flow temperature when the polymer starts to flow out is set to the average value of 3 measurements.
[0075] The thermoplastic polyurethane stretch yarn is not particularly limited as long as it has thermoplasticity and contains polyurethane. The thermoplastic polyurethane stretch yarn preferably contains, for example, polyurethane which is a polymer of a polymer polyol, a diisocyanate, and an active hydrogen-containing compound that reacts with an isocyanate group.
[0076] As the polymer polyol used in the polymerization of polyurethane, polyalkylene ether glycol, polyester glycol, and polycarbonate glycol commonly used in the polymerization of polyurethane are preferred, and polyalkylene ether glycol is particularly preferred, and the number average molecular weight is preferably 900 to 3,000. As the polyalkylene ether glycol, those in which the alkylene group is tetramethylene, tetramethylene, and a linear or branched alkylene group having 1 to 8 carbon atoms can be cited. That is, polytetramethylene ether glycol, copolymerized poly(tetramethylene·neopentylene) ether glycol, and copolymerized poly(tetramethylene·2-methylbutylene) ether glycol are preferred.
[0077] As the diisocyanate used in the polymerization of polyurethane, for example, all of the aliphatic diisocyanates, alicyclic diisocyanates and aromatic diisocyanates that are soluble or liquid under the reaction conditions can be used, and specifically, methylene-bis(4-phenylisocyanate), methylene-bis(3-methyl-4-phenylisocyanate), 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, meta-xylylene diisocyanate and para-xylylene diisocyanate, α,α,α',α'-tetramethyl-xylylene diisocyanate, meta-phenylene diisocyanate and para-phenylene diisocyanate, 4,4'-dimethyl-1,3-xylylene diisocyanate, 1-Alkylphenylene-2,4- and 2,6-diisocyanates, 3-(α-isocyanateethyl)phenylisocyanate, 2,6-diethylphenylene-1,4-diisocyanate, diphenyl-dimethylmethane-4,4-diisocyanate, diphenyl ether-4,4'-diisocyanate, naphthalene-1,5-diisocyanate, 1,6-hexamethylene diisocyanate, methylene-bis(4-cyclohexyl isocyanate), 1,3- and 1,4-cyclohexylene diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, and the like, with methylene-bis(4-phenylisocyanate) being particularly preferred.
[0078] As the active hydrogen-containing compound used in the polymerization of polyurethane, for example, a low molecular weight diol can be used, and specifically, ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 2,2-dimethyl-1,3-propylene glycol, 1,4-butanediol, 1,3-butanediol, hexamethylene glycol, diethylene glycol, 1,10-decanediol, 1,3-dihydroxymethylcyclohexane or 1,4-dihydroxymethylcyclohexanehydrazine can be mentioned, and 1,4-butanediol is particularly preferred. In addition, as the active hydrogen-containing compound, an alkanolamine such as monoethanolamine can also be used.
[0079] From the viewpoint of recyclability, the thermoplastic polyurethane stretch yarn preferably has no chemical crosslinking, and particularly preferably has no allophanate bond in which an isocyanate group reacts to crosslink a urethane bond.
[0080] The thermoplastic polyurethane stretch yarn may contain additives such as stabilizers and plasticizers as necessary. Examples of the stabilizer include compounds commonly used in polyurethane resins, such as ultraviolet absorbers, antioxidants, light stabilizers, gas resistance stabilizers, and antistatic agents.
[0081] For the purpose of bonding each component, the outer packaging portion may include a hot melt adhesive. Hot melt adhesives usually contain a base polymer, a tackifier and a plasticizer. As the base polymer, for example, acrylic, silicone or rubber, olefin polymers, etc. can be listed. As the aforementioned acrylic polymer, for example, (co)polymers (ethylene vinyl acetate copolymers, etc.) containing vinyl monomers with 2-ethylhexyl acrylate, butyl acrylate, ethyl acrylate, cyanoacrylate, vinyl acetate, methyl methacrylate, etc. as the main components can be listed. As a silicone polymer, for example, a polydimethylsiloxane polymer can be listed. As the aforementioned rubber polymer, for example, natural rubber, polyisoprene, styrene-butadiene copolymer (SBR), styrene-isoprene-styrene block copolymer (SIS), styrene-butadiene-styrene block copolymer (SBS), styrene-ethylene-butadiene-styrene block copolymer (SEBS), styrene-ethylene-propylene-styrene block copolymer (SEPS) can be listed.
[0082] From the viewpoint of suppressing the adhesion of the outer packaging part separated from the sanitary material in the recycling process and improving the handling property, the content of the hot-melt adhesive is preferably 20 mass % or less, more preferably 15 mass % or less, further preferably 10 mass % or less, and most preferably 5 mass % or less relative to the mass of the outer packaging part.
[0083] The outer packaging portion may include a fastening tape, a fixing material, or the like within a range that does not hinder recyclability, and may also be decorated with printing or the like.
[0084] From the viewpoint of suppressing viscosity fluctuations in the recycling process and improving the productivity (recyclability) of recycled raw materials, the coefficient of variation of the melt viscosity of the outer packaging part obtained by the following steps is preferably 3% or less, more preferably 2% or less, further preferably 1% or less, and most preferably 0.5% or less.
[0085] The outer packaging portion is melt-kneaded to obtain pellets;
[0086] The pellets were placed in the oven of a capillary rheometer set to 230°C for 30 minutes;
[0087] The melt viscosity was measured at a shear rate of 1857 / sec while maintaining the temperature at 230°C.
[0088] The coefficient of variation of the melt viscosity in any 3 minutes from 8 minutes after the start of the measurement to the end of the measurement (hereinafter also referred to as "the coefficient of variation of the melt viscosity") is measured;
[0089] The smaller the coefficient of variation of the melt viscosity, the smaller the change rate of the strand shape, the better the mixing state in the extruder, the smaller the variation of the ejection, and therefore the shape is stable when pelletized and the recyclability is good. In addition, when re-molding such as fiberization is performed using recycled raw materials, the deviation of the viscosity is small and the moldability is good, so the recyclability is good.
[0090] Regarding the outer packaging part, from the viewpoint of suppressing viscosity fluctuations and improving the productivity of recycled raw materials in the recycling process, the maximum value of the melt viscosity of 200-220°C when the pellets obtained by melt-kneading the outer packaging part are measured by a flow tester under the conditions of an extrusion load of 49N, a starting temperature of 120°C, and a temperature rise of 3°C / min is divided by the maximum value of the melt viscosity of 200-220°C when the pellets obtained by melt-kneading only the back sheet in the aforementioned outer packaging part are measured by the same method (hereinafter also referred to as "the ratio of melt viscosity") is preferably 5.0 or less, more preferably 4.0 or less, and further preferably 3.0 or less. The smaller the ratio of the melt viscosity, the smaller the variation rate of the strands, the better the kneading state in the extruder, the smaller the ejection variation, and therefore, the shape is stable when pelletizing, and the recyclability is good. In addition, when remolding such as fiberization is performed using recycled raw materials, the deviation of the viscosity is small, the moldability is good, and therefore, the recyclability is good.
[0091] Another embodiment of the present invention is a method for producing a renewable raw material, which comprises the following steps:
[0092] (1) a step of melt-kneading at least the outer packaging portion separated from the easily recyclable absorbent article; and
[0093] (2) A step of pelletizing the product of the above step (1).
[0094] The outer packaging part used in this embodiment can be separated from the absorbent article by some means, and the separation method is not particularly limited, and a conventionally known method can be used. The absorbent article can be any of a pre-consumer product and a post-consumer product. In addition, the outer packaging part can be cleaned, dried, sterilized, cut and / or crushed before or after separation.
[0095] The outer packaging part is preferably melt-kneaded in a cleaned, dried, sterilized, cut and / or pulverized state. The method of melt-kneading is not particularly limited, and examples thereof include a method using a screw. During melt-kneading, virgin raw materials may be added for the purpose of stabilizing the quality of the recycled raw materials finally obtained. In addition, during melt-kneading, constituent components of the absorbent article other than the outer packaging part containing a thermoplastic resin may be added within a range that does not hinder recyclability, and for example, all constituent components of the absorbent article other than the absorbent body may also be added.
[0096] The product produced by melt kneading is pelletized using a conventionally known method such as a strand cut method, a die face cut method, a flat die method, a ring die method, a heat cut method, a screw method, etc. to provide a recycled raw material.
[0097] Another embodiment of the present invention is a method for producing a renewable raw material, which comprises the following steps:
[0098] (i) a step of separating at least the outer packaging portion from the easily recyclable absorbent article;
[0099] (ii) a step of melt-kneading at least the outer packaging portion separated in the above step (i); and
[0100] (iii) A step of pelletizing the product of the above step (ii).
[0101] In this embodiment, the method of separating the outer packaging part from the absorbent article is not particularly limited, and a conventionally known method can be used. The absorbent article can be any one of a pre-consumer product and a post-consumer product. In addition, the outer packaging part can be cleaned, dried, sterilized, cut and / or crushed before or after separation.
[0102] The outer packaging part is preferably melt-kneaded in a cleaned, dried, sterilized, cut and / or pulverized state. The method of melt-kneading is not particularly limited, and examples thereof include a method using a screw. During melt-kneading, virgin raw materials may be added for the purpose of stabilizing the quality of the recycled raw materials finally obtained. In addition, during melt-kneading, constituent components of the absorbent article other than the outer packaging part containing a thermoplastic resin may be added within a range that does not hinder recyclability, and for example, all constituent components of the absorbent article other than the absorbent body may also be added.
[0103] The product produced by melt kneading is pelletized using a conventionally known method such as a strand cut method, a die face cut method, a flat die method, a ring die method, a heat cut method, a screw method, etc. to provide a recycled raw material.
[0104] In the manufacturing method of the above-mentioned recycled raw materials, strands may be passed through in the granulation process. In the case of passing through strands, from the viewpoint of preventing the strands from being fused and bonded to each other due to the shaking and disorder of the strands, the distance between the strand ejection holes is preferably set to be 5 mm or more, more preferably 7 mm or more, further preferably 10 mm or more, and most preferably 15 mm or more. In addition, the lower limit of the outer diameter of the strand is preferably set to be 2 mm or more, more preferably 4 mm or more, further preferably 6 mm or more, and most preferably 8 mm or more. The upper limit of the outer diameter is preferably 20 mm or less, more preferably 15 mm or less, further preferably 12 mm or less, and most preferably 10 mm or less.
[0105] In the above-mentioned method for producing recycled raw materials, water cooling may be performed in the pelletizing step. When water cooling is performed, the water temperature is preferably maintained at 50° C. or less, more preferably 40° C. or less, further preferably 30° C. or less, and most preferably 20° C. or less, from the viewpoint of reducing the adhesiveness of the polymer discharged after melt kneading and improving the cuttability in pelletizing.
[0106] In the case of water cooling, a water cooling tank can be provided after melt kneading. In the case of providing a water cooling tank, from the viewpoint of preventing the strands from being welded and bonded to each other due to the shaking and disorder of the strands, it is preferred that the height variation of the water surface be set to 100 mm or less, more preferably 80 mm or less, further preferably 50 mm or less, and most preferably 30 mm or less. In addition, in the case of providing a water cooling tank, from the viewpoint of preventing the strands from being welded and bonded to each other due to the shaking and disorder of the strands, it is preferred that the height from the ejection hole of the strand to the water surface of the water cooling tank be set to 500 mm or less, more preferably 300 mm or less, further preferably 100 mm or less, and most preferably 50 mm or less.
[0107] In the above-mentioned method for producing recycled raw materials, in the pelletizing step, from the viewpoint of reducing the stickiness of the strands, the moisture content of the strands immediately before cutting is preferably 20 mass % or less, more preferably 10 mass % or less, further preferably 5 mass % or less, and most preferably 3 mass % or less.
[0108] In addition, the water content was measured according to the following procedure.
[0109] About 100 g of the strands immediately before being fed into the granulator were taken and their mass was precisely weighed.
[0110] The collected strands were placed in a vacuum dryer with the furnace temperature set to 100° C., and the vacuum state was maintained for 12 hours using a vacuum pump, thereby obtaining dried strands.
[0111] Measure the mass of the dried strands and calculate the moisture content using the following formula:
[0112] Water content (mass %)={(mass before drying (g)−mass after drying (g)) / mass after drying (g)}×100.
[0113] When the recycled raw material produced by the above production method is bagged, the pellet temperature during bagging is preferably 60° C. or lower, more preferably 50° C. or lower, further preferably 40° C. or lower, and most preferably 30° C. or lower from the viewpoint of preventing the recycled raw material from sticking.
[0114] The recycled raw materials produced by the above-mentioned production method can be applied to products such as automobile parts, home appliance parts, packaging films, food containers, lids, pallets, containers, shelves, clothing boxes, fibers, medical instruments, daily necessities, and trash cans.
[0115] Another embodiment of the present invention is a method for producing fibers, comprising: a step of fiberizing the recycled raw material produced by the above-mentioned production method. The fiberizing method can use a conventionally known technique, which can be any of wet spinning, dry spinning and melt spinning.
[0116] Another embodiment of the present invention is a method for producing fiber products using the fibers produced by the above-mentioned production method. Here, "fiber products" refer to products containing fibers, and specifically, examples thereof include woven fabrics, knitted fabrics, nonwoven fabrics, clothing, bedding, interior decoration products, daily necessities, fishing nets, ropes, outdoor products, industrial materials, plastics, reinforcement materials such as concrete, and absorbent articles. When absorbent articles are produced by the production method of this embodiment, so-called horizontal recycling is achieved.
[0117] Another embodiment of the present invention is a method for producing a fiber, comprising the following steps:
[0118] (A) a step of melt-kneading at least the outer packaging portion separated from the easily recyclable absorbent article; and
[0119] (B) A step of melt-spinning the product of the above step (A).
[0120] The outer packaging part used in this embodiment can be separated from the absorbent article by some means, and the separation method is not particularly limited, and a conventionally known method can be used. The absorbent article can be any of a pre-consumer product and a post-consumer product. In addition, the outer packaging part can be cleaned, dried, sterilized, cut and / or crushed before or after separation.
[0121] The outer packaging part is preferably melt-kneaded in a cleaned, dried, sterilized, cut and / or pulverized state. The method of melt-kneading is not particularly limited, and examples thereof include a method using a screw. During melt-kneading, virgin raw materials may be added for purposes such as stabilizing the spinning in a subsequent spinning step and stabilizing the quality of the fiber finally obtained. In addition, during melt-kneading, constituent components of the absorbent article other than the outer packaging part containing a thermoplastic resin may be added within a range that does not hinder recyclability, and for example, all constituent components of the absorbent article other than the absorbent body may also be added.
[0122] The product produced by melt kneading is directly melt-spun without being pelletized to provide fibers. As the melt spinning method, a conventionally known method can be used.
[0123] The fibers produced in this manner can be suitably used as reinforcing materials for clothing, bedding, interior decoration products, daily necessities, fishing nets, ropes, outdoor products, industrial materials, plastics, concrete, and the like.
[0124] Another embodiment of the present invention is a method for producing a fiber, comprising the following steps:
[0125] (a) a step of separating at least the outer packaging portion from the easily recyclable absorbent article;
[0126] (b) a step of melt-kneading at least the outer packaging portion separated in the above step (a); and
[0127] (c) A step of melt-spinning the product of the step (b).
[0128] In this embodiment, the method of separating the outer packaging part from the absorbent article is not particularly limited, and a conventionally known method can be used. The absorbent article can be any of a pre-consumer product and a post-consumer product. In addition, the outer packaging part can be cleaned, dried, sterilized, cut and / or crushed before or after separation, and all components of the absorbent article except the absorbent body can also be added, for example.
[0129] The outer packaging part is preferably melt-kneaded in a cleaned, dried, sterilized, cut and / or pulverized state. The method of melt-kneading is not particularly limited, and examples thereof include a method using a screw. During melt-kneading, virgin raw materials may be added for purposes such as stabilizing spinning in a subsequent spinning step and stabilizing the quality of the fiber finally obtained. In addition, during melt-kneading, constituent components of the absorbent article other than the outer packaging part containing a thermoplastic resin may be added within a range that does not hinder recyclability.
[0130] The product produced by melt kneading is directly melt-spun without being pelletized to provide fibers. As the melt spinning method, a conventionally known method can be used.
[0131] The fibers produced in this manner can be suitably used as reinforcing materials for clothing, bedding, interior decoration products, daily necessities, fishing nets, ropes, outdoor products, industrial materials, plastics, concrete, and the like.
[0132] In the melt kneading process of the above-mentioned method for producing recycled raw materials or the method for producing fibers, when virgin raw materials are added, the addition rate is preferably 1% by mass or more, more preferably 10% by mass or more, further preferably 20% by mass or more, particularly preferably 30% by mass, and most preferably 40% by mass, and preferably 95% by mass or less, more preferably 80% by mass or less, further preferably 70% by mass or less, particularly preferably 60% by mass or less, and most preferably 50% by mass or less. If the addition rate of the virgin raw materials is 1% by mass or more, in the case where the shape of the separated outer packaging part is uneven, the bulk density is low, etc., in the raw material input part of the melt kneading process, it is pressed by the weight of the virgin raw materials, and it is not easy to scratch, blockage, etc., and the feeding becomes good. In addition, if the addition rate of the virgin raw materials is 95% by mass or less, the difference in melt viscosity between the outer packaging part and the virgin raw materials becomes small, so that the torque fluctuation during melt kneading is suppressed, the kneading state and the ejection are stable, and a recycled raw material or fiber of uniform shape can be obtained.
[0133] In the above-mentioned method for producing recycled raw materials or the method for producing fibers, in the melt-kneading step, the raw materials of the separated outer packaging part etc. supplied for melt-kneading are preferably cooled, specifically, preferably 60°C or less, more preferably 50°C or less, further preferably 40°C or less, and most preferably 30°C or less. In addition, the raw material input part of the extruder etc. is also preferably cooled, and specifically, the surface temperature of the sliding surface part is preferably 100°C or less, more preferably 80°C or less, further preferably 60°C or less, and most preferably 40°C or less. Since the raw materials and / or the raw material input part of the extruder etc. are cooled, it is easy to suppress the manufacturing failure caused by the following reasons: the outer packaging part is attached to the device at the raw material input part due to the hot melt adhesive contained in the separated outer packaging part, or the outer packaging parts are attached and fixed to each other and no longer fed.
[0134] In the above-mentioned method for producing recycled raw materials or the method for producing fibers, a lubricant may be added in the melt kneading process. The lubricant may be, for example, a metal salt of a fatty acid. When the lubricant is a fatty acid, the carbon number of the fatty acid is preferably 8 to 30, more preferably 11 to 28, and further preferably 12 to 22. As specific examples of the fatty acid, metal salts of stearic acid, palmitic acid, lauric acid, behenic acid, 12-hydroxystearic acid, etc. may be cited. In addition, as metals that form salts with fatty acids, alkali metals such as lithium, potassium, sodium, and alkaline earth metals such as magnesium, calcium, and barium may be cited. For fatty acid metal salts that are particularly suitable as lubricants, calcium stearate may be cited. The lubricant is preferably added in an amount exceeding 0% by mass relative to the mass of the outer packaging portion, and preferably added in an amount of 1% by mass or less, more preferably added in an amount of 0.7% by mass or less, further preferably added in an amount of 0.5% by mass, and most preferably added in an amount of 0.3% by mass or less.
[0135] In the above-mentioned method for producing a recycled raw material or a method for producing a fiber, in the melt kneading step, from the viewpoint of the feedability of the raw material input part, the bulk density of the raw material when it is input into the raw material input part is preferably 0.1 g / cm 3 Above and 1.0g / cm 3 Below, more preferably 0.2g / cm 3 Above and 0.9g / cm 3 Below, more preferably 0.3 g / cm 3 Above and 0.8g / cm 3 Below, most preferably 0.4g / cm 3 Above and 0.7g / cm 3 the following.
[0136] Example
[0137] Hereinafter, the present invention will be specifically described by way of Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0138] First, the evaluation methods used in the following examples will be described.
[0139] <Coefficient of variation of melt viscosity>
[0140] The outer packaging part was melt-kneaded and pelletized to prepare a sample for measurement. Using a capillary rheometer Rheograf20 (manufactured by Goettfert), a 0.5 mm × 5.0 mm capillary die was installed on a barrel with a barrel diameter of 9.55 mm, and the temperature in the furnace was heated to 230°C. About 5 g of the sample was pressed and inserted little by little from the upper part of the barrel without entrapping bubbles. After the sample was inserted, it was placed under a load for 30 minutes, and the melt viscosity at a shear rate of 1857 / second was measured while maintaining it at 230°C. The coefficient of variation of the melt viscosity in any and continuous 3 minutes from 8 minutes after the start of the measurement to the end of the measurement (the sample was ejected without remaining in the barrel, or the piston was pressed to the lower limit of the barrel and the equipment was stopped) was calculated. In addition, the arbitrary 3 minutes are selected within a range that does not include a sharp decrease in pressure that occurs when bubbles are entrapping, a sharp increase in pressure caused by foreign matter scratching the capillary, etc. When the above-mentioned rapid pressure change occurs and it is impossible to ensure any and continuous 3 minutes, the measurement is repeated. The melt viscosity η is obtained by solving the following simultaneous equations (1) to (4). The coefficient of variation (%) is calculated by dividing the standard deviation and the average value of the melt viscosity within any and continuous 3 minutes by the standard deviation.
[0141] Q=Aν…(1)
[0142] γ=32Q / πD 3 …(2)
[0143] τ=PD / 4L…(3)
[0144] η=τ / γ…(4)
[0145] {Where Q is the flow rate of molten resin (mm 3 / s), A is the piston cross-sectional area (mm 2 ), ν is the piston speed (mm / s), γ is the apparent shear velocity (s -1 ), D is the inner diameter of the capillary (mm), τ is the apparent shear stress (Pa), P is the lower barrel pressure (Pa), L is the capillary length (mm), and η is the melt viscosity (Pa·sec).}
[0146] <Outflow start temperature>
[0147] Cut the elastic yarn into appropriate lengths to make samples for measurement. Using Shimadzu flow tester CFT-500D (manufactured by Shimadzu Corporation), apply an extrusion load of 49N under the conditions of a sample weight of 1.5g, a mold (nozzle) diameter of 0.5mm, and a thickness of 1.0mm. After preheating for 240 seconds at an initial set temperature of 120°C, heat uniformly at a rate of 3°C / min to obtain the plunger stroke-temperature curve drawn at this time. As the temperature rises uniformly, the sample is slowly heated and the polymer begins to flow out. The temperature at which the polymer begins to flow out is set to the outflow start temperature. The measurement is performed 3 times, and the average temperature is used as the outflow start temperature.
[0148] <Ratio of Melt Viscosity>
[0149] The outer packaging part and only the back sheet in the outer packaging part were melt-kneaded and pelletized to prepare the samples for measurement, which were respectively provided for the following measurements. Using Shimadzu Flow Tester CFT-500D (manufactured by Shimadzu Corporation), under the conditions of sample weight of 1.5g, die (nozzle) diameter of 0.5mm, and thickness of 1.0mm, an extrusion load of 49N was applied, and after preheating at an initial setting temperature of 120°C for 240 seconds, the temperature was uniformly increased at a rate of 3°C / min, and the piston drop amount (flow amount) when the molten pellets were extruded from the fine hole of the die located at the lower part of the barrel at each time was recorded, and the horizontal axis was set as the drop amount and the vertical axis was set as time to draw the flow curve, and the melt viscosity at 200-220°C was detected. The maximum value of the melt viscosity of the pellets obtained by melt-kneading the outer packaging part was divided by the maximum value of the melt viscosity of the pellets obtained by melt-kneading only the back sheet in the outer packaging part as the ratio of the melt viscosity.
[0150] <Change rate of strand outer diameter>
[0151] In the strand production process of the following embodiment, a biaxial profile measuring instrument LS-9030D manufactured by KEYENCE was set at a position 35 mm below the ejection hole in order to measure the outer diameter of the strand, and the outer diameter of the strand was measured for 1 minute, and the change rate of the outer diameter of the strand was calculated by the following formula:
[0152] Variation rate of outer diameter (%) = {(maximum value of outer diameter - minimum value of outer diameter) / average value of outer diameter} × 100
[0153] In this evaluation, the smaller the variation rate of the strand outer diameter, the better the kneading state in the extruder, the smaller the variation of the ejection, and therefore, the shape is stable when pelletized and the recyclability is good, that is, "easy to recycle". If the variation rate is less than 100%, it can be said that the recyclability is sufficiently good.
[0154] [Comparative Example 1]
[0155] As absorbent articles, commercially available diapers were used. In the outer packaging of the aforementioned diaper, as a back sheet, a back sheet in which a thermoplastic polyethylene film was laminated on a thermoplastic polypropylene nonwoven fabric was used, and the pleats were formed by bonding dry-spun spandex to the back sheet using a styrene-based hot melt adhesive. The aforementioned outer packaging was composed of 75% by mass of polypropylene nonwoven fabric, 16% by mass of polyethylene film, 4% by mass of dry-spun spandex, and 5% by mass of hot melt adhesive relative to the mass of the outer packaging. In addition, the outflow start temperature of the aforementioned dry-spun spandex was 235°C, and it was not thermoplastic. The outer packaging was separated from a plurality of the aforementioned diapers by hand to obtain an outer packaging of about 1.3 kg. The separated outer packaging was heat-pressed at 150°C for 20 seconds through heat-resistant paper, cooled to room temperature, and cut into 5-10 mm square pieces using a cutter to obtain cut pieces of the outer packaging. The cut pieces of the outer packaging part were melt-kneaded at 160°C to 180°C using a twin-screw extruder, extruded into strands from three ejection holes with a hole spacing of 5 mm toward a water cooling tank, and after water cooling, cut using a pelletizer to produce pellets.
[0156] [Example 1]
[0157] In a dry nitrogen atmosphere, 2400 g of polytetramethylene ether glycol having a number average molecular weight of 1800 and 750.75 g of 4,4'-diphenylmethane diisocyanate were reacted at 60°C for 3 hours under stirring to obtain a polyurethane prepolymer terminated with terminal isocyanate. 9 g of AO-60 manufactured by ADEKA as an antioxidant and 9 g of LA-36 manufactured by ADEKA as an ultraviolet absorber were mixed into the reaction solution, and 150.95 g of 1,4-butanediol was further added and stirred for 15 minutes to obtain a polyurethane having a viscosity of 200 Pa·s (30°C).
[0158] Thereafter, the mixture was discharged into a Teflon (registered trademark) tray, and annealed in a hot air oven at 110° C. for 19 hours while the polyurethane was placed in the tray, thereby obtaining a polyurethane resin.
[0159] The polyurethane resin obtained in this way is crushed into a powder of about 3 mm using a pulverizer UG-280 manufactured by HORAI. For the polyurethane resin powder, 0.35 parts by mass of dried ethylene bisstearamide is added, put into the hopper, and melted in the extruder. The gear pump provided at the head is used for metering and pressurization. After filtering with a filter, the powder is ejected at a discharge rate of 31 g / min from a nozzle having a diameter of 0.23 mm and 60 holes at a mold temperature of 210°C. Cold air with a cold air velocity of 0.6 m / s and a cold air temperature of 16°C is blown out from a cold air chamber with a cold air length of 900 mm so that the cold air is in vertical contact with the filaments. The twist was propagated using a ring-type false twisting machine installed at the bottom of 5 m, and the distance from the spinning mouth to the propagation position of the twist, that is, the bundling position was set to 1400 mm. Thereafter, a treatment agent containing polydimethylsiloxane and mineral oil as main components was applied while winding at a speed of 500 m / min to obtain a thermoplastic polyurethane stretch yarn with a single yarn fineness of 10 dtex, a total fineness of 620 dtex, and a flow start temperature of 182° C. The application rate of the treatment agent to the polyurethane stretch yarn was 2 parts by mass.
[0160] Pellets as a recycled raw material were prepared in the same manner as in Comparative Example 1, except that the dry-spun spandex of the diaper used in Comparative Example 1 was replaced with the thermoplastic polyurethane stretch yarn prepared as described above.
[0161] [Example 2]
[0162] The same operation as in Example 1 was performed except that the amount of 4,4'-diphenylmethane diisocyanate was 1134.47 g, the amount of 1,4-butanediol was 292.47 g, and the mold temperature was 230°C to obtain a polyurethane stretch yarn having an outflow start temperature of 220°C. The same operation as in Comparative Example 1 was performed except that the dry-spun spandex of the diaper used in Comparative Example 1 was replaced with the thermoplastic polyurethane stretch yarn produced as above to produce pellets as a recycled raw material.
[0163] [Example 3]
[0164] Pellets as a recycled raw material were prepared in the same manner as in Example 1 except that 10 parts by mass of polypropylene pellets as a virgin raw material were added to 90 parts by mass of the cut pieces of the outer casing portion before melt-kneading.
[0165] [Example 4]
[0166] Pellets as recycled raw materials were prepared in the same manner as in Example 3 except that 50 parts by mass of the virgin raw material was added to 50 parts by mass of the cut pieces of the outer packaging portion.
[0167] [Example 5]
[0168] Pellets as recycled raw materials were prepared in the same manner as in Example 3 except that 80 parts by mass of the virgin raw material was added to 20 parts by mass of the cut pieces of the outer packaging portion.
[0169] [Example 6]
[0170] Pellets as a recycled raw material were prepared in the same manner as in Example 3 except that the distance between the strand ejection holes was set to 10 mm.
[0171] [Example 7]
[0172] Pellets as a recycled raw material were produced in the same manner as in Example 6 except that cooling water was passed through the water cooling tank to maintain the temperature in the water cooling tank at 20 to 22°C.
[0173] [Example 8]
[0174] Pellets as a recycled raw material were prepared in the same manner as in Example 7 except that baffles were provided in the water cooling tank and the positions of water inlet and outlet were adjusted so that the height variation of the water surface was controlled to a maximum of 15 mm.
[0175] [Example 9]
[0176] Pellets as recycled raw materials were prepared in the same manner as in Example 8 except that moisture adhering to the strands was blown off with compressed air from the time the strands left the water cooling tank until they entered the pelletizer, thereby setting the moisture content of the strands immediately before cutting to 5 mass %.
[0177] [Example 10]
[0178] The outer packaging portion was cut without pressurizing, and the bulk density of the cut piece of the outer packaging portion was set to 0.3 g / cm 3 Except for this, the same operation as in Example 8 was carried out to prepare pellets as a recycled raw material.
[0179] With respect to the above-mentioned Comparative Example 1 and Examples 1 to 10, various measurement results are summarized in Table 1 below.
[0180] [Table 1]
[0181]
[0182] As shown in Table 1, in the absorbent articles of Examples 1 to 10 in which the main components of the outer cover are all made of thermoplastic resin, the outer diameter variation rate of the strands is small when pellets as recycled raw materials are produced, and therefore recycling is easy.
[0183] [Evaluation of spinnability of produced pellets]
[0184] The pellets prepared in Comparative Example 1 and Examples 1 to 10 were melt-spun by a known method under the same conditions. Specifically, the prepared pellets were melted by an extruder at 200 to 230°C, metered and pressurized by a gear pump installed on the head, filtered by a filter with a metal mesh of 50 mesh, 200 mesh and 400 mesh overlapped, and then ejected from a nozzle with a diameter of 0.4 mm and 12 holes at a discharge rate of 15 g / min at a mold temperature of 220°C. Cold air with a cold air velocity of 0.6 m / s and a cold air temperature of 16°C was blown out from a cold air chamber with a cold air length of 900 mm so that it was in vertical contact with the filaments. Thereafter, the filaments were wound at a speed of 1000 m / min and spun under conditions that a single filament fineness of 1.3 dtex and a total fineness of 16 dtex could be obtained. When the pellets prepared in Comparative Example 1 were used, the spinning pack pressure increased sharply by 0.3 MPa / min, and the yarns broke frequently at a frequency of once every 3 minutes, and stable spinning could not be performed. On the other hand, when the pellets prepared in Examples 1 to 10 were used, the spinning pack pressure was 0.1 MPa / hour or less, there was no sharp pressure increase, and there was no yarn breakage during the 5-hour spinning, and stable spinning could be performed. It can be seen from this that the absorbent articles of Examples 1 to 10, in which the main components of the outer packaging part all consist of thermoplastic resin, are easy to recycle the outer packaging part.
[0185] Industrial Applicability
[0186] The absorbent article of the present invention can be easily recycled after being discarded, and therefore can be suitably used as an environmentally friendly absorbent article. In addition, the method for producing recycled raw materials and the method for producing fibers of the present invention can be suitably used as a method for obtaining recycled raw materials and fibers from waste of absorbent articles.
[0187] Description of Reference Numerals
[0188] 1. Absorbent articles
[0189] 2 Surface sheet
[0190] 3. Absorber
[0191] 4 back sheet
[0192] 5 pleats
[0193] 6Thermoplastic elastic yarn
[0194] 7. Fixing Materials
Claims
1. An absorbent article that is easily recyclable, It is characterized in that The absorbent article comprises an inner packaging part and an outer packaging part, wherein the inner packaging part comprises a surface sheet and an absorbent body, and the outer packaging part constitutes a part other than the inner packaging part and comprises a back sheet and gathers. The back sheet comprises a sheet material containing a thermoplastic resin, and The pleats include thermoplastic stretch yarns.
2. The absorbent article according to claim 1, in, The thermoplastic elastic yarn has an outflow start temperature of 160° C. or higher and 220° C. or lower.
3. The easily recyclable absorbent article according to claim 1 or 2, in, The thermoplastic elastic yarn is thermoplastic polyurethane yarn.
4. The easily recyclable absorbent article according to claim 1 or 2, in, The outer packaging portion contains a hot melt adhesive.
5. The easily recyclable absorbent article according to claim 1 or 2, in, The outer packaging portion includes a thermoplastic film.
6. The easily recyclable absorbent article according to claim 1 or 2, in, The coefficient of variation of the melt viscosity of the outer packaging portion obtained by the following steps is 0.5 or less: The outer packaging portion is melt-kneaded to obtain pellets; The pellets were placed in the oven of a capillary rheometer set to 230°C for 30 minutes; The melt viscosity was measured at a shear rate of 1857 / sec while maintaining the temperature at 230°C. The coefficient of variation of the melt viscosity in any 3 minutes from 8 minutes after the start of the measurement to the end of the measurement was calculated.
7. The easily recyclable absorbent article according to claim 1 or 2, in, Regarding the outer packaging part, the maximum value of the melt viscosity at 200-220°C obtained by melt-kneading the outer packaging part using a flow tester under the conditions of an extrusion load of 49N, a starting temperature of 120°C, and a temperature increase of 3°C / min is divided by the maximum value of the melt viscosity at 200-220°C obtained by melt-kneading only the back sheet in the outer packaging part using the same method, and the value obtained is 5.0 or less.
8. A method for producing a recycled raw material, comprising the following steps: (1) a step of melt-kneading at least the outer packaging portion separated from the easily recyclable absorbent article according to claim 1 or 2; and (2) A step of pelletizing the product of the step (1).
9. The manufacturing method according to claim 8, in, In the step (1), a raw material is further added.
10. The manufacturing method according to claim 9, in, In the step (1), the virgin raw material is added in an amount of 1 to 95% by mass based on the recycled raw material.
11. A method for producing a recycled raw material, comprising the following steps: (i) a step of separating at least the outer packaging portion from the easily recyclable absorbent article according to claim 1 or 2; (ii) a step of melt-kneading at least the outer packaging portion separated in the step (i); and (iii) A step of pelletizing the product of the step (ii).
12. The manufacturing method according to claim 11, in, In the step (ii), a raw material is further added.
13. The manufacturing method according to claim 12, in, In the step (ii), the virgin raw material is added in an amount of 1 to 95% by mass based on the recycled raw material.
14. A method for producing a fiber, wherein include: A step of fiberizing the recycled raw material produced by the production method according to claim 8. 15 . A method for producing a fiber product, comprising producing the fiber product using the fiber produced by the production method according to claim 14 .
16. A method for producing a fiber, comprising the following steps: (A) a step of melt-kneading at least the outer packaging portion separated from the easily recyclable absorbent article according to claim 1 or 2; and (B) A step of melt-spinning the product of step (A).
17. The manufacturing method according to claim 16, in, In the step (A), a raw material is further added.
18. The manufacturing method according to claim 17, in, In the step (A), the virgin raw material is added in an amount of 1 to 95% by mass based on the recycled raw material.
19. A method for producing a fiber, comprising the following steps: (a) a step of separating at least the outer packaging portion from the easily recyclable absorbent article according to claim 1 or 2; (b) a step of melt-kneading at least the outer packaging portion separated in the step (a); and (c) A step of melt-spinning the product of step (b).
20. The manufacturing method according to claim 19, in, In the step (b), a raw material is further added.
21. The manufacturing method according to claim 20, in, In the step (b), the virgin raw material is added in an amount of 1 to 95% by mass based on the recycled raw material.