Electrode for aluminum electrolysis cell and method for manufacturing same
By preparing TiB2 electrodes with high density, low porosity, and random particle orientation, the problem of easy corrosion of traditional carbon electrodes was solved, and the electrolysis efficiency and safety of aluminum electrolysis units were improved.
Patent Information
- Application Number
- CN202380027959.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-15
- Filing Date
- 2023-03-13
- Publication Date
- 2024-11-26
AI Technical Summary
The carbon electrode material used in existing aluminum electrolysis units is prone to corrosion at high temperatures, resulting in low electrolysis efficiency and high maintenance costs. Furthermore, traditional carbon electrodes pose safety hazards during use.
TiB2 raw materials are used to form predetermined products through pressing, casting and extrusion, and then heated at different temperatures to prepare TiB2 electrodes with specific density, particle size, porosity and particle orientation, which can replace traditional carbon electrodes.
This improved the electrolysis efficiency of the aluminum electrolysis unit, reduced maintenance costs, and enhanced the corrosion resistance and safety of the electrodes.
Smart Images

Figure CN119031990A_ABST
Abstract
Description
Background Art
[0001] An electrolysis cell is a container containing an electrolyte through which an externally generated electric current is passed via a system of electrodes (e.g., an anode and a cathode) to change the composition of the material. For example, aluminum compounds (Al2O3) can be decomposed into pure metallic aluminum (Al) via an electrolysis cell. Traditionally, the electrodes of an aluminum electrolysis cell are made of carbon. Summary of the invention
[0002] Broadly speaking, the disclosure relates to methods for making electrodes for use in electrochemical cells, such as aluminum electrolysis cells or aluminum purification cells. In some embodiments, the methods include forming TiB2 feedstock into a predetermined shaped product to achieve appropriate density, average particle size, interparticle porosity, average pore size, and / or random particle orientation.
[0003] Reference now Figure 1 In one method, the method (100) includes forming a TiB2 feedstock into a predetermined shaped product (110) and producing a final shaped product (130) from the predetermined shaped product. In one embodiment, the predetermined shaped product achieves a density of 40% to 70% of a theoretical density, wherein the theoretical density is the density of pure TiB2. In another embodiment, the density is a preselected density, wherein the predetermined shaped product achieves a preselected density, and wherein the preselected density is 40% to 70% of the theoretical density. In one embodiment, the producing step (130) includes exposing the predetermined shaped product to one or more elevated temperatures. In one embodiment, at least in part due to the exposing step, the final shaped product achieves multiple pores and one or more properties. In one embodiment, reference is now made to Figure 3a , the one or more properties (132) achieved by the final shaped product can be one or more of the following: (i) a density of 85% to 98% of the theoretical density of pure TiB2; (ii) an average particle size of no more than 15 microns; (iii) an interparticle porosity of 1 volume % to 15 volume %; (iv) an average pore size of no more than 120% of the average particle size; and (v) random particle orientation. In another embodiment, the one or more properties (132) achieved by the final shaped product can be pre-selected (i.e., selected before the final shaped product is produced) to include one or more of the foregoing (i) to (v).
[0004] As described above, the TiB2 raw material can be used to form a predetermined shaped product. Figure 2In one embodiment, the TiB2 raw material comprises TiB2 particles (20). In another embodiment, the TiB2 raw material comprises TiB2 granules (30). In yet another embodiment, the TiB2 raw material comprises a combination of TiB2 particles (20) and TiB2 granules (30). In another embodiment, a majority of the TiB2 raw material consists of TiB2 particles (20). In yet another embodiment, a majority of the TiB2 raw material consists of TiB2 granules (30). In another embodiment, the TiB2 raw material consists essentially of TiB2 particles (20). In yet another embodiment, the TiB2 raw material consists essentially of TiB2 granules (30).
[0005] As described above, the method may include forming the TiB2 feedstock into a predetermined shaped product (110). Referring now to Figure 2 In one embodiment, the forming step (110) can be one or more of pressing (114), casting (120) and extruding (126) the TiB2 feedstock to form a predetermined shaped product. In one embodiment, the forming step is performed at ambient temperature. In one embodiment, the forming step (110) includes applying a pressure of at least 5000 psi. In another embodiment, the forming step (110) includes applying a pressure of at least 6000 psi. In yet another embodiment, the forming step (110) includes applying a pressure of at least 7000 psi. In another embodiment, the forming step (110) includes applying a pressure of at least 7500 psi.
[0006] As described above, the forming step (110) may include pressing (114) the TiB2 feedstock into a predetermined shaped product. Figure 2 In one embodiment, the pressing step (114) comprises isostatic pressing (116). In one embodiment, the pressing step (114) comprises pressing at ambient temperature (117). In one embodiment, the pressing step (114) comprises uniaxial dry pressing (118).
[0007] As described above, the forming step (110) may include casting (120) the TiB2 feedstock into a predetermined shaped product. Figure 2 In one embodiment, the casting step (120) comprises slip casting (122). In another embodiment, the casting step (120) comprises tape casting (124).
[0008] As described above, the predetermined shaped product formed from the TiB2 feedstock can achieve a density of 40% to 70% of the theoretical density of pure TiB2. In one embodiment, the predetermined shaped product achieves a density of at least 45% of the theoretical density of pure TiB2. In another embodiment, the predetermined shaped product achieves a density of at least 50% of the theoretical density of pure TiB2. In yet another embodiment, the predetermined shaped product achieves a density of at least 55% of the theoretical density of pure TiB2. In another embodiment, the predetermined shaped product achieves a density of at least 58% of the theoretical density of pure TiB2. In yet another embodiment, the predetermined shaped product achieves a density of at least 60% of the theoretical density of pure TiB2. In one embodiment, the predetermined shaped product achieves a density of no greater than 68% of the theoretical density of pure TiB2.
[0009] As described above, the method may include producing a final shaped product from a predetermined shaped product (130). Referring now to Figure 1 and Figure 3c In one embodiment, the producing step (130) includes heating the predetermined shaped product at a first temperature for a first time period (140). In one embodiment, the producing step includes heating the predetermined shaped product at a second temperature for a second time period (144). In one embodiment, the second temperature is higher than the first temperature.
[0010] As mentioned above, continue to refer to Figure 1 and Figure 3c , the producing step (130) may include heating the predetermined shaped product for a first time at a first temperature for a first time period (140), and the heating may be performed isothermally or non-isothermally. In one embodiment, the first temperature is at least 200°C (141). In another embodiment, the first temperature is at least 300°C. In yet another embodiment, the first temperature is at least 400°C. In another embodiment, the first temperature is at least 500°C. In one embodiment, the first time period is at least 1 minute (143). In another embodiment, the first time period is at least 10 minutes. In yet another embodiment, the first time period is at least 30 minutes. In another embodiment, the first time period is at least 60 minutes. In one embodiment, the first temperature is not greater than 1200°C. In one embodiment, the first time period is not greater than 48 hours. In one embodiment, the first heating step is performed for a first time period at a first temperature, and the first temperature is sufficient to remove volatile compounds (e.g., organic matter), and the presence of volatile compounds may be undesirable during a subsequent heating step (such as the second heating step described herein).
[0011] As mentioned above, continue to refer to Figure 1 and Figure 3c, the producing step (130) may include heating the predetermined shaped product for a second time at a second temperature for a second time period (144), and the heating may be performed isothermally or non-isothermally. In one embodiment, the second temperature is at least 1600°C (145). In another embodiment, the second temperature is at least 1700°C. In yet another embodiment, the second temperature is at least 1800°C. In another embodiment, the second temperature is at least 1825°C. In one embodiment, the second time period is at least 1 minute. In another embodiment, the second time period is at least 10 minutes. In yet another embodiment, the second time period is at least 30 minutes. In another embodiment, the second time period is at least 1 hour (147). In yet another embodiment, the second time period is at least 4 hours. In another embodiment, the second time period is at least 8 hours. In yet another embodiment, the second time period is at least 12 hours. In one embodiment, the second temperature is not greater than 2300°C. In one embodiment, the second time period is not greater than 96 hours.
[0012] As described above, the generating step (130) may include heating the predetermined shaped product for a first time at a first temperature for a first time period (140). In one embodiment, the first heating includes heating from an initial temperature to the first temperature at a first heating rate. In one embodiment, the initial temperature is ambient temperature. In one embodiment, the first heating rate is no greater than 10°C / minute. In another embodiment, the first heating rate is no greater than 8°C / minute. In yet another embodiment, the first heating rate is no greater than 6°C / minute. In another embodiment, the first heating rate is no greater than 5°C / minute.
[0013] As described above, the producing step (130) may include heating the predetermined shaped product for a second time at a second temperature for a second period of time (144). In one embodiment, the second heating includes heating from the first temperature to the second temperature at a second heating rate. In one embodiment, the second heating rate is no greater than 8°C / minute. In another embodiment, the second heating rate is no greater than 7°C / minute. In yet another embodiment, the second heating rate is no greater than 6°C / minute. In another embodiment, the second heating rate is no greater than 5°C / minute.
[0014] As mentioned above, continue to refer to Figure 1 and Figure 3b, the final molded product produced by the predetermined molded product can achieve one or more of the following properties (132): (i) a density of 85% to 98% of the theoretical density of pure TiB2; (ii) an average particle size of no more than 15 microns; (iii) an interparticle porosity of 1 volume % to 15 volume %; (iv) an average pore size of no more than 120% of the average particle size; and (v) random particle orientation (132). In one embodiment, the final molded product achieves at least two of (i) to (v). In another embodiment, the final molded product achieves at least three of (i) to (v). In yet another embodiment, the final molded product achieves at least four of (i) to (v). In another embodiment, the final molded product achieves all of (i) to (v).
[0015] As described above, the final molded product produced from the predetermined molded product can achieve an average particle size of no greater than 15 microns. Figure 3b In one embodiment, the final molded product achieves an average particle size (133) of no more than 12 microns. In another embodiment, the final molded product achieves an average particle size (133) of no more than 10 microns. In yet another embodiment, the final molded product achieves an average particle size (133) of no more than 8 microns. In another embodiment, the final molded product achieves an average particle size (133) of no more than 6 microns. In yet another embodiment, the final molded product achieves an average particle size (133) of no more than 4 microns.
[0016] As described above, the final shaped product produced from the predetermined shaped product can achieve an interparticle porosity of 1% to 15% by volume. Figure 3b In one embodiment, the final molded product achieves an interparticle porosity (134) of no more than 14% by volume. In another embodiment, the final molded product achieves an interparticle porosity of no more than 13% by volume. In one embodiment, the final molded product achieves an interparticle porosity (135) of at least 2% by volume. In another embodiment, the final molded product achieves an interparticle porosity of at least 4% by volume. In yet another embodiment, the final molded product achieves an interparticle porosity of at least 6% by volume. In another embodiment, the final molded product achieves an interparticle porosity of at least 8% by volume.
[0017] As described above, the final molded product produced from the predetermined molded product can achieve an average pore size of no greater than 120% of the average particle size. Figure 3bIn one embodiment, the final molded product achieves an average pore size (136) of no more than 110% of the average particle size. In another embodiment, the final molded product achieves an average pore size of no more than 100% of the average particle size. In yet another embodiment, the final molded product achieves an average pore size of no more than 90% of the average particle size. In another embodiment, the final molded product achieves an average pore size of no more than 80% of the average particle size. In yet another embodiment, the final molded product achieves an average pore size of no more than 70% of the average particle size. In another embodiment, the final molded product achieves an average pore size of no more than 60% of the average particle size. In yet another embodiment, the final molded product achieves an average pore size of no more than 50% of the average particle size.
[0018] As described above, the method may include producing a final formed product (130) from a predetermined formed product. In one embodiment, the final formed product achieves an ODF strength of no more than 3 times random. In another embodiment, the final formed product achieves an ODF strength of no more than 2.75 times random. In yet another embodiment, the final formed product achieves an ODF strength of no more than 2.5 times random. In another embodiment, the final formed product achieves an ODF strength of no more than 2.25 times random. In yet another embodiment, the final formed product achieves an ODF strength of no more than 2.0 times random. In another embodiment, the final formed product achieves an ODF strength of no more than 1.75 times random. In yet another embodiment, the final formed product achieves an ODF strength of no more than 1.5 times random.
[0019] As described above, the method may include forming the TiB2 feedstock into a predetermined shaped product (110). Referring now to Figure 4 to Figure 5b and Figure 7 In one embodiment, the method includes preparing a TiB2 feedstock (90) for forming step (110). In one embodiment, the preparing step (90) includes spray drying the slurry (80) to produce TiB2 particles (92). In one embodiment, the slurry (80) includes a TiB2 powder (82) and a liquid medium. In one embodiment, the slurry (80) includes at least one of a dispersant (84) and a binder (86). In one embodiment, the binder (86) includes an organic binder. In one embodiment, due to one or more of the dispersant (86) and the binder (86), the TiB2 particles achieve one or more properties as described below.
[0020] As described above, the TiB2 particles can achieve one or more properties due to one or more of the dispersant and the binder. Figure 5bIn one embodiment, one or more properties of the TiB2 particles may be one or more of the following: (i) a D of not greater than 200 microns; 90 (93); (ii) D of at least 10 μm 10 (94); (iii) 1.0 g / cm 3 Up to 1.8g / cm 3 (iv) a liquid medium content of not more than 0.5 wt% (96); and (v) a flow rate of at least 0.2 g / s (97). In another embodiment, the TiB2 particles achieve at least two of (i) to (v). In yet another embodiment, the TiB2 particles achieve at least three of (i) to (v). In another embodiment, the TiB2 particles achieve at least four of (i) to (v). In yet another embodiment, the TiB2 particles achieve all of (i) to (v). In another embodiment, one or more properties achieved by the TiB2 particles can be pre-selected (i.e., selected before the TiB2 particles are produced), including one or more of the aforementioned (i) to (v).
[0021] As described above, the method may include preparing a TiB2 feedstock (90) for forming step (110). Referring now to Figure 6 In one embodiment, the method includes deagglomerating the TiB2 powder (50) prior to the preparing step (90). In one embodiment, the method includes deagglomerating the first TiB2 powder to produce a second TiB2 powder. In one embodiment, the method includes combining the deagglomerated TiB2 powder with a liquid medium to form a slurry (80). In one embodiment, the combining step (70) precedes the preparing step (90). In one embodiment, the slurry (80) includes the deagglomerated TiB2 powder and at least one of a dispersant (84) and a binder (86). In one embodiment, the binder (86) includes an organic binder.
[0022] As described above, prior to the preparing step (90), the method may include a deagglomeration step (50), and the deagglomeration step (50) may include deagglomerating the first TiB2 powder to produce a second TiB2 powder. Figure 7 In one embodiment, the deagglomerated TiB2 powder can achieve one or more of the following properties: (i) a D 50 ; (ii) 1.0m 2 / g to 3.0m 2 / g surface area; (iii) no more than 5.0 wt% O, or no more than 4 wt% O, or no more than 3 wt% O, or no more than 2.5 wt% O, or no more than 2.0 wt% O, or no more than 1.5 wt% O, or no more than 1 wt% O; (iv) no more than 5.0 wt% C, or no more than 4 wt% C, or no more than 3 wt% C, or no more than 2.5 wt% C, or no more than 2.0 wt% C, or no more than 1.5 wt% C, or no more than 1 wt% C; and (v) irregular particle morphology. In another embodiment, the deagglomerated TiB2 powder achieves at least two of (i) to (v). In yet another embodiment, the deagglomerated TiB2 powder achieves at least three of (i) to (v). In another embodiment, the deagglomerated TiB2 powder achieves at least four of (i) to (v). In yet another embodiment, the deagglomerated TiB2 powder achieves all of (i) to (v). In another embodiment, one or more properties achieved by the deagglomerated TiB2 powder may be pre-selected (i.e., selected before the deagglomeration step (50)) to include one or more of the aforementioned (i) to (v).
[0023] As described above, the method can include producing a final shaped product from a predetermined shaped product (130). In one method, the final shaped product is an electrode. In one embodiment, the electrode is a cathode. In another embodiment, the electrode is an anode.
[0024] In one embodiment, the electrochemical cell comprises a final shaped product in the form of an electrode. The electrochemical cell may comprise any number and type of final shaped products in the form of an electrode, i.e., the electrochemical cell may comprise therein any number of final shaped products in the form of an anode and / or a cathode. In one embodiment, the electrochemical cell is an aluminum electrolysis cell. In another embodiment, the electrochemical cell is an aluminum purification cell.
[0025] In one embodiment, the method may include using the final shaped product as an electrode in an electrochemical cell. In one embodiment, the electrochemical cell is an aluminum electrolysis cell, wherein the final shaped product is an electrode, and the electrode is used to produce aluminum metal in the aluminum electrolysis cell (e.g., as an anode and / or cathode). In another embodiment, the electrochemical cell is an aluminum purification cell, wherein the final shaped product is an electrode, and the electrode is used to produce aluminum in the aluminum purification cell (e.g., as an anode and / or cathode).
[0026] definition
[0027] The TiB2 powder may have a median particle size. As used herein, "median particle size" is defined according to ASTM B822. The median particle size value of the TiB2 powder is measured using a Malvern Mastersizer 2000 according to ASTM B822. As described above, the TiB2 powder may have a surface area. The surface area value of the TiB2 powder is measured using a Micromeritics Tristar II Plus according to ASTM C1274. As described above, the TiB2 powder may have an oxygen content and a carbon content. The oxygen content of the TiB2 powder is measured using a LECO ON836 according to ASTM1409. The carbon content of the TiB2 powder is measured using a LECO CS844 according to ASTM E1915.
[0028] As described above, the TiB2 powder can have an irregular particle morphology. As used herein, the term "irregular particle morphology" means that the particles are angular and have no specific shape, that is, no regular / repeating geometric shapes are seen in scanning electron micrographs of TiB2 powders having irregular morphology. As described above, the TiB2 particles can have a PSD D90 or PSDD10. As used herein, "particle size distribution" or "PSD" refers to the relative amount of particles present classified according to the number of sizes present. For example, a PSD D10 of 7 microns means that 10% of the particles are less than about 7 microns, and 90% of the particles are equal to or greater than about 7 microns. For another example, a PSD D50 of 12 microns means that half of the particles are less than about 12 microns, and the other half are equal to or greater than about 12 microns, and a PSD D90 of 20 microns means that 90% of the particles are less than about 20 microns, and 10% of the particles are equal to or greater than about 20 microns. Typically, when referring to the same material, the particle size distribution D10 to D90 will be on an upward trend (i.e., the D90 value is greater than both the D50 value and the D10 value, and the D50 value is greater than the D10 value). Although D10, D50, and D90 are mentioned herein, it is readily appreciated that when measuring particle size, the PSD can be any useful PSD and is not limited to D10, D50, and D90 values. The particle size distribution values of TiB2 powders are measured according to ASTM B214.
[0029] As described above, the TiB2 particles can have a bulk density, a moisture content, and a flow rate. The bulk density of the TiB2 particles was measured according to ASTM D7481. The moisture content of the TiB2 particles was measured using a Mettler Toledo Moisture Analyzer HE53. The flow rate of the TiB2 particles was measured according to ASTM B213.
[0030] As described above, the predetermined shaped product (eg, a green electrode) may have a density. The density of the predetermined shaped product is calculated using the total mass and dimensions of the predetermined shaped product.
[0031] As described above, the final shaped product (eg, TiB2 board) may have a density. The density of the final shaped product is measured according to ASTM B962.
[0032] As described above, the predetermined shaped product and the final shaped product may have a theoretical density. Theoretical density (ρtheoretical) is the highest density that a material can achieve, calculated from atomic weight and crystal structure.
[0033]
[0034] Where: Nc = number of atoms in the unit cell
[0035] A = atomic weight [kg mol-1]
[0036] Vc = unit cell volume [m3]
[0037] NA = Avogadro's constant [atoms mol-1]
[0038] For the purposes of this patent application, the theoretical density is 4.52 g / cc, which is the approximate theoretical density of pure TiB2.
[0039] As described above, the final molded product can have an average particle size and an average pore size. As used herein, "average particle size" and "average pore size" are defined in accordance with ASTM E112. As used herein, "pores" refer to openings or voids that are typically small (e.g., <1 cm) formed as a result of exposing a predetermined molded product to one or more elevated temperatures. As used herein, "porosity" refers to the ratio of the volume of pores in a material to the volume of the material. As used herein, "interparticle porosity" refers to the porosity between TiB2 particles, which is in contrast to "intraparticle porosity", which refers to the porosity within the TiB2 particles.
[0040] As described above, the final formed product is analyzed via scanning electron microscopy. Scanning electron microscopy is performed using a JOEL SEM instrument or other suitable SEM. Samples for SEM analysis are prepared by first obtaining sections of the plate via electron discharge machining, diamond saw cutting, or other appropriate machining methods. Then, the sample is mounted and ground using diamond, silicon carbide, or other abrasive media until the sample is flat. Finally, the sample is polished to an acceptable finish using diamond, silicon carbide, aluminum oxide, silicon dioxide, or other polishing media.
[0041] The samples were analyzed via scanning electron (SE) mode and electron backscatter diffraction (EBSD) mode. The average particle size of the final molded product was measured using SEM with EBSD mode via orientation imaging microscopy (OIM) analysis. In brief, the EBSD pattern was obtained by tilting the sample to about 70 ° and obtaining the diffraction pattern of the sample. The obtained Kikuchi pattern was analyzed to obtain particle orientation information.
[0042] As described above, the final molded product can have an average pore size. The average pore size and the volume % of the intergranular and intragranular porosity are measured on the SEM micrograph according to the modified procedure of ASTM E112§13 (linear intercept method). In short, three lines are drawn on the SEM micrograph. The length of each hole intersecting with each line is measured. The OIM image is used to determine whether each measured hole is an intergranular hole or an intragranular hole. The average value of these lengths is calculated to obtain the average intergranular pore size and the average intragranular pore size. The intergranular pore lengths are added to obtain the sum of the intergranular pores. The intragranular pore lengths are added to obtain the sum of the intragranular pores. Then, all measured pore lengths are added to obtain the sum of all pore lengths. The volume % of the intergranular and intragranular porosity is calculated from the above values. The total pore volume is calculated by dividing the sum of all pore lengths by the sum of all three line lengths.
[0043] As used herein, "random particle orientation" means that the particles have no or limited preference for aligning in a particular direction, ie, the crystallographic orientation of a particle is independent of the crystallographic orientation of its neighboring particles.
[0044] The distribution of crystallographic orientations within a polycrystalline TiB2 sample can be determined from an inverse pole figure. An inverse pole figure is a stereographic projection in which the orientation is aligned with one of the known axes of the identified crystal structure of the specimen.
[0045] The inverse pole figure is derived from the electron backscatter pattern produced in a scanning electron microscope, in which the intersecting bands of diffracted electrons represent the crystal planes of the crystalline sample.
[0046] The diffracted beam produces a pattern of intersecting bands, called electron backscatter patterns. These patterns can be used to determine the orientation of the crystal lattice with respect to a specific crystal direction.
[0047] The measured intensity of the represented crystallographic orientation is usually normalized by calculating a background intensity or random intensity and comparing the background intensity to the intensity of the orientation present in the image.
[0048] Orientation imaging microscopy (OIM) uses electron backscatter patterns to analyze the orientation of each crystallite or grain imaged in a sample.
[0049] OIM analysis can determine the background (random) intensity and use the orientation distribution function (ODF) to produce relative ODF intensity values for the imaged population of crystallites of the sample.
[0050] A series of ODF plots containing intensity (time-random) representations can be created for the imaged sample.
[0051] The ODF map contains the maximum intensity levels relative to a predetermined scale and can be used as a quantitative measure of the degree of orientation between individual crystallites of a polycrystalline sample.
[0052] Relative to a population of individual crystallites of a sample, a higher ODF intensity indicates a high degree of crystalline orientation between crystallites within the sample, and a lower ODF intensity indicates a lower degree of orientation.
[0053] As described above, the disclosed final shaped product in the form of an electrode can be used in an aluminum electrolysis cell. As used herein, an "aluminum electrolysis cell" is a cell in which the cathode is located at the bottom of the cell, the anode is located at the top of the cell, and the produced aluminum moves to the bottom of the cell. An example of an aluminum electrolysis cell can be found in commonly owned U.S. Patent Publication No. 2017 / 0283968, filed on March 30, 2017, entitled "Apparatuses and Systems for Vertical Electrolysis Cells."
[0054] As described above, the disclosed final shaped product in the form of an electrode can be used in an aluminum purification unit. As used herein, an "aluminum purification unit" is a unit in which the cathode is located at the top of the unit, the anode is located at the bottom of the unit, and the purified aluminum moves to the top of the unit. An example of an aluminum purification unit can be found in commonly owned U.S. Patent No. 10,407,786, filed on February 11, 2016, entitled "Systems and Methods for Purifying Aluminum."
[0055] The above examples are intended to illustrate the present invention and should not be construed as limiting the present invention in any way.
[0056] Reference is now made to the accompanying drawings, which at least partially illustrate various relevant features of the technology disclosed herein. The drawings shown are not necessarily drawn to scale, but generally focus on illustrating the principles of the present invention. In addition, some features may be exaggerated to illustrate the details of specific components. In addition, any measurements, specifications, etc. shown in the drawings are intended to be illustrative and not restrictive. Therefore, the specific structural and functional details disclosed herein should not be interpreted as limiting, but only as a representative basis for teaching those skilled in the art to use the present invention in various ways.
[0057] In addition to those benefits and improvements already disclosed, other objects and advantages of the present invention will become apparent from the following description in conjunction with the accompanying drawings. Detailed embodiments of the present invention are disclosed herein; however, it should be understood that the disclosed embodiments are merely illustrative of the present invention that can be implemented in various forms. In addition, each example given in conjunction with various embodiments of the present invention is intended to be illustrative and not restrictive.
[0058] Throughout the specification and claims, the following terms take the meanings clearly associated with this document unless the context clearly dictates otherwise. As used herein, the phrases "in one embodiment" and "in some embodiments" do not necessarily refer to the same embodiment, although they may refer to the same embodiment. In addition, as used herein, the phrases "in another embodiment" and "in some other embodiments" do not necessarily refer to different embodiments, although they may refer to different embodiments. Therefore, as described below, various embodiments of the present invention can be easily combined without departing from the scope or spirit of the present invention.
[0059] In addition, as used herein, the term "or" is an inclusive "or" operator and is equivalent to the term "and / or", unless the context clearly dictates otherwise. The term "based on" is not exclusive and allows for being based on additional factors that are not described, unless the context clearly dictates otherwise. In addition, throughout the specification, the meanings of "a", "an", and "the" include plural references. The meaning of "in" includes "in" and "on".
[0060] These and other aspects, advantages and novel features of the new technology of the present invention are set forth in part in the description that follows and will become apparent to those skilled in the art after studying the following description and drawings, or may be learned by practicing one or more embodiments of the technology provided in the disclosure.
[0061] Although the disclosure generally relates to products (e.g., electrodes) and methods of making products for use in aluminum electrochemical cells (such as aluminum electrolysis cells or aluminum purification cells), the products and methods described herein are applicable to other electrochemical cells (such as magnesium electrolysis cells or magnesium purification cells). BRIEF DESCRIPTION OF THE DRAWINGS
[0062] This patent or application file contains at least one drawing drawn in color. Copies of this patent or patent application publication with color drawing(s) will be provided by the Office upon request and payment of the necessary fee.
[0063] Figure 1 is a flow chart illustrating one embodiment of a method of producing a final shaped product (130).
[0064] Figure 21 is an embodiment showing the step of forming a TiB2 raw material into a predetermined shaped product (110).
[0065] Figure 3a is a flow chart illustrating one embodiment of the properties (132) of the final formed product.
[0066] Figure 3b is a flow chart showing one embodiment of the properties (133 to 136) of the final shaped product.
[0067] Figure 3c is a flow chart illustrating one embodiment of a method of heating a predetermined shaped product (140, 144).
[0068] Figure 4 is a flow chart illustrating one embodiment of a method of producing a final shaped product (130).
[0069] Figure 5a is a flow chart showing one embodiment of a method for preparing a TiB2 feedstock (90).
[0070] Figure 5b is a flow chart showing one embodiment of the properties (93 to 97) of the raw materials for TiB2 particles.
[0071] Figure 6 is a flow chart illustrating one embodiment of a method of producing a final shaped product (130).
[0072] Figure 7 is a flow chart showing one embodiment of a method of producing a final shaped product (130), and the components (82, 84, 86) of a slurry used in preparing a TiB2 feedstock, and the properties (52) of a deagglomerated TiB2 powder.
[0073] Figure 8 is a SEM micrograph of an exemplary embodiment of a TiB2 electrode fabricated according to the disclosure.
[0074] Figure 9a is a SEM micrograph of an exemplary embodiment of a TiB2 electrode fabricated in accordance with the disclosure and analyzed using OIM analysis.
[0075] Figure 9b is from Figure 9a The corresponding particle size analysis results obtained from the OIM analysis in .
[0076] Fig.10a is a SEM micrograph of a comparative example of a TiB2 electrode not according to the invention, which was made according to the disclosure and analyzed using OIM analysis.
[0077] Fig.10b is from Fig.10a The corresponding particle size analysis results obtained from the OIM analysis in .
[0078] Fig.11a is a SEM micrograph of an exemplary embodiment of a major surface of a TiB2 electrode fabricated in accordance with the disclosure and analyzed using OIM analysis.
[0079] Fig.11b is a SEM micrograph of an exemplary embodiment of a second face orthogonal (perpendicular) to the major face of a TiB2 electrode fabricated in accordance with the disclosure and analyzed using OIM analysis.
[0080] Fig.12a is an inverse pole figure generated from an OIM analysis of an exemplary embodiment of a major surface of a TiB2 electrode fabricated according to the disclosure.
[0081] Figure 12b is an inverse pole figure generated from an OIM analysis of an exemplary embodiment of a second face orthogonal (perpendicular) to the major face of a TiB2 electrode fabricated according to the disclosure.
[0082] Fig.13a is a SEM micrograph of a comparative example of the main surface of a TiB2 electrode not according to the invention, manufactured according to the disclosure and analyzed using OIM analysis.
[0083] Fig.13b is a SEM micrograph of a comparative example of a second face orthogonal (perpendicular) to the main face of a TiB2 electrode not according to the invention, manufactured according to the disclosure and analyzed using OIM analysis.
[0084] Fig.14a is an inverse pole figure generated from an OIM analysis of a comparative example of a major surface of a non-inventive TiB2 electrode fabricated according to the disclosure.
[0085] Fig.14b is an inverse pole figure generated from an OIM analysis of a comparative example of a second face orthogonal (perpendicular) to the major face of a TiB2 electrode not of the present invention fabricated according to the publication. DETAILED DESCRIPTION
[0086] Example
[0087] Two plates were made, one according to the invention and one not according to the invention. The plates according to the invention are described in further detail below. A first powder having TiB2 particles was deagglomerated to produce a second powder having TiB2 particles. The deagglomeration was accomplished by air flow milling. The properties of the second powder were measured. The results are shown below:
[0088] Median particle size is 1.8μm to 2.6μm
[0089] Surface area: 1.5m 2 / g to 2.5m 2 / g
[0090] Oxygen content not more than 1.25% by weight
[0091] Carbon content is not more than 1.0% by weight
[0092] Irregular particle shape
[0093] The deagglomerated TiB2 powder is then mixed with water, a dispersant and a binder to form a slurry. The slurry is then spray dried to form TiB2 particles having the following properties:
[0094] D90 less than 200μm
[0095] D10 is at least 20 μm
[0096] Bulk density is 1.0g / cc to 1.8g / cc
[0097] Water content less than 0.5% by weight
[0098] • The flow rate is at least 0.2 g / s.
[0099] About 10 kg of the spray-dried TiB2 particles were transferred to a 26.5 inch x 14.5 inch mold. Then, a pressure of 7500 psi was applied to the mold at room temperature to form a green electrode (eg, a predetermined shaped product). The density of the green electrode was about 60% of the theoretical density of TiB2.
[0100] The green electrode is then sintered by first heating to 500°C at a rate of 5°C / min, then holding at 500°C for one hour, then heating to 1825°C at a rate of 5°C / min, and then holding at 1825°C for 12 hours to produce a final TiB2 plate (e.g., a final shaped product) (130). After holding at 1825°C, the final TiB2 plate is cooled in the furnace until it reaches ambient temperature. The density of the final TiB2 plate is measured to be 4.10 g / cc (90.7% of the theoretical density of TiB2).
[0101] Figure 8 A SEM micrograph of a typical TiB2 plate made by the above process is shown. As shown, the holes (820) are evenly distributed throughout the plate area (810). Figure 8 In the plate shown, the pores account for about 10% of the total plate area. The plate also includes a non-TiB2 secondary phase (830) that does not react with aluminum, which accounts for about 2% of the TiB2 plate by volume. The pore sizes shown in the SEM were calculated by the linear intercept method, and the results are shown in Table 1 below.
[0102] Table 1: Pore sizes of exemplary inventive plates
[0103] Hole Type Average pore size (micrometers) Pore diameter standard deviation (micrometer) Intergranular 1.53 1.04 Intragranular 0.6 0.43
[0104] Figure 9a SEM micrographs analyzed using OIM analysis are shown. As shown, there are evenly distributed pores (920) throughout the plate. OIM analysis is used to determine whether the pores are inter-particle pores or intra-particle pores. The analysis shows that 96.4% of the pores are inter-particle pores, while 3.6% of the pores are intra-particle pores. Figure 9a It is also shown that the plate is composed of TiB2 particles (940). The average particle size was determined using OIM analysis and is shown in Figure 9b The average particle size of the plate was measured to be 2.86 μm ± 1.46. The pore size and particle size results show that the average pore size of the plate is smaller than the average particle size.
[0105] Fig.11a and Fig.11b Particle orientation determined by OIM analysis of a major face and a second face orthogonal (perpendicular) to the major face are shown, respectively. In an exemplary embodiment, the major face is orthogonal to the pressing direction. Fig.12a and Figure 12b The inverse pole figures generated from the OIM analysis for the primary and secondary faces are shown, respectively. As shown, the grains in both the primary and secondary faces are similarly randomly oriented.
[0106] Non-inventive plates were made via conventional methods (e.g., uniaxial hot pressing). TiB2 powder was loaded between two graphite plates in a graphite mold. Uniaxial pressure was applied to the major faces of the graphite plates while the graphite mold was heated to greater than 1800°C. The TiB2 powder was densified to a near-final molded product and then machined to remove the surface reaction layer. The density of the comparative plate was measured to be 4.335 g / cc (95.9% of the theoretical density of TiB2).
[0107] Fig.10a An SEM micrograph of a non-inventive plate analyzed using OIM analysis is shown. As shown, the plate is composed of TiB2 particles (1040) that are larger on average than the inventive plate. Fig.10a As shown, the non-inventive plate has pores (1020), some of which are very large compared to the inventive plate. The average particle size was determined using OIM analysis and is shown in Fig.10b middle.
[0108] Fig.13a and Fig.13bThe particle orientation determined by OIM analysis of the main face and the second face orthogonal (perpendicular) to the main face for a non-inventive plate is shown respectively. In the comparative example, the main face is orthogonal to the hot pressing direction. The particles in the main face show a preferred orientation in the 0001-direction. The particles in the second face show a preferred orientation in the 2 Preferred orientation in the 0-direction.
[0109] Fig.14a and Fig.14b The inverse pole figures generated from the OIM analysis of the primary and secondary surfaces for the non-inventive panels are shown, respectively. Applying the ODF to the data set shows that the comparative sample has greater than 5 times the random ODF intensity along the 0001 direction, compared to <3 times the random ODF intensity of the exemplary embodiment sample, as shown in FIG. Fig.13a and Fig.13b The relative difference in ODF strength between these samples can be used to quantify the degree of orientation present in the samples; the comparative sample has 2.5 times the degree of orientation as the exemplary embodiment sample.
[0110] In addition to dry pressing, ceramic manufacturing techniques can be used to form green electrodes. Possible green electrode formation techniques include, but are not limited to, pressing TiB2 particles in an isostatic press, rolling TiB2 particles, extruding TiB2 powder, and casting TiB2 powder into a desired predetermined shape.
Claims
1. A method comprising: (a) forming a TiB2 feedstock into a predetermined shaped product, wherein the predetermined shaped product achieves a density of 40% to 70% of the theoretical density of pure TiB2; and (b) producing a final shaped product from the predetermined shaped product; wherein said producing comprises exposing said predetermined shaped product to an elevated temperature, wherein as a result of said exposure, said final shaped product realizes a plurality of pores and at least one of the following properties: (i) a density of 85% to 98% of the theoretical density of TiB2; (ii) an average particle size of not more than 15 μm; (iii) an interparticle porosity of 1% to 15% by volume; (iv) an average pore size no greater than 120% of the average particle size; and (v) Random particle orientation.
2. The method according to claim 1, wherein the TiB2 raw material comprises TiB2 particles, TiB2 granules and combinations thereof.
3. The method according to claim 1, wherein the forming step (a) comprises one or more of pressing, rolling, casting and extruding the TiB2 raw material to form the predetermined shaped product.
4. The method of claim 1, wherein the forming step (a) is performed at ambient temperature.
5. The method of any one of claims 2 to 4, wherein the forming step (a) comprises applying a pressure of at least 5000 psi, or at least 6000 psi, or at least 7000 psi, or at least 7500 psi.
6. The method according to any one of the preceding claims, wherein the predetermined shaped product achieves a density of at least 45%, or at least 50%, or at least 55%, or at least 58%, or at least 60% of the theoretical density of TiB2.
7. The method according to claim 6, wherein the predetermined shaped product realizes a density not greater than 68% of the theoretical density of TiB2.
8. The method of claim 1, wherein the generating step (b) comprises: heating the predetermined shaped product for a first time at a first temperature for a first period of time; The predetermined shaped product is heated a second time at a second temperature for a second period of time, wherein the second temperature is higher than the first temperature.
9. The method of claim 8, wherein the first temperature is at least 200°C, or at least 300°C, or at least 400°C, or at least 500°C.
10. The method of claim 8 or 9, wherein the first period of time is at least 1 minute, or at least 10 minutes, or at least 30 minutes, or at least 60 minutes.
11. The method according to any one of claims 8 to 10, wherein the first period of time is no greater than 48 hours.
12. The method according to any one of claims 8 to 11, wherein the first temperature is no greater than 1200°C.
13. The method of any one of claims 8 to 12, wherein the second temperature is at least 1600°C, or at least 1700°C, or at least 1800°C, or at least 1825°C.
14. The method of any one of claims 8 to 13, wherein the second period of time is at least 1 minute, or at least 10 minutes, or at least 30 minutes, or at least 1 hour, or at least 4 hours, or at least 8 hours, or at least 12 hours.
15. The method of any one of claims 8 to 14, wherein the second period of time is no greater than 96 hours.
16. The method of any one of claims 8 to 15, wherein the second temperature is no greater than 2300°C.
17. The method according to any one of claims 8 to 16, wherein the first heating comprises heating from an initial temperature to the first temperature at a first heating rate, wherein the first heating rate is no greater than 10°C / minute, or no greater than 8°C / minute, or no greater than 6°C / minute, or no greater than 5°C / minute. The method of claim 17 , wherein the initial temperature is ambient temperature.
19. The method of claim 17 or 18, wherein the second heating comprises heating from the first temperature to the second temperature at a second heating rate, wherein the second heating rate is no greater than 8°C / minute, or no greater than 7°C / minute, or no greater than 6°C / minute, or no greater than 5°C / minute.
20. The method of any one of the preceding claims, wherein the final shaped product achieves at least two of the properties (b)(i) to (b)(v).
21. The method of any one of the preceding claims, wherein the final shaped product achieves at least three of the properties (b)(i) to (b)(v).
22. The method of any one of the preceding claims, wherein the final shaped product achieves at least four of the properties (b)(i) to (b)(v).
23. A method according to any one of the preceding claims, wherein the final shaped product achieves all of the properties of (b)(i) to (b)(v).
24. The method of any one of the preceding claims, wherein the final shaped product achieves an average particle size of no greater than 12 microns, or no greater than 10 microns, or no greater than 8 microns, or no greater than 6 microns, or no greater than 4 microns.
25. The method of any one of the preceding claims, wherein the final shaped product achieves an inter-particle porosity of no greater than 14% by volume or an inter-particle porosity of no greater than 13% by volume.
26. A method according to any of the preceding claims, wherein the final formed product achieves an inter-particle porosity of at least 2 volume %, or an inter-particle porosity of at least 4 volume %, or an inter-particle porosity of at least 6 volume %, or an inter-particle porosity of at least 8 volume %.
27. A method according to any of the preceding claims, wherein the final molded product achieves an average pore size of no more than 110% of the average particle size, or an average pore size of no more than 100% of the average particle size, or an average pore size of no more than 90% of the average particle size, or an average pore size of no more than 80% of the average particle size, or an average pore size of no more than 70% of the average particle size, or an average pore size of no more than 60% of the average particle size, or an average pore size of no more than 50% of the average particle size.
28. The method of any one of the preceding claims, wherein the final shaped product achieves an ODF strength of no greater than 3 times random, or no greater than 2.75 times random, or no greater than 2.50 times random, or no greater than 2.25 times random, or no greater than 2.00 times random, or no greater than 1.75 times random, or no greater than 1.50 times random.
29. A method according to any one of the preceding claims, comprising: The TiB2 raw material is prepared for the forming step, wherein the preparing step includes spray drying a slurry to produce TiB2 particles prior to the forming step.
30. The method of claim 29, wherein the slurry comprises a liquid medium, wherein the TiB2 particles comprise at least one of the following due at least to a dispersant and a binder: (i) D not greater than 200 μm 90 ; (ii) D of at least 10 μm 10 ; (iii) 1.0 g / cm 3 Up to 1.8g / cm 3 The bulk density; (iv) a liquid medium content of not more than 0.5% by weight; and (v) A flow rate of at least 0.2 g / s.
31. The method of claim 29, wherein prior to said spray drying, TiB2 powder is combined with said liquid medium, wherein said slurry comprises said TiB2 powder, said dispersant, and said binder.
32. The method of claim 29, wherein the preparing step comprises: Deagglomerating the first TiB2 powder to produce a second TiB2 powder, wherein the second TiB2 powder achieves at least one of the following: (i) D from 0.5 μm to 4.0 μm 50 ; (ii) 1.0m 2 / g to 3.0m 2 Surface area / g; (iii) not more than 5.0 wt% O, or not more than 4 wt% O, or not more than 3 wt% O, or not more than 2.5 wt% O, or not more than 2.0 wt% O, or not more than 1.5 wt% O, or not more than 1 wt% O; (iv) not more than 5.0 wt% C, or not more than 4 wt% C, or not more than 3 wt% C, or not more than 2.5 wt% C, or not more than 2.0 wt% C, or not more than 1.5 wt% C, or not more than 1 wt% C; and (v) Irregular particle morphology.
33. The method of claim 32, wherein the second TiB2 powder is added to a liquid medium to form the slurry.
34. A method according to any one of the preceding claims, wherein the final shaped product is an electrode.
35. The method of claim 34, wherein the electrode is a cathode.
36. The method of claim 34, wherein the electrode is an anode.
37. An aluminium electrolysis cell comprising an electrode according to any one of claims 34 to 36.
38. An aluminium purification unit comprising an electrode according to any one of claims 34 to 36.
39. A method comprising: Use of the final shaped product according to any one of claims 1 to 33 as an electrode in an aluminium electrolysis cell to produce aluminium metal.
40. A method comprising: Use of the final shaped product according to any one of claims 1 to 33 as an electrode in an aluminium purification unit to produce aluminium metal.
41. An integrally formed titanium diboride (TiB2) product, comprising: (a) at least 50% by volume of TiB2; (b) At least one of the following properties: (i) a density of 85% to 98% of the theoretical density of TiB2; (ii) an average particle size of not more than 15 μm; (iii) an interparticle porosity of 1% to 15% by volume; (iv) an average pore size no greater than 120% of the average particle size; and (v) Random particle orientation.
42. The integrally formed titanium diboride (TiB2) product of claim 41, wherein the integrally formed titanium diboride (TiB2) product comprises at least two of (b)(i) to (v).
43. The integrally formed titanium diboride (TiB2) product of claim 41, wherein the integrally formed titanium diboride (TiB2) product comprises at least three of (b)(i) to (v).
44. The integrally formed titanium diboride (TiB2) product of claim 41, wherein the integrally formed titanium diboride (TiB2) product comprises at least four of (b)(i) to (v).
45. The integrally formed titanium diboride (TiB2) product of claim 41, wherein the integrally formed titanium diboride (TiB2) product comprises all of (b)(i) to (v).
46. An integrally formed titanium diboride (TiB2) product according to claim 41, wherein at least one of properties (b)(i) to (v) is preselected.
47. The integrally formed titanium diboride (TiB2) product of claim 41, wherein the integrally formed titanium diboride (TiB2) product is configured for use in an electrochemical cell.
48. An integrally formed titanium diboride (TiB2) product according to claim 47, wherein the electrochemical cell is an aluminum purification cell.
49. The integrally formed titanium diboride (TiB2) product of claim 47, wherein the electrochemical cell is an aluminum electrolysis cell.
50. The integrally formed titanium diboride (TiB2) product of claim 41, wherein the integrally formed titanium diboride (TiB2) product is an electrode.
51. An integrally formed titanium diboride (TiB2) product according to claim 50, wherein the electrode is a cathode.
52. The integrally formed titanium diboride (TiB2) product of claim 50, wherein the electrode is an anode.
53. The integrally formed titanium diboride (TiB2) product of claim 41, wherein the integrally formed titanium diboride (TiB2) product comprises at least a first face and a second face, wherein the second face is adjacent to or perpendicular to the first face.