Graphite carbon material for negative electrode of lithium ion secondary battery, negative electrode material for lithium ion secondary battery, negative electrode for lithium ion secondary battery, and lithium ion secondary battery

By optimizing the crystal crystal diameter and tap density of graphite carbon materials, the insufficient performance of lithium-ion secondary battery negative electrode materials in long-term reliability and high-temperature environments is solved, and excellent input characteristics, high-temperature storage characteristics and cycle characteristics are achieved. .

CN119032439APending Publication Date: 2024-11-26RESONAC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380034414.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The performance of existing lithium-ion secondary battery anode materials in long-term reliability and high temperature environments is insufficient, especially the input characteristics and cycle characteristics need to be further improved.

Method used

Graphite carbon materials with a microcrystal diameter Lc (002) of 35nm to 150nm and a tap density greater than or equal to 0.90g/cm3 were used, and the particle size distribution and specific surface area were optimized by laser diffraction scattering method and nitrogen adsorption measurement to form a A lithium-ion secondary battery negative electrode material with excellent input characteristics, high temperature storage characteristics and cycle characteristics.

Benefits of technology

The excellent input characteristics, high-temperature storage characteristics and cycle characteristics of the negative electrode material of lithium-ion secondary battery are realized, and the overall performance and reliability of the battery are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005086938930000191
    Figure BDA0005086938930000191
  • Figure BDA0005086938930000201
    Figure BDA0005086938930000201
Patent Text Reader

Abstract

The graphitic carbon material for negative electrodes of lithium ion secondary batteries has a crystallite diameter Lc (002) of 35-150 nm as determined by X-ray diffraction, and a tap density of 0.90 g / cm3 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a graphite carbon material for a negative electrode of a lithium ion secondary battery, a negative electrode material for a lithium ion secondary battery, a negative electrode for a lithium ion secondary battery, and a lithium ion secondary battery. Background Art

[0002] In recent years, with the rapid popularization of information-related devices such as personal computers, cameras, mobile phones, and communication equipment, the development of batteries used as their power sources has received attention. In addition, in the automotive industry, the development of high-output and high-capacity batteries for electric vehicles and hybrid vehicles is also being promoted. At present, among various batteries, lithium-ion secondary batteries have received attention from the perspective of high energy density.

[0003] For lithium ion secondary batteries mounted on electric vehicles and hybrid electric vehicles, rapid charging and long-term reliability are required. That is, it is desirable to take into account both high input and high life batteries. From the viewpoint of rapid charging, it is proposed to reduce the particles of negative electrode active materials to improve the solid internal diffusion of lithium ions. In addition, from the viewpoint of high life, a lithium ion secondary battery negative electrode active material with a small specific surface area is proposed.

[0004] As an example of such an idea, Patent Document 1 proposes a graphite carbon material for a negative electrode of a lithium ion secondary battery, which improves the solid diffusion of lithium ions by having a small particle size and reduces side reactions on the surface of the active material by setting the specific surface area in a small range.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2018-6270 Summary of the invention

[0008] Problems to be solved by the invention

[0009] In the above-mentioned Patent Document 1, although the initial charge and discharge efficiency is excellent, further improvement in long-term reliability is required.

[0010] Therefore, an object of one embodiment of the present disclosure is to provide a graphite carbon material for a lithium ion secondary battery negative electrode, a lithium ion secondary battery negative electrode material, a lithium ion secondary battery negative electrode, and a lithium ion secondary battery that can achieve excellent input characteristics, high temperature storage characteristics, and cycle characteristics.

[0011] Methods for solving problems

[0012] Specific means for solving the above-mentioned problems include the following aspects.

[0013] <1> A graphite carbon material for a negative electrode of a lithium-ion secondary battery, wherein the crystallite diameter Lc(002) obtained by X-ray diffraction is 35nm to 150nm, and the tap density is greater than or equal to 0.90g / cm 3 .

[0014] <2> like <1> The graphite carbon material for lithium ion secondary battery negative electrode has a particle size distribution measured by laser diffraction scattering method, and when a volume cumulative distribution curve is drawn from the small diameter side, the particle size (D50) at the cumulative 50% is 5 μm to 30 μm.

[0015] <3> like <1> or <2> The graphite carbon material for the negative electrode of the lithium-ion secondary battery has a wavelength of 1330 cm-1 in laser Raman spectrophotometry. -1 The intensity of the maximum peak near 1580 cm -1 The intensity ratio (Id / Ig) of the intensity Ig of the nearby maximum peak is 0.1 to 0.5.

[0016] <4> like <1> ~ <3> The graphite carbon material for a negative electrode of a lithium ion secondary battery according to any one of the preceding claims has a specific surface area of ​​0.7 m 2 / g~8m 2 / g.

[0017] <5> like <1> ~ <4> The graphite carbon material for a negative electrode of a lithium ion secondary battery described in any one of the above aspects has a crystallite diameter La(110) of 50 nm to 450 nm as determined by X-ray diffraction.

[0018] <6> like <1> ~ <5> The graphite carbon material for a negative electrode of a lithium ion secondary battery as described above has an oil absorption of 30 mL to 75 mL per 100 g of the graphite material in a linseed oil absorption measurement.

[0019] <7> A negative electrode material for a lithium ion secondary battery, comprising <1> ~ <6> The graphite carbon material for lithium ion secondary battery described in any one of the preceding claims.

[0020] <8> A negative electrode for a lithium ion secondary battery, comprising a graphite carbon material layer and a current collector, wherein the graphite carbon material layer comprises <1> ~ <6> The graphite carbon material for lithium ion secondary battery described in any one of the preceding claims.

[0021] <9> A lithium ion secondary battery comprising <8> The lithium-ion secondary battery comprises a negative electrode, a positive electrode and an electrolyte.

[0022] Effects of the Invention

[0023] In one embodiment of the present disclosure, a graphite carbon material for a lithium ion secondary battery negative electrode, a lithium ion secondary battery negative electrode material, a lithium ion secondary battery negative electrode, and a lithium ion secondary battery can be provided, which can achieve excellent input characteristics, high temperature storage characteristics, and cycle characteristics. DETAILED DESCRIPTION

[0024] Hereinafter, the mode for implementing the present invention is described in detail. However, the present invention is not limited to the following embodiments. In the following embodiments, except for the cases specifically indicated, its constituent elements (including element steps, etc.) are not necessary. Numerical values ​​and their ranges are also the same, and do not limit the present invention.

[0025] In the present disclosure, in a numerical range expressed using "to", the numerical values ​​described before and after "to" are included as the minimum value and the maximum value, respectively.

[0026] In the numerical range recorded in stages in the present disclosure, the upper limit or lower limit recorded in one numerical range can also be replaced by the upper limit or lower limit of the numerical range recorded in other stages. In addition, in the numerical range recorded in the present disclosure, the upper limit or lower limit of the numerical range can also be replaced by the value shown in each test.

[0027] In the present disclosure, a plurality of substances equivalent to each component may be included in the graphite carbon material for the negative electrode of a lithium ion secondary battery and the composition. Hereinafter, "graphite carbon material for the negative electrode of a lithium ion secondary battery" is sometimes referred to as "graphite carbon material". In the case where there are a plurality of substances equivalent to each component in the graphite carbon material and the composition, unless otherwise specified, the content and content of each component refer to the total content and content of the plurality of substances present in the graphite carbon material and the composition.

[0028] In the present disclosure, the particles corresponding to each component in the graphite carbon material and the composition may include multiple types. In the case where multiple types of particles corresponding to each component are present in the graphite carbon material and the composition, unless otherwise specified, the particle size of each component refers to the value for the mixture of the multiple types of particles present in the graphite carbon material and the composition.

[0029] In the present disclosure, the term "layer" includes not only the case where a layer is formed in the entire region when a region where the layer exists is observed, but also the case where the layer is formed in only a part of the region.

[0030] In the present disclosure, the term “stacked” means stacking layers, and two or more layers may be connected or two or more layers may be detachable.

[0031] In the present disclosure, the crystallite diameters Lc(002) and La(110) determined by X-ray diffraction are determined by the following method using an X-ray diffractometer (XRD).

[0032] The sample was prepared by mixing graphite powder: Si powder in a mass ratio of 5:1 in an agate mortar for 5 minutes, and the X-ray diffraction peak spectrum was determined under the following measurement conditions. It should be noted that the diffraction peak position uses standard silicon powder (e.g., NIST Si 640f) as an internal standard. As an X-ray diffraction apparatus (XRD), for example, SmartLab 3kW manufactured by Rigaku Co., Ltd. can be used. The measurement conditions and calculation methods are based on JIS R7651:2007 (method for measuring lattice constants and crystallite sizes of carbon materials).

[0033] In the present disclosure, the particle size (D50) is a particle size at which the accumulation is 50% when a volume cumulative distribution curve is drawn from the smaller diameter side in a particle size distribution measured by a laser diffraction particle size distribution analyzer.

[0034] As a laser diffraction type particle size distribution measuring apparatus, SALD-3000J manufactured by Shimadzu Corporation is mentioned, for example.

[0035] In the present disclosure, the tap density is measured in accordance with JIS R1628: 1997. The tap density can be measured using a packing density measuring device (e.g., KRS-406, manufactured by Kuramochi Scientific Instruments Co., Ltd.). 100 mL of graphite carbon material for lithium ion secondary battery is added to a measuring cylinder, and the density is calculated by tapping (dropping the measuring cylinder from a predetermined height) until the density reaches saturation.

[0036] In the present disclosure, in laser Raman spectrophotometry, 1330 cm -1 The intensity of the maximum peak near 1580 cm -1 The intensity ratio of the intensity Ig of the maximum peak in the vicinity (Id / Ig, hereinafter also referred to as “R value”) was determined by the following method using a laser Raman spectrophotometer.

[0037] The measurement sample is placed flat on a sample plate and irradiated with argon laser light, and the measurement is performed using a laser Raman spectrophotometer. As the laser Raman spectrophotometer, for example, NRS-1000 manufactured by JASCO Corporation can be used. The measurement conditions are as follows.

[0038] Wavelength of argon laser: 532nm

[0039] Wave number resolution: 2.56cm -1

[0040] Measuring range: 1180cm -1~1730cm -1

[0041] Peak Finding: Background Removal

[0042] The specific surface area obtained by nitrogen adsorption measurement at 77 K (hereinafter, sometimes simply referred to as "specific surface area") is obtained by using the BET method based on JIS Z8830: 2013 from the adsorption isotherm obtained by nitrogen adsorption measurement at 77 K. The specific surface area is calculated by using a high-speed specific surface area / pore distribution measuring device (e.g., FlowSorb III manufactured by Shimadzu Corporation) to measure nitrogen adsorption at liquid nitrogen temperature (77 K) by a single-point method, and applying the BET method.

[0043] When measuring the BET specific surface area, it is considered that moisture adsorbed on the surface and structure of the sample affects the gas adsorption capacity, so it is preferred to first perform a pretreatment for removing moisture by heating.

[0044] In the pretreatment, the sample cell for measurement into which 0.05 g of the measurement sample was put was depressurized to 10 Pa or less by a vacuum pump, and then heated at 110°C and kept for 3 hours or more, and then naturally cooled to room temperature (25°C) while maintaining the decompression. After the pretreatment, the evaluation temperature was set to 77K, and the evaluation pressure range was measured in a manner that the relative pressure (equilibrium pressure relative to the saturated vapor pressure) was less than 1.

[0045] In the present disclosure, in the measurement of linseed oil absorption, the oil absorption per 100 g of graphite material (hereinafter also referred to as "linseed oil absorption") is measured according to the method described in JIS K6217-4:2008 "Carbon black for rubber - Basic properties - Part 4: Method for determining oil absorption", wherein the measurement is performed by using linseed oil (manufactured by Kanto Chemical Co., Ltd.) instead of dibutyl phthalate (DBP) as the reagent liquid.

[0046] The specific method for measuring the oil absorption of linseed oil is as follows. Linseed oil is titrated to the measurement sample using a constant-rate burette, and the change in viscosity characteristics is measured using a torque detector. The amount of reagent liquid added per 100 g of the measurement sample corresponding to a torque of 70% of the maximum torque generated is taken as the oil absorption of linseed oil (mL). As a measuring instrument, for example, an absorption measuring device manufactured by Asahi Soken Co., Ltd. can be cited.

[0047] <Graphite carbon material for lithium ion secondary battery negative electrode>

[0048] The graphite carbon material for lithium ion secondary battery negative electrode disclosed in the present invention has a crystallite diameter Lc(002) of 35 nm to 150 nm as determined by X-ray diffraction, and a tap density of greater than or equal to 0.90 g / cm 3 .

[0049] The graphite carbon material for a negative electrode of a lithium ion secondary battery having the above-described structure has excellent input characteristics, high temperature storage characteristics, and cycle characteristics. The reason for this is not clear, but is presumed as follows.

[0050] By setting the crystallite diameter Lc(002) to a range of 35 nm to 150 nm, the input characteristics and cycle characteristics are excellent. Furthermore, by setting the tap density to be greater than or equal to 0.90 g / cm 3 , which can inhibit the absorption of the binder by the graphite carbon material, thereby improving the adhesion of the active material layer containing the graphite carbon material and the binder, resulting in further improvement of the high-temperature storage characteristics and cycle characteristics.

[0051] It should be noted that if one attempts to obtain a graphite carbon material having a small particle size as in Patent Document 1, the graphite carbon material is pulverized vigorously, which tends to reduce the yield and productivity.

[0052] The crystallite diameter Lc(002) is preferably greater than or equal to 40 nm, more preferably greater than or equal to 45 nm, and further preferably greater than or equal to 60 nm. The crystallite diameter Lc(002) is preferably less than or equal to 140 nm, more preferably less than or equal to 130 nm, and further preferably less than or equal to 120 nm.

[0053] Tap density greater than or equal to 0.90g / cm 3 , preferably greater than or equal to 0.91 g / cm 3 , more preferably greater than or equal to 0.92 g / cm 3 In addition, the tap density can be less than or equal to 1.30 g / cm 3 , or less than or equal to 1.25 g / cm 3 .

[0054] The particle size (D50) is preferably 5 μm to 30 μm. When the particle size (D50) is less than or equal to 30 μm, the diffusion distance of lithium from the surface to the inside of the graphite carbon material can be inhibited from becoming longer, and there is a tendency to further improve the input characteristics of the lithium ion secondary battery. The particle size (D50) is preferably less than or equal to 25 μm, more preferably less than or equal to 20 μm, and further preferably less than or equal to 17 μm.

[0055] When the particle size (D50) is greater than or equal to 5 μm, the pressing pressure required for forming the active material layer can be reduced, and as a result, there is a tendency for the input characteristics to be more excellent. The particle size (D50) is preferably greater than or equal to 5.5 μm, more preferably greater than or equal to 6.0 μm, and further preferably greater than or equal to 6.2 μm.

[0056] The R value is preferably 0.10 to 0.50. When the R value is 0.10 or more, graphite lattice defects are sufficient for the absorption and release of lithium ions, and there is a tendency to suppress the reduction of input characteristics. The R value is more preferably 0.15 or more, and further preferably 0.20 or more.

[0057] When the R value is 0.50 or less, the capacity tends to be excellent. The R value is preferably 0.40 or less, more preferably 0.35 or less, and further preferably 0.30 or less.

[0058] The specific surface area is preferably 0.7 m 2 / g~8m 2 When the specific surface area is within the above range, a good balance between input characteristics and life characteristics tends to be obtained.

[0059] The specific surface area is more preferably greater than or equal to 0.8 m 2 / g, more preferably greater than or equal to 0.9m 2 / g, particularly preferably greater than or equal to 1.0m 2 / g. In addition, the specific surface area is more preferably less than or equal to 4.0m 2 / g, more preferably less than or equal to 3.5m 2 / g, particularly preferably less than or equal to 2.5m 2 / g.

[0060] The crystallite diameter La(110) is preferably 50 nm to 450 nm. When the crystallite diameter La(110) is 50 nm or more, the capacity tends to be excellent. When the crystallite diameter La(110) is 450 nm or less, the input tends to be excellent.

[0061] The crystallite diameter La(110) is more preferably equal to or greater than 100 nm, and further preferably equal to or greater than 150 nm. La(110) is more preferably equal to or less than 440 nm, and further preferably equal to or less than 400 nm.

[0062] The linseed oil absorption is preferably 30 mL / 100 g to 75 mL / 100 g. When the linseed oil absorption is within the above range, it is easy to prepare a slurry for forming an active material layer, and workability tends to be excellent.

[0063] The linseed oil absorption is more preferably 70 mL / 100 g or less, and further preferably 65 mL / 100 g or less. The linseed oil absorption is more preferably 40 mL / 100 g or more.

[0064] The average interplanar spacing d obtained by X-ray diffraction 002The average interplanar spacing d is preferably 0.334 nm to 0.338 nm. 002 When the particle size is 0.338 nm or less, the initial charge and discharge efficiency and energy density of the lithium ion secondary battery tend to be excellent.

[0065] In the present disclosure, the average surface spacing d 002 It is calculated using the Bragg formula based on the diffraction peak corresponding to the carbon 002 plane appearing near the diffraction angle 2θ=24°~27°, based on the diffraction pattern obtained by irradiating the sample with X-rays (CuKα rays) and measuring the diffraction lines with a goniometer.

[0066] Specifically, a measurement sample is filled in a concave portion of a quartz sample holder and placed on a measurement table, and measurement is performed under the following measurement conditions using a wide-angle X-ray diffraction apparatus (eg, manufactured by Rigaku Corporation).

[0067] Radiation source: CuKα ray average surface spacing (wavelength = 0.15418nm)

[0068] Output: 40kV, 20mA

[0069] Sampling width: 0.010°

[0070] Scanning range: 10°~35°

[0071] Scanning speed: 0.5° / min

[0072] As graphite carbon material, graphite such as artificial graphite, natural graphite, graphitized mesophase carbon, graphitized carbon fiber can be cited. The shape of graphite is not particularly limited, and flaky, spherical, massive, fibrous, etc. can be cited. From the viewpoint of obtaining a high tap density, spherical is preferred.

[0073] Artificial graphite can be obtained by sintering a graphitizable aggregate. One type of the graphitizable aggregate can be used alone, or two or more types can be used in combination. In addition, graphite can also be used together with the graphitizable aggregate. One type of graphite can be used alone, or two or more types can be used in combination.

[0074] As the graphitizable aggregate, for example, coke powder, carbide of resin, etc. can be used, and there is no particular limitation as long as it is a graphitizable powder material. Among them, coke powder that is easily graphitized is preferred, and examples thereof include mosaic coke, needle coke, etc. From the viewpoint of easily adjusting the crystallite diameter Lc (002) to the range of 35nm to 150nm, mosaic coke is more preferred.

[0075] A binder (organic binder) may be used together with the graphitizable aggregate. The binder may be used alone or in combination of two or more.

[0076] The binder (organic binder) is not particularly limited as long as it can be graphitized by firing, and examples of the binder include organic materials such as tar, pitch, starch, thermosetting resins, and thermoplastic resins.

[0077] Other materials may be used together with the graphitizable aggregate. Examples of other materials include fluidity imparting agents and graphitization catalysts. Other materials may be used alone or in combination of two or more.

[0078] The type of fluidity imparting agent is not particularly limited. As the fluidity imparting agent, specifically, hydrocarbons such as liquid paraffin, paraffin, polyethylene wax, fatty acids such as stearic acid, oleic acid, erucic acid, 12-hydroxystearic acid, fatty acid metal salts such as zinc stearate, lead stearate, aluminum stearate, calcium stearate, magnesium stearate, stearic acid amide, oleamide, erucic acid amide, methylene bis stearic acid amide, fatty acid amides such as ethylene bis stearic acid amide, stearic acid monoglyceride, stearyl stearate, fatty acid esters such as hardened oil, higher alcohols such as stearyl alcohol, etc. can be cited. Among them, preferred fatty acids, more preferably stearic acid.

[0079] The type of graphitization catalyst is not particularly limited. Specific examples of the graphitization catalyst include substances having a graphitization catalytic effect such as silicon, iron, nickel, titanium, and boron, and carbides, oxides, and nitrides of these substances.

[0080] As the shape of artificial graphite, there is no particular limitation, and it can be primary particles or agglomerated particles. In the case of agglomerated particles, carbon materials from a binder may be included or not included. In addition, it can also be graphite particles (hereinafter referred to as "blocky graphite particles") in which a plurality of flat particles are assembled or combined in a manner in which the orientation planes (main faces) are not parallel. In blocky graphite particles, the non-parallel main faces of a plurality of flat particles refer to that the face (main face) with the largest cross-sectional area of ​​the flat graphite particles is not aligned in a certain direction. Regarding blocky graphite particles, reference may also be made to Japanese Patent Gazette No. 3285520, Japanese Patent Gazette No. 3325021, etc.

[0081] The shape of artificial graphite can be confirmed by observation using a scanning electron microscope (SEM).

[0082] Before the firing for graphitization, the mixture containing the graphitizable aggregate, the binder, and other components such as graphite may be formed into a predetermined shape, or may be directly fired into a powder shape without being formed. 3 From the viewpoint of the present invention, it is preferred to perform pulverization after molding and before graphitization, and perform graphitization after adjusting the particle size using a sieve or the like.

[0083] The method for forming into a predetermined shape is not particularly limited. For example, a molding method in which a mixture is placed in a container such as a mold and pressurized in a uniaxial direction, a vibration molding method in which a mixture is placed in a container such as a mold and a weight is placed on the upper surface to apply vibration and impact to the mold frame to form, and an extrusion molding method in which the mixture is pressed laterally and extruded from a nozzle using a press to form the mixture, etc. are cited. From the viewpoint of improving the production efficiency of the molded product, extrusion molding is preferred.

[0084] The proportion of each material in the mixture is not particularly limited. For example, the content of the binder can be 0.5 to 20 parts by mass, 1 to 18 parts by mass, or 1.2 to 15 parts by mass relative to 100 parts by mass of the graphitizable aggregate and graphite. The binder may not be used.

[0085] For example, the content of the binder during graphitization after molding may be 1.0 to 20 parts by mass, 1.5 to 18 parts by mass, or 2.0 to 15 parts by mass based on 100 parts by mass of the graphitizable aggregate and graphite.

[0086] In addition, from the viewpoint of suppressing the specific surface area of ​​the obtained graphite carbon material to a low level, the content of the binder can be 1.0 to 14 parts by mass, 1.2 to 12 parts by mass, or 1.5 to 10 parts by mass relative to 100 parts by mass of the graphitizable aggregate and graphite.

[0087] The mixture preferably contains a fluidity-imparting agent from the viewpoint of easy molding. In particular, when the mixture is molded by extrusion molding, it is preferable to contain a fluidity-imparting agent in order to mold the mixture while making it flow.

[0088] When the mixture contains a fluidity-imparting agent, the amount thereof is not particularly limited. For example, the content of the fluidity-imparting agent relative to the entire mixture may be 0.1% to 20% by mass, 0.5% to 10% by mass, or 0.5% to 5% by mass. The mixture may also contain no fluidity-imparting agent.

[0089] When the mixture contains a graphitization catalyst, its amount is not particularly limited. For example, the content of the graphitization catalyst relative to the entire mixture may be 0.1% to 50% by mass, 0.5% to 40% by mass, or 0.5% to 30% by mass. The mixture may also contain no graphitization catalyst.

[0090] The calcination is preferably carried out under conditions where the mixture is difficult to oxidize, for example, a method of calcining in a nitrogen atmosphere, an argon atmosphere or a vacuum. The graphitization temperature is preferably greater than or equal to 2000°C, more preferably greater than or equal to 2500°C, and further preferably 2800°C to 3200°C.

[0091] When the graphitization temperature is 2000° C. or higher, the growth of graphite crystals becomes good, and the discharge capacity tends to be improved. When the graphitization temperature is 3200° C. or lower, the crystallite diameter Lc(002) tends to be easily adjusted to the range of 35 nm to 150 nm.

[0092] The obtained graphite carbon material is preferably pulverized into a desired volume average particle size. The method for pulverizing the graphite is not particularly limited, and a known method such as a jet mill, a vibration mill, a pin mill, a hammer mill, etc. can be applied.

[0093] At least a portion of the surface of the obtained graphite carbon material may be coated with amorphous carbon. The amorphous carbon is preferably selected from at least one of the group consisting of a carbonaceous substance and carbonaceous particles obtained by heat treatment of an organic compound that can be converted into a carbonaceous substance (hereinafter also referred to as a precursor of amorphous carbon).

[0094] The precursor of amorphous carbon is not particularly limited, and examples thereof include asphalt, organic polymer compounds, etc. Examples of asphalt include, for example, ethylene heavy end fraction asphalt, crude oil asphalt, coal tar asphalt, asphalt decomposition asphalt, asphalt produced by thermal decomposition of polyvinyl chloride, etc., and asphalt produced by polymerizing naphthalene, etc. in the presence of a super acid. Examples of organic polymer compounds include thermoplastic resins such as polyvinyl chloride, polyvinyl alcohol, polyvinyl acetate, polyvinyl butyral, and natural substances such as starch and cellulose.

[0095] The carbonaceous particles used as the amorphous carbon are not particularly limited, and examples thereof include particles of acetylene black, oil furnace black, Ketjen black, channel black, thermal black, and soil graphite.

[0096] The method of coating with amorphous carbon includes, for example, a method of heat treating a mixture containing a graphite carbon material and a precursor of amorphous carbon. From the perspective of improving the input characteristics of the lithium ion secondary battery, the temperature when the mixture is heat treated is preferably 800°C to 1500°C, more preferably 900°C to 1300°C, and further preferably 1050°C to 1250°C. The temperature when the mixture is heat treated can be constant from the beginning to the end of the heat treatment, or it can vary.

[0097] <Negative electrode materials for lithium-ion secondary batteries>

[0098] The negative electrode material for lithium ion secondary battery of the present disclosure (hereinafter sometimes simply referred to as "negative electrode material") includes the graphite carbon material for lithium ion secondary battery of the present disclosure. The graphite carbon material of the present disclosure can be suitably used as a negative electrode active material of lithium ion secondary battery.

[0099] As the negative electrode active material, the graphite carbon material of the present disclosure may be used alone or in combination with other negative electrode active materials. As other negative electrode active materials, there are no particular restrictions, and for example, artificial graphite, amorphous carbon, carbon black, fibrous carbon and nanocarbon that do not belong to the graphite carbon material of the present disclosure may be cited. Other carbon materials may be used alone or in combination with two or more.

[0100] The negative electrode active material may also contain particles containing an element capable of absorbing and releasing lithium ions other than the carbon material. The element capable of absorbing and releasing lithium ions is not particularly limited, and examples thereof include Si, Sn, Ge, and In.

[0101] The content of the graphite carbon material of the present disclosure in the negative electrode active material is not particularly limited, but is, for example, preferably 50% by mass or more, more preferably 80% by mass or more, further preferably 90% by mass or more, and particularly preferably 100% by mass.

[0102] <Negative electrode for lithium ion secondary battery>

[0103] The negative electrode for lithium ion secondary battery of the present disclosure comprises a graphite carbon material layer containing the graphite carbon material for lithium ion secondary battery of the present disclosure and a current collector. The negative electrode for lithium ion secondary battery may comprise other components as required in addition to the graphite carbon material layer containing the graphite carbon material of the present disclosure and the current collector.

[0104] The negative electrode for lithium ion secondary battery can be prepared by, for example, mixing a graphite carbon material and a binder with a solvent to prepare a slurry of a graphite carbon material composition, applying it on a current collector to form a graphite carbon material layer, or by forming the graphite carbon material composition into a sheet, a granular shape, etc., and integrating it with the current collector. Mixing can be carried out using a dispersing device such as a stirrer, a ball mill, a super sand mill, and a pressurized kneading machine.

[0105] The binder for preparing the graphite carbon material composition is not particularly limited. As a binder, styrene-butadiene copolymer, methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, acrylonitrile, methacrylonitrile, hydroxyethyl acrylate, hydroxyethyl methacrylate and other olefinic unsaturated carboxylic acid esters polymers, acrylic acid, methacrylic acid, itaconic acid, fumaric acid, maleic acid and other olefinic unsaturated carboxylic acid polymers, polyvinylidene fluoride, polyethylene oxide, polyepichlorohydrin, polyphosphazene, polyacrylonitrile and other ionic conductivity large polymer compounds etc. can be cited. When the graphite carbon material composition includes a binder, its amount is not particularly limited. The content of the binder can be, for example, 0.5 mass parts to 20 mass parts relative to a total of 100 mass parts of the graphite carbon material and the binder.

[0106] The solvent is not particularly limited as long as it is a solvent that can dissolve or disperse the binder. Specifically, organic solvents such as N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, γ-butyrolactone, water, etc. can be cited. The amount of solvent used is not particularly limited as long as it can make the graphite carbon material composition into a desired state such as a paste. The amount of solvent used is preferably greater than or equal to 60 parts by mass and less than 150 parts by mass relative to 100 parts by mass of the graphite carbon material.

[0107] The graphite carbon material composition may include a thickener. As the thickener, carboxymethyl cellulose or its salt, methyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, ethyl cellulose, polyvinyl alcohol, polyacrylic acid or its salt, alginic acid or its salt, oxidized starch, phosphorylated starch, casein, etc. can be cited. When the graphite carbon material composition includes a thickener, its amount is not particularly limited. The content of the thickener can be, for example, 0.1 to 5 parts by mass relative to 100 parts by mass of the graphite carbon material.

[0108] The graphite carbon material composition may include a conductive auxiliary material. As a conductive auxiliary material, carbon materials such as artificial graphite, carbon black (acetylene black, thermal black, furnace black, etc.), oxides showing conductivity, nitrides showing conductivity, etc. can be cited. When the graphite carbon material composition includes a conductive auxiliary material, its amount is not particularly limited. The content of the conductive auxiliary material can be, for example, 0.5 to 15 parts by mass relative to 100 parts by mass of the graphite carbon material.

[0109] The material of the current collector is not particularly limited, and can be selected from aluminum, copper, nickel, titanium, stainless steel, etc. The state of the current collector is not particularly limited, and can be selected from foil, perforated foil, net, etc. In addition, porous materials such as porous metal (foamed metal), carbon paper, etc. can also be used as the current collector.

[0110] When the graphite carbon material composition is applied to the collector to form a graphite carbon material layer, the method is not particularly limited, and known methods such as metal mask printing, electrostatic coating, dip coating, spraying, roller coating, scraper, notch wheel coating, gravure coating, screen printing can be used. After the graphite carbon material composition is applied to the collector, the solvent contained in the graphite carbon material composition is removed by drying. Drying can be carried out using, for example, a hot air dryer, an infrared dryer or a combination of these devices. Rolling treatment can also be performed as needed. Rolling treatment can be performed by methods such as a flat press and a calendering roller.

[0111] When the graphite carbon material composition formed into a sheet, particle or the like is integrated with the current collector to form a graphite carbon material layer, the method of integration is not particularly limited. For example, it can be performed by a roller, a flat plate press or a combination of these methods. The pressure during integration is preferably 1 MPa to 200 MPa, for example.

[0112] <Lithium-ion secondary battery>

[0113] The lithium ion secondary battery of the present disclosure includes the negative electrode for the lithium ion secondary battery of the present disclosure (hereinafter also simply referred to as “negative electrode”), a positive electrode, and an electrolyte solution.

[0114] The positive electrode can be obtained by forming a positive electrode material layer on a current collector in the same manner as the above-mentioned negative electrode production method. As the current collector, a current collector made of a metal or alloy such as aluminum, titanium, stainless steel, etc. in a foil, perforated foil, mesh, etc. can be used.

[0115] There is no particular limitation on the positive electrode material used to form the positive electrode material layer. For example, metal compounds (metal oxides, metal sulfides, etc.) and conductive polymer materials that can be doped or embedded with lithium ions can be cited. More specifically, lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2), and their complex oxides (LiCo x Ni y Mn z O2, x+y+z=1), a complex oxide containing an additional element M' (LiCo a Ni b Mn c M' d O2, a+b+c+d=1, M': Al, Mg, Ti, Zr or Ge), spinel lithium manganese oxide (LiMn2O4), lithium vanadium compounds, V2O5, V6O 13, VO2, MnO2, TiO2, MoV2O8, TiS2, V2S5, VS2, MoS2, MoS3, Cr3O8, Cr2O5, olivine-type LiMPO4 (M: Co, Ni, Mn, Fe) and other lithium-containing compounds, polyacetylene, polyaniline, polypyrrole, polythiophene, polyacene and other conductive polymers, porous carbon, etc. The positive electrode material can be a single type or two or more types.

[0116] The electrolyte solution is not particularly limited, and for example, an electrolyte solution (so-called organic electrolyte solution) obtained by dissolving a lithium salt as an electrolyte in a non-aqueous solvent can be used.

[0117] Examples of the lithium salt include LiClO4, LiPF6, LiAsF6, LiBF4, LiSO3CF3, etc. The lithium salt may be used alone or in combination of two or more.

[0118] Examples of the non-aqueous solvent include ethylene carbonate, fluoroethylene carbonate, chloroethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, cyclopentanone, cyclohexylbenzene, sulfolane, propane sultone, 3-methylsulfolane, 2,4-dimethylsulfolane, 3-methyl-1,3-oxazolidin-2-one, γ-butyrolactone, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, methyl butyl carbonate, ethyl propyl carbonate, ethyl butyl carbonate, dipropyl carbonate, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, methyl acetate, ethyl acetate, trimethyl phosphate, triethyl phosphate, etc. The non-aqueous solvent may be one kind alone or two or more kinds.

[0119] The state of the positive electrode and the negative electrode in the lithium ion secondary battery is not particularly limited. For example, the positive electrode and the negative electrode and a separator disposed between the positive electrode and the negative electrode as required may be wound in a spiral or may be stacked in a flat plate shape.

[0120] The separator is not particularly limited, for example, a nonwoven fabric, a cloth, a microporous membrane or a combination thereof made of a resin can be used. As the resin, a resin having a polyolefin such as polyethylene or polypropylene as a main component can be cited. In the structure of a lithium ion secondary battery, when the positive electrode is not in direct contact with the negative electrode, a separator may not be used.

[0121] The shape of the lithium ion secondary battery is not particularly limited, and examples thereof include laminated batteries, paper batteries, button batteries, coin batteries, stacked batteries, cylindrical batteries, and square batteries.

[0122] The lithium ion secondary battery disclosed in the present invention is suitable as a large-capacity lithium ion secondary battery used in electric vehicles, power tools, power storage devices, etc. due to its excellent output characteristics. It is particularly suitable as a lithium ion secondary battery used in electric vehicles (EV), hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV), etc., which require high current charging and discharging in order to improve acceleration performance and braking regeneration performance.

[0123] Example

[0124] Hereinafter, the present disclosure will be specifically described by the following examples, but the present disclosure is not limited to these examples.

[0125] The particle size (D50) was measured by the following method. The crystallite diameter Lc (002), crystallite diameter La (110), R value, specific surface area, linseed oil absorption and tap density were measured by the above methods.

[0126] [Measurement of particle size]

[0127] A graphite carbon material sample was dispersed in purified water together with 0.2 mass % of a surfactant (trade name: LIPONOL T / 15, manufactured by LION Corporation), and the resulting solution was placed in a sample water tank of a laser diffraction particle size distribution measuring apparatus (SALD-3000J, manufactured by Shimadzu Corporation). Next, the solution was circulated with a pump (the pump flow rate was from the maximum value to 65%) while applying ultrasonic waves to the solution, and the amount of water was adjusted so that the absorbance was 0.10 to 0.15, and the volume-based particle size distribution was measured.

[0128] In the volume cumulative distribution (%), the particle size D50 (μm) (average particle size) at which 50% of the particles are smaller in terms of particle size is determined.

[0129] [Example 1]

[0130] (Manufacturing of graphite carbon materials)

[0131] The semi-needle coke (coke A) was coarsely pulverized and further finely pulverized with a jet mill to a particle size (D50) of 16 μm. It was heat treated at a maximum temperature of 1000°C in a nitrogen atmosphere for 1 hour and then sintered at 3000°C for 1 hour to graphitize the graphitizable components. The obtained graphite carbon material was pulverized with a shredder and then granulated to obtain graphite carbon material A. The particle size (D50) of graphite carbon material A was 15 μm.

[0132] The physical properties of the produced graphite carbon material were measured.

[0133] (Production of negative electrode)

[0134] With respect to 97 parts by mass of graphite carbon material A, an aqueous solution of CMC (carboxymethyl cellulose, manufactured by Daicel Fine Chem Co., Ltd., product number 2200) as a thickener (CMC concentration: 1.5% by mass) was added so that the solid content of CMC became 1.5 parts by mass, and kneading was performed for 10 minutes. Next, purified water was added so that the total solid content concentration of the negative electrode material and CMC became 40% to 50% by mass, and kneading was performed for 10 minutes. Next, an aqueous dispersion of SBR (BM400-B, Japan Zeon Co., Ltd.) as a styrene butadiene copolymer rubber (SBR concentration: 40% by mass) was added as a binder so that the solid content of SBR was 1.5 parts by mass, and mixing was performed for 10 minutes to prepare a paste-like negative electrode material composition. Next, the negative electrode material composition was applied onto an electrolytic copper foil having a thickness of 11 μm using a notched wheel coater with an adjusted gap so that the coating amount per unit area was 10.0 mg / cm 2 Then, the electrode density was adjusted to 1.6 g / cm by using a roller press. 3 .

[0135] (Coin-type battery production)

[0136] The electrolytic copper foil with the negative electrode material layer formed thereon was punched into a disc shape with a diameter of 14 mm to prepare a sample electrode (negative electrode) for a coin-type battery. The sample electrode (negative electrode), separator, and counter electrode (metallic lithium) were placed in a coin-type battery container in the order prepared, and an electrolyte was injected to prepare a coin-type lithium-ion secondary battery. As the electrolyte, a mixed solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) (the volume ratio of EC to EMC is 3:7) was used, and 0.5% by mass of vinylene carbonate (VC) was added relative to the total amount of the mixed solution to dissolve LiPF6 in a manner to obtain a concentration of 1 mol / L. As a separator, a polyethylene microporous membrane with a thickness of 20 μm was used. Using the prepared lithium-ion secondary battery, the initial charge and discharge characteristics were evaluated by the following method.

[0137] The coin-type battery was produced in a glove box at an open air temperature of -70°C and an Ar atmosphere with an oxygen concentration of less than 10 ppm.

[0138] (Determination of discharge specific capacity)

[0139] The coin-shaped battery was left standing in a thermostatic chamber at 25°C for 3 hours and then charged with a constant current (CC charge) at a current value equivalent to 0.2C to 0V (Li / Li +), and then constant voltage charging (CV charging) was performed to a current value equivalent to 0.02C. After resting for 15 minutes, CC discharge was performed to 1.5V at a current value equivalent to 0.2C. The value obtained by dividing the amount of electricity at this time by the mass of the active material of the electrode (the mass of the graphite material alone) was calculated as the discharge specific capacity.

[0140] Discharge specific capacity (mAh / g) = discharge capacity (mAh) ÷ active material mass (g)

[0141] (Fabrication of laminated batteries)

[0142] The negative electrode prepared above was punched out in such a way that the coated surface was 4 cm × 5 cm in size and the tab (uncoated part) was 1 cm × 1.5 cm in size, and the positive electrode was punched out in such a way that it was 3.99 cm × 4.99 cm in size. As for the tab part, the lead tab with a sealant made of nickel for the negative electrode and aluminum for the positive electrode was joined by ultrasonic welding. The negative electrode separator was wound around for one week, and the collector side was heat-fused.

[0143] Fold the aluminum laminate sheet of 12cm horizontally and 10cm vertically in half horizontally, place the negative electrode with the membrane wrapped around it in the part where the sealant part overlaps with the edge of the aluminum laminate sheet, and fix the lower part of the sealant and the aluminum laminate sheet with polyimide tape. Next, place the positive electrode in a manner that it overlaps exactly with the negative electrode coating surface, and fix it with polyimide tape in the same way. The overlapping part (upper part) and the side of the aluminum laminate sheet and the seal part are respectively welded with a hot welder. After vacuum drying at 60°C for 12 hours with a vacuum dryer, inject the electrolyte from the bottom, and then heat-weld the lower part with a vacuum hot welder under vacuum. As the electrolyte, a mixed solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) (the volume ratio of EC to EMC is 3:7) is used, and 0.5% by mass of vinyl carbonate (VC) is added relative to the total amount of the mixed solution to dissolve LiPF6 in a manner to a concentration of 1 mol / L. As the separator, a polyethylene microporous film having a thickness of 20 μm was used.

[0144] It should be noted that the laminated battery was produced in a dry room at an outdoor temperature of -50°C.

[0145] (Aging treatment)

[0146] After the laminated battery is allowed to stand in a thermostatic chamber at 25°C for 12 hours, it is charged with a constant current (CC charge) to 4.2V at a current value equivalent to 0.2CA, and then charged with a constant voltage (CV charge) to a current value equivalent to 0.02CA. Next, CC discharge is performed to 2.7V at a current value equivalent to 0.2CA. This is regarded as one cycle. After repeating 3 cycles, CC-CV charge is performed again to 4.2V (CC: equivalent to 0.2CA, CV: equivalent to 0.02CA), and allowed to stand in a thermostatic chamber set at 60°C for 12 hours. Then, it is discharged to 2.7V at a current value equivalent to 0.2CA and aged. A rest time of 15 minutes is set between charging and discharging.

[0147] (Input Characteristics)

[0148] Regarding input characteristics, the aged battery was placed in a thermostatic chamber set at 25°C for 1 hour, and after adjusting the depth of charge (SOC) to 50%, it was charged for 10 seconds at current values ​​equivalent to 0.2C, 1C, 3C, and 5C, and the difference in voltage change at this time and the slope between each current value were calculated as the DC internal resistance (DC-IR). A rest time of 15 minutes was set between measurements at each current value.

[0149] It should be noted that the SOC can be adjusted by separately calculating the open circuit voltage for each SOC and performing CC-CV charging (CC: equivalent to 0.2 A, CV: equivalent to 0.02 C) to the voltage.

[0150] (Cycle Characteristics)

[0151] After the aged battery was left to stand in a thermostatic chamber set at 25°C for 1 hour, constant current charging (CC charging) was performed at a current value equivalent to 0.2C to 4.2V, and then constant voltage charging (CV charging) was performed to a current value equivalent to 0.02C. Next, CC discharge was performed at a current value equivalent to 0.2C to 2.7V. The discharge capacity at this time was taken as the initial discharge capacity. Then, the current value was changed to 1C, constant current charging was performed to 4.2V, and then constant voltage charging was performed to a current value equivalent to 0.02C. Next, discharge was performed to 2.7V at a current value equivalent to 1C. After repeating this 100 times, constant current charging (CC charging) was performed at a current value equivalent to 0.2C to 4.2V, and then constant voltage charging (CV charging) was performed to a current value equivalent to 0.02C. Next, CC discharge was performed at a current value equivalent to 0.2C to 2.7V. The discharge capacity at this time was taken as the discharge capacity after the cycle.

[0152] The cycle characteristics were calculated by the following formula.

[0153] Cycle performance (%) = discharge capacity after cycle (mAh) / initial discharge capacity (mAh) × 100

[0154] (Expansion rate)

[0155] The thickness of the laminated battery after initial discharge and after 100 cycles of discharge were measured, and the expansion rate was calculated from the following formula.

[0156] Expansion rate (%) = thickness after 100 cycles of discharge (mm) / thickness after initial discharge (mm) × 100

[0157] (Save Properties)

[0158] After the aged battery was left to stand in a thermostatic chamber set at 25°C for 1 hour, constant current charging (CC charging) was performed to 4.2 V at a current value equivalent to 0.2 C, and then constant voltage charging (CV charging) was performed to a current value equivalent to 0.02 C. Next, CC discharge was performed to 2.7 V at a current value equivalent to 0.2 C. The discharge capacity at this time was taken as the initial discharge capacity.

[0159] Then, the thermostat was changed to 60°C and left to stand for 10 days. After 10 days, the thermostat was set to 25°C, left to stand for 3 hours, and then discharged to 2.7V at a current value equivalent to 0.2C. Next, constant current charging (CC charging) was performed to 4.2V at a current value equivalent to 0.2C, and then constant voltage charging (CV charging) was performed to a current value equivalent to 0.02C. Next, CC discharge was performed to 2.7V at a current value equivalent to 0.2C. The capacity at this time was taken as the discharge capacity after storage.

[0160] The high temperature storage characteristics were calculated by the following formula.

[0161] High temperature storage characteristics (%) = discharge capacity after storage (mAh) / initial discharge capacity (mAh) × 100

[0162] [Example 2 to Example 6]

[0163] Graphite carbon materials B to F were obtained in the same manner as in the graphite carbon material A except that coke B (mosaic coke), coke C (mosaic coke), coke D (semi-needle coke), coke E (super needle coke) or coke F (mosaic coke) was used instead of coke A in Example 1. Batteries were prepared in the same manner as in Example 1 using the graphite carbon materials B to F, and the batteries were evaluated.

[0164] [Example 7]

[0165] Graphite carbon material A2 was obtained in the same manner as in Example 1 except that the particle size (D50) of graphite carbon material A was changed to 9 μm. A battery was produced in the same manner as in Example 1 using the graphite carbon material A2, and the battery was evaluated.

[0166] [Example 8]

[0167] Graphite carbon material A3 was obtained in the same manner as in Example 1 except that the particle size (D50) of graphite carbon material A was changed to 30 μm. A battery was produced in the same manner as in Example 1 using the graphite carbon material A3, and the battery was evaluated.

[0168] [Example 9]

[0169] After obtaining the graphite material A in Example 1, 5 parts by mass of coal tar pitch (softening point:) were mixed with 100 parts by mass of the graphite material A, and the temperature was raised to 1000°C at a heating rate of 200°C / h, and then kept for 1 hour for calcination. The calcination was carried out under a nitrogen atmosphere. After cooling to room temperature (25°C), the calcined sample was crushed to 15 μm with a shredder, and then screened with a sieve with a mesh of 0.109 mm to obtain a graphite carbon material AC1. Using the graphite carbon material AC1, a battery was made by the same method as in Example 1, and the battery was evaluated.

[0170] [Comparative Example 1]

[0171] The same operation was carried out except that the type of coke in Example 1 was changed to coke G which is super needle coke to obtain graphite carbon material G. A battery was produced by the same method as in Example 1 using the graphite carbon material G, and the battery was evaluated.

[0172] [Comparative Example 2]

[0173] A graphite carbon material H was obtained in the same manner as in Example 1 except that the type of coke in Example 1 was changed to coke H which is mosaic coke. A battery was produced using the graphite carbon material H in the same manner as in Example 1, and the battery was evaluated.

[0174] [Comparative Example 3]

[0175] In Example 1, except that coke B (mosaic coke) was used, the particle size (D50) was finely pulverized to 5.5 μm, heat treated at a maximum temperature of 1300° C., sintered at 2800° C., and no particle classification was performed after sintering, a graphite carbon material B2 was obtained by the same method as in Example 1. Using the graphite carbon material B2, a battery was manufactured by the same method as in Example 1, and the battery evaluation was performed.

[0176] [Table 1]

[0177]

[0178] [Table 2]

[0179]

[0180] As shown in the results of Table 2, the lithium ion secondary battery made using the negative electrode material of the embodiment has excellent input characteristics, high temperature storage characteristics and cycle characteristics compared with the lithium ion secondary battery made using the negative electrode material of the comparative example. Regarding other items, it can be seen that the characteristics are equal to or higher than those of the comparative example.

Claims

1. A graphite carbon material for a negative electrode of a lithium ion secondary battery, wherein the crystallite diameter Lc(002) determined by X-ray diffraction is 35 nm to 150 nm, and the tap density is greater than or equal to 0.90 g / cm 3 .

2. The graphite carbon material for a negative electrode of a lithium ion secondary battery according to claim 1, wherein in a particle size distribution measured by a laser diffraction scattering method, when a volume cumulative distribution curve is drawn from the smaller diameter side, the particle size D50 at the cumulative 50% is 5 μm to 30 μm.

3. The graphite carbon material for lithium ion secondary battery negative electrode according to claim 1 or 2, wherein in laser Raman spectrophotometry, 1330 cm -1 The intensity of the maximum peak near 1580 cm -1 The intensity ratio of the intensity Ig of the maximum peak in the vicinity, that is, Id / Ig, is 0.1 to 0.

5.

4. The graphite carbon material for a negative electrode of a lithium ion secondary battery according to any one of claims 1 to 3, wherein the specific surface area determined by nitrogen adsorption measurement at 77 K is 0.7 m 2 / g~8m 2 / g. 5 . The graphite carbon material for a negative electrode of a lithium ion secondary battery according to claim 1 , wherein a crystallite diameter La (110) determined by X-ray diffraction is 50 nm to 450 nm. 6 . The graphite carbon material for a negative electrode of a lithium ion secondary battery according to claim 1 , wherein the oil absorption of the graphite carbon material per 100 g is 30 mL to 75 mL in a linseed oil absorption measurement. 7 . A negative electrode material for a lithium ion secondary battery, comprising the graphite carbon material for a lithium ion secondary battery according to claim 1 . 8 . A negative electrode for a lithium ion secondary battery, comprising a graphite carbon material layer and a current collector, wherein the graphite carbon material layer comprises the graphite carbon material for a lithium ion secondary battery according to claim 1 . 9 . A lithium ion secondary battery comprising the negative electrode for a lithium ion secondary battery according to claim 8 , a positive electrode and an electrolyte.

Citation Information

Patent Citations

  • Graphite carbon material for lithium ion secondary battery negative electrode, method for manufacturing the same, and negative electrode or battery arranged by use thereof