Machine tool hard rail adjusting type ceramic spraying coating and method
Through laser spraying technology and multi-layer coating treatment, combined with sand blasting and heat treatment, the integrity and stability of ceramic coatings are solved, significantly improving the wear resistance, corrosion resistance and high temperature resistance of machine tool hard rails, and extending the Coating life.
Patent Information
- Application Number
- CN202411172966.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, it is difficult to ensure integrity and stability of ceramic spray coatings, especially in the case of multi-layer coatings, cracking and peeling are prone to occur, and wear resistance, corrosion resistance and high temperature resistance are insufficient.
Multi-layer ceramic coating spraying is used to spray with laser spraying, and appropriate cooling and curing are performed between each layer, combined with sandblasting and grinding pretreatment, high-purity silicon carbide is used as the ceramic coating material, and heat treatment and surface finishing Complete treatment to improve hardness and wear resistance, while regularly maintaining and maintaining to extend coating life.
It significantly improves the integrity, stability, wear resistance, corrosion resistance and high temperature resistance of the coating, reduces porosity and cracks, extends the service life of the coating, and ensures the continuous excellent performance of the coating.
Smart Images

Figure CN119040879A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of machine tool manufacturing, and in particular relates to an adjustable ceramic spray coating for a machine tool hard rail and a method thereof. Background Art
[0002] With the continuous development of industrial technology, the requirements for machine tool performance are getting higher and higher. Therefore, how to improve the wear resistance, corrosion resistance and high temperature resistance of hard rails has become an important research direction. Ceramic spraying technology, as an advanced surface treatment technology, has attracted much attention because it can form a layer of high hardness, high wear resistance and corrosion resistance on the surface of the substrate.
[0003] In the Chinese patent with publication number CN117960546A, a ductile iron metal ceramic spraying method is mentioned, including, S1, selecting ductile iron parts, selecting aluminum oxide and silicon carbide as metal ceramic powders, and cleaning and sandblasting the surface of the ductile iron parts, S2, mixing aluminum oxide, silicon carbide powder, adhesive, and solvent according to the ratio of 25% aluminum oxide powder, 25% silicon carbide powder, 15% epoxy resin adhesive, and 35% solvent, using a mixer to ensure that the slurry is evenly mixed, S3, selecting ion spraying technology to adjust the spraying. By adjusting the ratio of aluminum oxide and silicon carbide powder, and limiting the diameter and shape of aluminum oxide and silicon carbide powder, a consistent and high-quality coating is ensured, uniform coverage is ensured, and two drying methods are used to ensure a solid bond between the metal ceramic slurry and the ductile iron parts.
[0004] However, the above technical solution adjusts the ratio of aluminum oxide and silicon carbide powders, and limits the diameter and shape of aluminum oxide and silicon carbide powders to ensure consistency and high-quality coatings and uniform coverage. Although this method can form a strong bond with the parts through drying, the coating sprayed in this way is only a single layer, and it is difficult to ensure the integrity and stability of the coating, so the staff needs to improve it. Summary of the invention
[0005] The object of the present invention is to provide a machine tool hard rail adjustable ceramic spray coating and method to solve the problems raised in the above background technology.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A machine tool hard rail adjustable ceramic spraying method, comprising the following steps:
[0008] S1. Pretreatment and surface roughening of machine tool hard rails;
[0009] S2, ceramic coating selection;
[0010] S3, machine tool hard rail spraying process;
[0011] S4, post-spraying treatment;
[0012] S5. Maintenance and care.
[0013] Preferably, in step S1, the hard rail of the machine tool is thoroughly cleaned and degreased to remove grease, dirt and oxides on the surface.
[0014] Preferably, in step S1, the surface of the machine tool hard rail is formed to a certain degree of roughness by one of sandblasting and grinding.
[0015] Preferably, in step S2, silicon carbide is selected as the ceramic coating material.
[0016] Preferably, in step S3, the spraying equipment is prepared by selecting a laser spraying equipment, ensuring that the laser spraying equipment is in good working condition, and adjusting the spraying parameters.
[0017] Preferably, in step S3, ceramic powder spraying: silicon carbide is fed into a laser spraying device, the powder is melted by laser and sprayed onto the pre-treated surface of the machine tool hard rail, and during the spraying process, the uniformity and continuity of the spraying are maintained.
[0018] Preferably, in step S3, multi-layer spraying is performed: during multi-layer spraying, appropriate cooling and curing treatment is required between each layer to avoid cracking and peeling of the coating.
[0019] Preferably, in step S4, after spraying is completed, the coating is heat treated to improve its hardness and wear resistance, the heat treated coating is surface finished to remove burrs and uneven parts on the surface, and finally, the coating is quality inspected.
[0020] Preferably, in step S5, the machine tool hard rail ceramic coating is regularly maintained and serviced, including but not limited to cleaning the coating surface, avoiding contact with corrosive substances and regularly checking the coating condition.
[0021] A machine tool hard rail adjustable ceramic spray coating, comprising:
[0022] Guide rail body;
[0023] A first ceramic coating is fixedly connected to one side of the surface of the guide rail body, a second ceramic coating is fixedly connected to one side of the surface of the first ceramic coating, and a third ceramic coating is fixedly connected to one side of the surface of the second ceramic coating.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) Multilayer ceramic coatings can better disperse stress and resist wear, and provide better wear resistance, corrosion resistance and high temperature resistance. During the multilayer spraying process, proper cooling and curing treatment is required between each layer to avoid cracking and peeling of the coating, ensuring the integrity and stability of the multilayer coating and improving the comprehensive performance of the coating.
[0026] (2) Ceramic coatings are sprayed using laser spraying technology. Laser spraying technology has the advantages of high energy density, high precision and high efficiency. It can instantly melt ceramic powder and evenly spray it onto the surface of the substrate to form a high-quality coating. It not only improves the density and uniformity of the coating, but also significantly reduces defects such as porosity and cracks in the coating.
[0027] (3) The importance of regular maintenance and care of the machine tool hard rail ceramic coating, including cleaning the coating surface, avoiding contact with corrosive substances and regularly checking the coating condition, can extend the service life of the coating and ensure its continued excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 is a process flow chart of the present invention;
[0029] Figure 2 A perspective view of the present invention;
[0030] Figure 3 is a three-dimensional diagram of the first ceramic coating of the present invention;
[0031] In the figure: 1. guide rail body; 2. first ceramic coating; 3. second ceramic coating; 4. third ceramic coating. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Embodiment 1:
[0034] See also Figures 1 to 3 As shown, a machine tool hard rail adjustable ceramic spraying method comprises the following steps:
[0035] S1. Pretreatment and surface roughening of machine tool hard rails;
[0036] S2, ceramic coating selection;
[0037] S3, machine tool hard rail spraying process;
[0038] S4, post-spraying treatment;
[0039] S5. Maintenance and care.
[0040] In step S1, the machine tool hard rail is thoroughly cleaned and degreased to remove grease, dirt and oxides on the surface, which is achieved by one of sandblasting and grinding, so that the surface of the machine tool hard rail has a certain degree of roughness;
[0041] First, use a high-pressure water gun and special cleaning agent to thoroughly clean the machine tool hard rail to remove grease, dirt and most oxides on the surface. Then, use a sand blasting machine to roughen the surface. Select medium-sized sand particles and sandblast the surface of the guide rail at appropriate pressure and angle to ensure that the surface forms a uniform microstructure with a certain degree of roughness, which helps to enhance the bonding between the ceramic coating and the substrate.
[0042] In step S2, silicon carbide is selected as the ceramic coating material;
[0043] High-purity silicon carbide is selected as the ceramic coating material because of its excellent hardness, wear resistance and corrosion resistance, and is very suitable for surface protection of machine tool hard rails.
[0044] In step S3, spraying equipment preparation: select laser spraying equipment, ensure that the laser spraying equipment is in good working condition, and adjust the spraying parameters; ceramic powder spraying: feed silicon carbide into the laser spraying equipment, melt the powder by laser and spray it onto the pre-treated machine tool hard rail surface, and maintain the uniformity and continuity of the spraying during the spraying process; multi-layer spraying: during multi-layer spraying, appropriate cooling and curing treatment is required between each layer to avoid cracking and peeling of the coating;
[0045] Spraying equipment preparation: Select high-precision, high-stability laser spraying equipment, and conduct a comprehensive equipment inspection to ensure that all components are operating normally. According to the characteristics of silicon carbide powder and the requirements of the guide rail surface, adjust the laser power, spraying speed, and the distance between the spray gun and the guide rail surface.
[0046] Ceramic powder spraying: Silicon carbide powder is evenly fed into the laser spraying equipment through the powder feeding system. The laser beam melts the powder instantly and sprays it at high speed onto the pre-treated guide rail surface. During the spraying process, an automatic control system is used to monitor the spraying quality to ensure the uniformity and continuity of the spraying.
[0047] Multi-layer spraying: In order to obtain a thicker and more uniform ceramic coating, multi-layer spraying is performed. After each layer of spraying is completed, sufficient cooling and curing treatment is carried out to prevent the coating from cracking and peeling. At the same time, the thickness and cooling time of each layer of spraying are adjusted according to the coating thickness and performance requirements.
[0048] In step S4, after spraying, the coating is heat treated to improve its hardness and wear resistance, and the heat-treated coating is surface finished to remove burrs and uneven parts on the surface. Finally, the coating is quality tested;
[0049] Heat treatment: Place the sprayed guide rail in a vacuum heat treatment furnace for high-temperature heat treatment to improve the hardness and wear resistance of the coating. During the heat treatment process, the temperature and time are strictly controlled to avoid cracks or deformation of the coating.
[0050] Surface finishing: After heat treatment, use precision grinding and polishing equipment to finish the coating surface to remove burrs and uneven parts on the surface, making the coating surface smoother and flatter.
[0051] Quality inspection: Use hardness testers, wear testers, microscopes and other testing equipment to conduct comprehensive quality inspections on the coating to ensure that the coating performance meets the design requirements.
[0052] In step S5, the machine tool hard rail ceramic coating is regularly maintained and serviced, including but not limited to cleaning the coating surface, avoiding contact with corrosive substances, and regularly checking the coating condition;
[0053] Clean, inspect and maintain the ceramic coating on the machine tool hard rail regularly. Use special cleaning agents and soft cloth to clean the coating surface. Avoid scratching or colliding the coating with hard objects. At the same time, pay attention to avoid contact between the coating and corrosive substances. Check the coating condition regularly and repair it in time if it is damaged.
[0054] A machine tool hard rail adjustable ceramic spray coating, comprising:
[0055] Guide rail body 1;
[0056] A first ceramic coating 2 is fixedly connected to one side of the surface of the guide rail body 1 , a second ceramic coating 3 is fixedly connected to one side of the surface of the first ceramic coating 2 , and a third ceramic coating 4 is fixedly connected to one side of the surface of the second ceramic coating 3 .
[0057] The ceramic coating can be adhered to the surface of the guide rail body 1 by glue.
[0058] Experimental Materials:
[0059] Machine tool hard rail sample (material: HT250 gray cast iron);
[0060] Ceramic coating material: high purity silicon carbide powder;
[0061] Laser spraying equipment: Model XYZ-LP100, laser power adjustable range is 500W to 3000W;
[0062] Cleaning and degreasing agent: special cleaning agent XYZ-C100;
[0063] Sandblasting machine: Model ABC-S500, using medium-sized sand;
[0064] Heat treatment furnace: vacuum heat treatment furnace, the maximum temperature can reach 1200℃;
[0065] Testing equipment: hardness tester (model HV-1000), wear tester (model AM-500), microscope (model MX-50);
[0066] Experimental steps:
[0067] Follow the steps in Example 1, as follows:
[0068] S1: Cleaning and degreasing: Use a high-pressure water gun and XYZ-C100 cleaning agent to thoroughly clean the surface of the guide rail, and then perform sandblasting to form a uniform roughness.
[0069] S2: Silicon carbide is selected as the ceramic coating material.
[0070] S3: Use XYZ-LP100 laser spraying equipment for spraying, adjust the laser power to 2000W, set the spraying speed to 50mm / s, keep the distance between the spray gun and the guide rail surface at 10mm, perform multi-layer spraying, and the cooling and curing time between each layer is 10 minutes. After spraying the ceramic coating, perform high-precision circular grinding.
[0071] S4: Heat treatment is carried out in a vacuum heat treatment furnace, the temperature is set to 1000°C, the holding time is 2 hours, and then surface finishing treatment is carried out.
[0072] S5: Conduct coating quality inspection and performance test.
[0073] Experimental results and data:
[0074] Surface roughness:
[0075] After sandblasting, the surface roughness Ra value of the guide rail reaches 6.3μm, which meets the roughness requirements of ceramic coating spraying.
[0076] Coating thickness:
[0077] After three layers of ceramic coating spraying, the total coating thickness reaches 1mm, the thickness of each layer is about 0.33mm, and the coating uniformity is good.
[0078] Hardness test:
[0079] Using a HV-1000 hardness tester to test, the surface hardness of the coating reaches HV1200, which is significantly higher than the hardness of the substrate HT250 gray cast iron (about HB180-220).
[0080] Abrasion resistance test:
[0081] In the test on the AM-500 wear tester, the coating was subjected to a load of 500N and after 1000 reciprocating frictions, the wear loss was only 0.02mm, showing excellent wear resistance.
[0082] Corrosion resistance test:
[0083] After the coating was immersed in 5% NaCl solution for 72 hours, there was no obvious corrosion sign on the surface, indicating that the coating has good corrosion resistance.
[0084] Porosity and crack detection:
[0085] The coating surface and cross-section were observed using an MX-50 microscope, and no obvious pores or cracks were found, indicating that the coating had good density.
[0086] Conclusion: Experimental data show that the ceramic spraying method for machine tool hard rails can significantly improve the hardness, wear resistance and corrosion resistance of the guide rails, while ensuring the uniformity and density of the coating. Through multi-layer spraying and appropriate cooling and curing treatment, the cracking and peeling of the coating are effectively avoided, ensuring the integrity and stability of the coating. Therefore, this method has broad application prospects in the surface protection of machine tool hard rails.
[0087] Embodiment 2:
[0088] See also Figures 1 to 3 As shown, a machine tool hard rail adjustable ceramic spraying method comprises the following steps:
[0089] S1. Pretreatment and surface roughening of machine tool hard rails;
[0090] S2, ceramic coating selection;
[0091] S3, machine tool hard rail spraying process;
[0092] S4, post-spraying treatment;
[0093] S5. Maintenance and care.
[0094] In step S1, the machine tool hard rail is thoroughly cleaned and degreased to remove grease, dirt and oxides on the surface, the surface of the rail is micro-arc oxidized, and then one of sandblasting and grinding is used to form a certain roughness on the surface of the machine tool hard rail;
[0095] First, use a high-pressure water gun and a special cleaning agent to thoroughly clean the machine tool hard rail to remove grease, dirt and most oxides on the surface. Micro-arc oxidation is a technology that forms a ceramic oxide film on the metal surface, which can further improve the bonding strength between the substrate and the ceramic coating. Subsequently, a sand blasting machine is used for surface roughening treatment. Medium-sized sand particles are selected and the guide rail surface is sandblasted at appropriate pressure and angle to ensure that the surface forms a uniform microstructure with a certain degree of roughness, which helps to enhance the bonding strength between the ceramic coating and the substrate. Micro-arc oxidation treatment is performed first, and then sandblasting or grinding is performed to obtain better surface roughness and bonding strength.
[0096] In step S2, silicon carbide is selected as the ceramic coating material;
[0097] High-purity silicon carbide is selected as the ceramic coating material because of its excellent hardness, wear resistance and corrosion resistance, and is very suitable for surface protection of machine tool hard rails.
[0098] In step S3, spraying equipment preparation: select laser spraying equipment, ensure that the laser spraying equipment is in good working condition, and adjust the spraying parameters; ceramic powder spraying: feed silicon carbide into the laser spraying equipment, melt the powder by laser and spray it onto the pre-treated machine tool hard rail surface, and maintain the uniformity and continuity of the spraying during the spraying process; multi-layer spraying: during multi-layer spraying, appropriate cooling and curing treatment is required between each layer to avoid cracking and peeling of the coating;
[0099] Spraying equipment preparation: Select high-precision, high-stability laser spraying equipment, and conduct a comprehensive equipment inspection to ensure that all components are operating normally. According to the characteristics of silicon carbide powder and the requirements of the guide rail surface, adjust the laser power, spraying speed, and the distance between the spray gun and the guide rail surface.
[0100] Ceramic powder spraying: Silicon carbide powder is evenly fed into the laser spraying equipment through the powder feeding system. The laser beam melts the powder instantly and sprays it at high speed onto the pre-treated guide rail surface. During the spraying process, an automatic control system is used to monitor the spraying quality to ensure the uniformity and continuity of the spraying.
[0101] Multi-layer spraying: In order to obtain a thicker and more uniform ceramic coating, multi-layer spraying is performed. After each layer of spraying is completed, sufficient cooling and curing treatment is carried out to prevent the coating from cracking and peeling. At the same time, the thickness and cooling time of each layer of spraying are adjusted according to the coating thickness and performance requirements.
[0102] In step S4, after spraying, the coating is heat treated to improve its hardness and wear resistance, and the heat-treated coating is surface finished to remove burrs and uneven parts on the surface. Finally, the coating is quality tested;
[0103] Heat treatment: Place the sprayed guide rail in a vacuum heat treatment furnace for high-temperature heat treatment to improve the hardness and wear resistance of the coating. During the heat treatment process, the temperature and time are strictly controlled to avoid cracks or deformation of the coating.
[0104] Surface finishing: After heat treatment, use precision grinding and polishing equipment to finish the coating surface to remove burrs and uneven parts on the surface, making the coating surface smoother and flatter.
[0105] Quality inspection: Use hardness testers, wear testers, microscopes and other testing equipment to conduct comprehensive quality inspections on the coating to ensure that the coating performance meets the design requirements.
[0106] In step S5, the machine tool hard rail ceramic coating is regularly maintained and serviced, including but not limited to cleaning the coating surface, avoiding contact with corrosive substances, and regularly checking the coating condition;
[0107] Clean, inspect and maintain the ceramic coating on the machine tool hard rail regularly. Use special cleaning agents and soft cloth to clean the coating surface. Avoid scratching or colliding the coating with hard objects. At the same time, pay attention to avoid contact between the coating and corrosive substances. Check the coating condition regularly and repair it in time if it is damaged.
[0108] A machine tool hard rail adjustable ceramic spray coating, comprising:
[0109] Guide rail body 1;
[0110] A first ceramic coating 2 is fixedly connected to one side of the surface of the guide rail body 1 , a second ceramic coating 3 is fixedly connected to one side of the surface of the first ceramic coating 2 , and a third ceramic coating 4 is fixedly connected to one side of the surface of the second ceramic coating 3 .
[0111] Embodiment three:
[0112] See also Figures 1 to 3 As shown, a machine tool hard rail adjustable ceramic spraying method comprises the following steps:
[0113] S1. Pretreatment and surface roughening of machine tool hard rails;
[0114] S2, ceramic coating selection;
[0115] S3, machine tool hard rail spraying process;
[0116] S4, post-spraying treatment;
[0117] S5. Maintenance and care.
[0118] In step S1, the machine tool hard rail is thoroughly cleaned and degreased to remove grease, dirt and oxides on the surface, the surface of the rail is micro-arc oxidized, and then sandblasted or polished to form a certain roughness on the surface of the machine tool hard rail;
[0119] First, use a high-pressure water gun and a special cleaning agent to thoroughly clean the machine tool hard rail to remove grease, dirt and most oxides on the surface. Micro-arc oxidation is a technology that forms a ceramic oxide film on the metal surface, which can further improve the bonding strength between the substrate and the ceramic coating. Subsequently, a sand blasting machine is used for surface roughening treatment. Medium-sized sand particles are selected and the guide rail surface is sandblasted at appropriate pressure and angle to ensure that the surface forms a uniform microstructure with a certain degree of roughness, which helps to enhance the bonding strength between the ceramic coating and the substrate. Micro-arc oxidation treatment is performed first, and then sandblasting or grinding is performed to obtain better surface roughness and bonding strength.
[0120] In step S2, silicon carbide is selected as the ceramic coating material;
[0121] High-purity silicon carbide is selected as the ceramic coating material because of its excellent hardness, wear resistance and corrosion resistance, and is very suitable for surface protection of machine tool hard rails.
[0122] In step S3, spraying equipment preparation: plasma spraying equipment is selected to ensure that the plasma spraying equipment is in good working condition and the spraying parameters are adjusted. Ceramic powder spraying: plasma spraying has higher energy density and better coating uniformity, and is particularly suitable for spraying high melting point and high hardness ceramic materials. Plasma spraying equipment is selected to feed silicon carbide powder into a plasma spray gun, and the powder is melted by a plasma arc and sprayed onto the surface of the guide rail at high speed. Multi-layer spraying: During multi-layer spraying, appropriate cooling and curing treatment is required between each layer to avoid cracking and peeling of the coating.
[0123] Spraying equipment preparation: Select high-precision, high-stability laser spraying equipment, and conduct a comprehensive equipment inspection to ensure that all components are operating normally. According to the characteristics of silicon carbide powder and the requirements of the guide rail surface, adjust the laser power, spraying speed, and the distance between the spray gun and the guide rail surface.
[0124] Ceramic powder spraying: Silicon carbide powder is evenly fed into the laser spraying equipment through the powder feeding system. The laser beam melts the powder instantly and sprays it at high speed onto the pre-treated guide rail surface. During the spraying process, an automatic control system is used to monitor the spraying quality to ensure the uniformity and continuity of the spraying.
[0125] Multi-layer spraying: In order to obtain a thicker and more uniform ceramic coating, multi-layer spraying is performed. After each layer of spraying is completed, sufficient cooling and curing treatment is carried out to prevent the coating from cracking and peeling. At the same time, the thickness and cooling time of each layer of spraying are adjusted according to the coating thickness and performance requirements.
[0126] In step S4, after spraying, the coating is heat treated to improve its hardness and wear resistance, and the heat-treated coating is surface finished to remove burrs and uneven parts on the surface. Finally, the coating is quality tested;
[0127] Heat treatment: Place the sprayed guide rail in a vacuum heat treatment furnace for high-temperature heat treatment to improve the hardness and wear resistance of the coating. During the heat treatment process, the temperature and time are strictly controlled to avoid cracks or deformation of the coating.
[0128] Surface finishing: After heat treatment, use precision grinding and polishing equipment to finish the coating surface to remove burrs and uneven parts on the surface, making the coating surface smoother and flatter.
[0129] Quality inspection: Use hardness testers, wear testers, microscopes and other testing equipment to conduct comprehensive quality inspections on the coating to ensure that the coating performance meets the design requirements.
[0130] In step S5, the machine tool hard rail ceramic coating is regularly maintained and serviced, including but not limited to cleaning the coating surface, avoiding contact with corrosive substances, and regularly checking the coating condition;
[0131] Clean, inspect and maintain the ceramic coating on the machine tool hard rail regularly. Use special cleaning agents and soft cloth to clean the coating surface. Avoid scratching or colliding the coating with hard objects. At the same time, pay attention to avoid contact between the coating and corrosive substances. Check the coating condition regularly and repair it in time if it is damaged.
[0132] A machine tool hard rail adjustable ceramic spray coating, comprising:
[0133] Guide rail body 1;
[0134] A first ceramic coating 2 is fixedly connected to one side of the surface of the guide rail body 1 , a second ceramic coating 3 is fixedly connected to one side of the surface of the first ceramic coating 2 , and a third ceramic coating 4 is fixedly connected to one side of the surface of the second ceramic coating 3 .
[0135] The standard parts used in the present invention can all be purchased from the market, and the special-shaped parts can be customized according to the description and the drawings. The specific connection methods of each part adopt conventional means such as mature bolts, rivets, welding, etc. in the prior art. The machinery, parts and equipment all adopt conventional models in the prior art, and the circuit connection adopts the conventional connection method in the prior art, which will not be described in detail here. The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.
[0136] In the description of the present invention, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. "Multiple" means two or more, unless otherwise clearly and specifically defined.
[0137] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0138] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0139] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.
[0140] In the drawings of the embodiments disclosed in the present invention, only the structures related to the embodiments disclosed in the present invention are involved, and other structures can refer to the general design. In the absence of conflict, the same embodiment and different embodiments of the present invention can be combined with each other.
[0141] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A machine tool hard rail adjustable ceramic spraying method, characterized in that: The following steps are involved: S1. Pretreatment and surface roughening of machine tool hard rails; S2, ceramic coating selection; S3, machine tool hard rail spraying process; S4, post-spraying treatment; S5. Maintenance and care.
2. The method for adjusting ceramic spraying of machine tool hard rail according to claim 1, characterized in that: In step S1, the hard rail of the machine tool is thoroughly cleaned and degreased to remove grease, dirt and oxides on the surface.
3. The method for adjusting ceramic spraying of machine tool hard rail according to claim 1, characterized in that: In step S1, a certain roughness is formed on the surface of the machine tool hard rail by one of sandblasting and grinding.
4. The method for adjusting ceramic spraying of machine tool hard rail according to claim 1, characterized in that: In step S2 , silicon carbide is selected as the ceramic coating material.
5. The method for adjusting ceramic spraying of machine tool hard rail according to claim 1, characterized in that: In step S3, the spraying equipment is prepared: a laser spraying equipment is selected, the laser spraying equipment is ensured to be in good working condition, and the spraying parameters are adjusted.
6. The method for adjusting ceramic spraying of machine tool hard rail according to claim 1, characterized in that: In step S3, ceramic powder spraying: silicon carbide is fed into a laser spraying device, the powder is melted by laser and sprayed onto the pre-treated surface of the machine tool hard rail, and during the spraying process, the uniformity and continuity of the spraying are maintained.
7. The method for adjusting ceramic spraying of machine tool hard rail according to claim 1, characterized in that: In step S3, multi-layer spraying: During multi-layer spraying, appropriate cooling and curing treatment is required between each layer to avoid cracking and peeling of the coating.
8. The method for adjusting ceramic spraying of machine tool hard rail according to claim 1, characterized in that: In step S4, after spraying, the coating is heat treated to improve its hardness and wear resistance, and the heat-treated coating is surface finished to remove burrs and uneven parts on the surface. Finally, the coating is quality inspected.
9. The method for adjusting ceramic spraying of machine tool hard rail according to claim 1, characterized in that: In step S5, the machine tool hard rail ceramic coating is regularly maintained and serviced, including but not limited to cleaning the coating surface, avoiding contact with corrosive substances, and regularly checking the coating condition.
10. An adjustable ceramic spray coating for machine tool hard rail, suitable for the adjustable ceramic spray coating method for machine tool hard rail according to claims 1 to 9, characterized in that: include: Guide rail body (1); A first ceramic coating (2) is fixedly connected to one side of the surface of the guide rail body (1), a second ceramic coating (3) is fixedly connected to one side of the surface of the first ceramic coating (2), and a third ceramic coating (4) is fixedly connected to one side of the surface of the second ceramic coating (3).