An apparatus and method for rapid preparation of hollow nanofibers via airflow induction

The method of preparing hollow nanofibers by airflow-induced coaxial needles solves the problems of difficult preparation conditions and safety hazards in existing technologies, and realizes the rapid, safe and clean mass preparation of hollow nanofibers. It is applicable to a variety of materials and has good application prospects.

CN119041037BActive Publication Date: 2026-11-17SICHUAN UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411003648.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2026-11-17
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

Existing technologies for preparing hollow nanofibers suffer from problems such as difficult preparation conditions, low yield, significant safety hazards, inapplicability to non-conductive materials, and electric field interference, which limit the production and application of hollow nanofibers.

Method used

Using an airflow-induced method, the core and shell solutions are combined under high-speed airflow through a coaxial needle to form coaxial nanofibers, which are then collected by a collector. Subsequently, the core material is removed by high-temperature calcination to prepare hollow nanofibers.

Benefits of technology

It has achieved rapid, safe, and clean preparation of large quantities of uniform hollow nanofibers, which are suitable for a variety of materials, have self-spinning properties, and are highly adaptable to applications in fields such as thermal insulation and mechanics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119041037B_ABST
    Figure CN119041037B_ABST
Patent Text Reader

Abstract

This invention discloses an apparatus and method for rapidly preparing hollow nanofibers via airflow induction. First, the structure of a coaxial needle is designed, consisting of two capillary tubes of different inner diameters coaxially nested together. The inner tube at one end of the coaxial needle extends to the outside of the outer tube, serving as the fiber outlet. A section of the coaxial needle near the fiber outlet is bent at 90° to form a vertical segment. An airflow channel is positioned on the side of the bend, with the gas outlet of the airflow channel facing the vertical segment. Hollow fibers are prepared using airflow induction combined with the coaxial needle. A core layer solution and a shell layer solution are injected into the coaxial needle, respectively. The two solutions converge at the fiber outlet and directly solidify under the action of a high-speed airflow to form core-shell coaxial nanofibers. After collecting the fibers using a collector, they are then subjected to high-temperature calcination to remove the core layer material, yielding the hollow nanofibers. This method can rapidly and directly prepare large quantities of uniform hollow nanofibers and is safe and clean.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of materials science and engineering, and in particular to an apparatus and method for the rapid and large-scale preparation of hollow nanofibers by airflow induction. Background Technology

[0002] One-dimensional nanostructures of polymer materials possess unique morphological structures that grant them advantages such as high aspect ratio, light weight, high temperature resistance, good thermal stability, stable chemical properties, and resistance to mechanical vibration, making them profoundly influential in numerous fields including aerospace, biomedicine, environmental energy, and electronic communications. To obtain lighter, more stable, and more flexible one-dimensional nanomaterials, hollow nanofibers have become a new research hotspot. Current methods for preparing hollow nanofibers include phase inversion, template methods, extrusion molding, and electrospinning. However, these methods often suffer from drawbacks such as difficult preparation conditions, low yield, and high cost, limiting the production and application of hollow nanofibers.

[0003] Currently, hollow nanofibers are mostly prepared using electrospinning, which is essentially the same principle as the traditional preparation of solid fibers, with improvements made to the equipment, specifically the spinneret. Solutions of the core and shell materials are separately packaged into two different syringes. The spinneret system consists of two coaxial capillaries with different inner diameters. Under the influence of a high-voltage electric field, the outer liquid flows out and merges with the core liquid. Because the merging time of the two solutions at the nozzle is very short during spinning, and the polymer has a low diffusion coefficient, they do not mix before solidification. Under the influence of the high-voltage electric field, the shell liquid is subjected to high-frequency stretching and high-speed jetting. During high-speed jetting, strong shear stress is generated at the interface between the inner and outer solutions. Under this shear stress, the core solution moves coaxially along the shell, bending, deforming, and solidifying into ultrafine coaxial composite nanofibers. The coaxial composite nanofibers are then subjected to post-treatment methods such as solvent extraction or high-temperature calcination to remove the core material, while preserving the outer physical structure, resulting in nanofibers with a hollow structure. Electrospinning requires high-voltage electrostatic discharge to produce nanofibers, but the 5-30 kV voltage poses numerous safety hazards. Non-conductive precursor solutions lack self-spinning properties. Electrospinning equipment requires conductive materials as collecting plates, as some non-conductive surfaces cannot be directly spun. The fibers collected during electrospinning adhere to the collecting plate, and the secondary transfer process may cause some damage to the sample. In industrial production with multi-needle electrospinning, the excessively dense needles can cause mutual interference of electric fields, disrupting the spinning process and affecting the quality of nanofibers. Therefore, to obtain hollow nanofibers with a simple preparation process, high efficiency, and large yield, a direct, rapid, efficient, and universally applicable method needs to be developed. Summary of the Invention

[0004] The purpose of this invention is to provide an apparatus and method for rapidly preparing hollow nanofibers by airflow induction.

[0005] This invention employs an airflow-induced method with coaxial needles to directly prepare hollow fibers. Core layer solution and shell layer solution are injected into two coaxial needles formed by capillaries with different inner diameters. The two solutions converge at the fiber outlet of the coaxial needle and are directly solidified into shell-core coaxial nanofibers under the action of high-speed airflow. The fibers are collected by a collector. Then, the core layer material is removed by calcination to obtain hollow nanofibers.

[0006] The device for rapidly preparing hollow nanofibers by airflow induction provided by the present invention includes: a coaxial needle for electrospinning, a compressed air pump, a collector, a high-temperature calcination device, a shell solution injection pump, and a core solution injection pump.

[0007] The coaxial needle consists of two capillary tubes with different inner diameters, coaxially fitted together. Both the inner and outer tube ends at one end of the coaxial needle are sealed. At the other end, the inner tube extends beyond the outer tube as the fiber outlet, with the inner tube extending by a length H relative to the outer tube, where H is equal to half the radius of the outer tube. A section of the coaxial needle near the fiber outlet is bent at 90° to form a vertical section. An airflow channel is positioned on the side of the bend, with its centerline aligned with the centerline of the vertical section. The airflow channel is connected to a compressed air pump, with its gas outlet facing the vertical section, used to apply airflow to the fibers at the fiber outlet. The compressed air pump injects any one of the following gases: air, nitrogen, argon, or a mixture of gases, into the airflow channel.

[0008] The shell solution injection pump injects the shell solution into the annular space between the inner and outer tubes; the core solution injection pump injects the core solution into the internal cavity of the inner tube; the collector is used to collect the fibers prepared by the coaxial needle; the high-temperature calcination device removes the core material by high-temperature sintering to obtain hollow nanofibers.

[0009] Preferably, the collector can be a cage-type collector used to collect spun fibers to form a three-dimensional structure, which is then calcined to form a hollow nanofiber sponge.

[0010] The apparatus is used to prepare hollow fibers from any of the following materials: polyimide, polyacrylonitrile, yttrium-stabilized zirconium oxide, and polyvinyl butyral.

[0011] This invention also provides a method for rapidly preparing hollow nanofibers via airflow induction, namely, using the aforementioned apparatus. The method steps are as follows: S1. Select the shell material and core solution. The shell material is selected from any one of polyimide, polyacrylonitrile, yttrium-stabilized zirconium oxide, and polyvinyl butyral. A solvent is used to dissolve the shell material to form the shell solution. The core solution must be immiscible with the shell solution and not react with it, have a viscosity similar to the shell material, and be removable during the preparation process by high-temperature calcination. The core solution does not require self-spinning properties; it can be either a precursor solution capable of spinning two different materials, or an oily substance that is immiscible and lacks self-spinning properties.

[0012] S2. The shell solution and core solution are injected into the coaxial needle respectively and converge at the tip of the coaxial needle. The compressed air pump is turned on to provide airflow. Under the action of high-speed airflow, the shell solution and core solution are stretched to form a coaxial Taylor cone. Then the coaxial jet undergoes bending and unstable motion, while the solvent evaporates and the solute finally solidifies and deposits in the collector.

[0013] S3. The collected fibers are calcined at high temperature to remove the core material, resulting in hollow nanofibers.

[0014] Preferably, polyethylene oxide (PEO) or polyvinylpyrrolidone (PVP) can also be added to the shell solution to increase the viscosity and spinnability of the solution.

[0015] Preferably, in step S2, the ratio of the propulsion rates of the shell solution and the core solution in the coaxial needle is controlled to be 2:1.

[0016] Compared with the prior art, the advantages of the present invention are: (1) The method of the present invention can rapidly and directly prepare a large number of uniform hollow nanofibers, and is safe and clean; the diameter of the prepared hollow nanofibers is controllable and the uniformity is good, and the prepared materials have good applications in the fields of heat insulation and mechanical high-temperature elasticity.

[0017] (2) The device and method of this invention prepare hollow fiber structures at the physical level through the design of coaxial needles. All self-spinning systems (polymer, ceramic and other systems) are applicable. This preparation method has good portability.

[0018] Other advantages, objectives and features of the present invention will become apparent in part from the following description, and in part from those skilled in the art through study and practice of the invention. Attached Figure Description

[0019] Figure 1 : A schematic diagram of the device for rapid preparation of hollow nanofibers by airflow induction provided by the present invention.

[0020] Figure 2Figure 1 shows the structure of the coaxial needle. Figure (a) shows the relationship between the airflow direction and the position of the coaxial needle, and Figure (b) shows the specific dimensions of the coaxial needle in this embodiment.

[0021] Figure 3 Optical photographs of the formation, stretching process, and shell-core structure of a coaxial jet taken with a high-speed camera.

[0022] Figure 4 Different V in / V out SEM images of fibers obtained under the ratio; (a) is V in / V out SEM image of beaded fibers obtained when = 1 / 4, (b) is V in / V out SEM image of uniform hollow fiber obtained when = 1 / 2.

[0023] Figure 5 : Performance diagrams of sponges made of polyimide hollow nanofibers; where (a) is an ultralight demonstration diagram, (b) is a low-magnification SEM image of polyimide hollow nanofibers, (c) is a high-magnification SEM image, and (d) is a fiber diameter distribution diagram.

[0024] Figure 6 : Thermal conductivity performance of polyimide hollow nanofiber sponge; (a) is a graph showing the relationship between thermal conductivity and sponge density, and (b) is a comparison of the working space of polyimide hollow nanofiber sponge and other thermal insulation sponges.

[0025] Figure 7 The results of the heat resistance test of polyimide hollow nanofiber sponge and other materials: (a) is a comparison of the thermogravimetric curves of polyimide hollow nanofiber sponge, polyurethane sponge, polystyrene sponge and cork; (b) is the curve of the surface temperature of the sample versus time in the heat resistance comparison experiment of polyimide hollow nanofiber sponge, polyurethane sponge and polystyrene sponge; (c) is the optical and infrared thermal imaging comparison of the heat resistance comparison experiment.

[0026] Figure 8 Infrared thermal image of polyimide hollow nanofiber sponge.

[0027] Figure 9 Demonstration diagram of the compression and recovery of polyimide hollow nanofiber sponge at different temperatures.

[0028] Figure 10 Fatigue test curves of hollow nanofiber sponges with different densities; (a) is the density of 50 mg / cm³. 3 The fatigue test curves of hollow nanofiber sponge after 1000 cycles, (b) is for a density of 80 mg / cm³. 3The strain curve of the fiber sponge after 1000 cycles at 80% strain is shown.

[0029] Figure 11 Optical image recovered after hollow nanofiber sponge is bent and folded at 180°.

[0030] Figure 12 Polyimide hollow nanofiber sponges in various colors.

[0031] Figure 13 Comparative experiment of hollow nanofiber sponge filled with argon and air after vacuuming. Detailed Implementation

[0032] The preferred embodiments of the present invention will be described below with reference to the accompanying drawings. It should be understood that the preferred embodiments described herein are for illustration and explanation only and are not intended to limit the present invention.

[0033] like Figure 1 As shown, the structure of the device for rapidly preparing hollow nanofibers by airflow induction provided by the present invention includes a coaxial needle for electrospinning, a compressed air pump, a collector, a high-temperature calcination device, a shell solution injection pump, and a core solution injection pump.

[0034] The design of the coaxial needle described above is as follows: Figure 2 As shown, the coaxial needle consists of two capillary tubes with different inner diameters, coaxially fitted together. Both the inner and outer tube ends at one end of the coaxial needle are sealed. At the other end, the inner tube extends beyond the outer tube as the fiber outlet, with the inner tube extending H relative to the outer tube. A section of the coaxial needle near the fiber outlet end is bent at 90° to form a vertical section. An airflow channel is located on the side of the bend, with the centerline of the airflow channel and the centerline of the vertical section collinear. See details... Figure 2 In section (a), an airflow duct is connected to a compressed air pump, with the gas outlet of the duct facing the vertical section to apply airflow to the fibers at the fiber outlet. The compressed air pump is used to inject any one of the following gases: air, nitrogen, argon, or a mixed gas, into the airflow duct. In practical applications, the wall thickness of the hollow fibers obtained after calcination can be adjusted by changing the ratio of the inner diameter of the inner tube to the outer tube of the coaxial needle. The value of H directly affects the structural formation of the hollow fibers. If H is too small, the core layer solution in the inner tube is blocked by the shell layer solution in the outer tube; in this case, the core layer solution cannot be stretched, and the shell layer solution forms a jet independently. Figure 3 As shown, when H is increased to approximately half the radius of the outer tube, a better coaxial jet can be obtained. At this point, the Taylor cone section becomes significantly longer, and the jet can be clearly observed. Figure 3The image shows the formation process of a coaxial jet captured by a high-speed camera (the core material is shown in red, and the shell material is shown in transparent). When H is further increased to be greater than the radius of the outer tube, the shell solution flows out along the outer surface of the inner tube, failing to completely encapsulate the core solution within the inner tube, thus preventing the formation of a stable, single coaxial jet. Therefore, in this invention, H is set to be equal to half the radius of the outer tube. Figure 3 It also demonstrates that the device of the present invention produces a stable and uniform coaxial jet, without splitting or droplets.

[0035] The shell solution injection pump injects the shell solution into the annular space between the inner and outer tubes. The core solution injection pump injects the core solution into the internal cavity of the inner tube. The collector is used to collect the fibers prepared by the coaxial needle, preferably a cage-type collector, for collecting the spun fibers to form a three-dimensional structure. The high-temperature calcination device removes the core material through high-temperature sintering to obtain hollow nanofibers.

[0036] The device for rapidly preparing hollow nanofibers by airflow induction of the present invention has a simple structure and a simple spinning process. Industrial production can achieve high production efficiency by spinning multiple needles simultaneously.

[0037] The specific method for preparing polyimide hollow fibers using the above-mentioned apparatus is as follows: First, shell solution A was prepared: 0.8 g of polyethylene oxide (PEO) powder was weighed using an electronic balance and added to 10 g of N,N-dimethylformamide (DMF) solution. The mixture was magnetically stirred at 60 °C for 3 hours until completely dissolved. Subsequently, 10 g of polyacrylic acid (PAA)-DMF solution (20 wt.%) was added to the previously prepared PEO solution, and the mixture was magnetically stirred at 50 °C for 6 hours until a homogeneous polyacrylic acid (PAA) precursor solution was obtained, which is shell solution A.

[0038] Preparation of core layer solution B: Dimethyl silicone oil (PMX-200, 12500 cSt) was used as the core layer material and heated to 60 °C under magnetic stirring.

[0039] Polyacrylic acid (PAA) precursor solution and dimethyl silicone oil were respectively used as shell solution and core solution and then passed into a coaxial needle while hot; the flow rate of the outer layer solution was 0.02 mL / min. -1 The internal flow rate of the solution was 0.01 mL / min. -1The airflow velocity was kept constant at 0.1 MPa. Under the shear force of the high-speed airflow, the shell-core solution converged and stretched at the needle tip to form a Taylor cone. Subsequently, the coaxial jet underwent bending and unstable motion, while the solvent evaporated. The solute eventually solidified and deposited on the collecting device to form a polyacrylic acid-dimethyl silicone oil coaxial nanofiber sponge. The collected coaxial nanofiber spinning precursor sponge was kept at 70 °C for 8 hours in a vacuum oven to evaporate all the residual DMF solution from the spinning process. Then, it was heated to 320 °C in a muffle furnace at 2.6 °C / min and held for 120 min, followed by furnace cooling. Due to the thermal imidization of polyacrylic acid (PAA) into polyimide, the dimethyl silicone oil was thermally decomposed at 320 °C into products such as silane and carbon dioxide, which evaporated. Finally, a three-dimensional structure composed of hollow polyimide nanofibers was obtained.

[0040] In the above methods, the shell-core solution propulsion rate ratio has a significant impact on the formation of hollow structures. When V in / V out When the fiber volume was 1 / 4, the morphology after calcination showed that the fiber had a porous structure and did not achieve the ideal hollow structure. The low flow rate of methyl silicone oil resulted in poor continuous filamentation performance. At this point, the methyl silicone oil was distributed in droplets within the precursor fiber, forming a beaded fiber structure. Figure 4 As shown in (a). When V in / V out When the ratio is 1 / 2, the morphology of the calcined fiber shows a distinct hollow structure. Increasing the core fluid flow rate allows the interfacial shear stress to be sufficient for the continuous distribution of methyl silicone oil within the fiber. Figure 4 As shown in (b). Further increase the flow rate ratio V in / V out When the volume is greater than 1 / 2, the PI solution cannot coat the methyl silicone oil, and no coaxial jet can be obtained at the needle tip. The methyl silicone oil drips down in droplets. Only the PI solution forms a jet.

[0041] Figure 5 The images show a sponge composed of polyimide hollow nanofibers and its ultralightness (a), low-magnification SEM images (b), high-magnification SEM images (c), and fiber diameter distribution (d). As can be seen from the figures, this invention can obtain ultralight hollow nanofiber and sponge structures, and can easily produce a large quantity of hollow nanofiber sponge structures with uniform fiber diameter and high-quality hollow structures.

[0042] Figure 6Figure (a) shows the relationship between the thermal conductivity of the polyimide hollow nanofiber sponge and the sponge density, and Figure (b) shows a comparison of the working space of the polyimide hollow nanofiber sponge and other thermal insulation sponges. As can be seen from the figures, the hollow nanofiber sponge prepared in this invention has low thermal conductivity and its density can be controlled. At the same density, its thermal conductivity is lower than that of other polymer thermal insulation sponges, demonstrating the advantages of hollow nanofibers.

[0043] Figure 7 The figures show the thermogravimetric curves (a) of polyimide hollow nanofiber sponge, polyurethane sponge, polystyrene sponge, and cork; the surface temperature versus time curves of the samples in the heat resistance comparison experiment (b); and the optical and infrared thermal imaging comparison images (c) of the heat resistance comparison experiment. The figures show that the polyimide hollow nanofiber sponge exhibits superior heat insulation performance, achieving a maximum operating temperature of 400 ℃ compared to existing finished thermal insulation materials (polystyrene sponge, polyurethane sponge, and cork).

[0044] Figure 8 This is an infrared thermal image of a polyimide hollow nanofiber sponge heated on a 400℃ hot stage for 120 minutes. The image shows that the polyimide hollow nanofiber sponge can operate at 400℃ for an extended period, exhibiting good thermal stability.

[0045] Figure 9 This is a demonstration diagram showing the compression and recovery of polyimide hollow nanofiber sponge at different temperatures. Figure 10 In the middle (a) and (b), the density is 50 mg / cm³. 3 The fatigue test curve of hollow nanofiber sponge after 1000 cycles, and the density of 80 mg / cm³ 3 The strain curve of the fiber sponge after 1000 cycles at 80% strain is shown. Figure 11 This is an optical image recovered after the hollow nanofiber sponge is bent and folded at 180°. As shown in the figure, the hollow nanofiber sponge prepared by this invention has good elasticity at both high and low temperatures (-196℃~300℃), and the hollow nanofiber sponge can withstand 1000 cycles of 80% strain compression, exhibiting good fatigue resistance.

[0046] Figure 12 Polyimide hollow nanofiber sponges of various colors were obtained by dyeing the core layer solution. Different colored polyimide hollow nanofiber sponges can be obtained by filling the core layer with solutions of different colors.

[0047] Figure 13The process involved evacuating a hollow nanofiber sponge, filling it thoroughly with argon gas, and then dropping the same sample from the same height, one filled with argon and the other with air. Because argon is lighter than air, the argon-filled sample fell much slower than the air-filled sample. This demonstrates that the polyimide hollow nanofiber sponge contains numerous entangled and complex hollow tubular structures, which can fill and adsorb gases without completely exchanging them with the air in a short time. Images from the same frame taken with a high-speed camera show that the argon-filled sample fell significantly slower than the air-filled sample. With improved encapsulation technology, this could potentially enable practical applications such as gas storage.

[0048] In summary, the preparation method of this invention is highly efficient and clean, and suitable for industrial production. The prepared hollow fibers, in addition to their basic functions of flexibility, elasticity, and thermal insulation, can also achieve diverse colors, gas storage, adsorption, and other additional functions.

[0049] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A polyimide hollow nanofiber sponge prepared by airflow induction method, characterized by, The preparation apparatus used includes a coaxial needle, a compressed air pump, a cage-type collector, a high-temperature calcination device, a shell solution injection pump, and a core solution injection pump. The coaxial needle consists of two capillary tubes with different inner diameters, coaxially fitted together. Both the inner and outer tube ends at one end of the coaxial needle are sealed. The inner tube at the other end extends beyond the outer tube as the fiber outlet. The length of the inner tube extending beyond the outer tube is H, where H is equal to half the radius of the outer tube. A section of the coaxial needle near the fiber outlet is bent at 90° to form a vertical section. An airflow channel is installed on the side of the bend, with the centerline of the airflow channel aligned with the centerline of the vertical section. The airflow channel is connected to a compressed air pump, which injects any one of the following gases: air, nitrogen, argon, or a mixture. The gas outlet of the airflow channel faces the vertical section, applying airflow to the fibers at the fiber outlet. The shell solution injection pump injects the shell solution into the annular space between the inner and outer tubes; The core layer solution injection pump injects the core layer solution into the internal cavity of the inner tube; The shell solution is prepared as follows: polyethylene oxide powder is added to DMF and stirred at 60 °C until completely dissolved; then a DMF solution of polyacrylic acid is added, and stirring is continued at 50 °C until a homogeneous polyacrylic acid precursor solution is obtained, which is the shell solution. The core layer solution is dimethyl silicone oil; The shell solution and core solution are injected separately into a coaxial needle and converge at the tip. The ratio of the injection rates of the shell solution and core solution in the coaxial needle is controlled to be 2:

1. A compressed air pump is turned on to provide airflow. Under the action of high-speed airflow, the shell solution and core solution are stretched to form a coaxial Taylor cone. Then, the coaxial jet undergoes a bending unstable motion, while the solvent evaporates and the solute finally solidifies and deposits in a cage-type collector. The collected fibers are placed in a high-temperature calcination device to remove the core material, resulting in a hollow nanofiber sponge.

2. The polyimide hollow nanofiber sponge prepared by airflow induction method according to claim 1, characterized in that, The outer shaft solution flow rate was 0.02 mL min -1 The inner shaft solution flow rate was 0.01 mL min -1 .

Citation Information

Patent Citations

  • Nano material preparation device

    CN108950701A