Polarizing plate and image display device

By designing a protective layer with high bending durability in the polarizer and optimizing resin material in the prior art, the problem of insufficient bending of the polarizer in the prior art is solved, and efficient bending performance suitable for bendable or foldable image display devices is achieved.

CN119045106APending Publication Date: 2024-11-29NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410678821.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-05-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing polarizers are not flexible enough in a bendable or foldable image display device, making it difficult to meet the needs of flexibility and bendability.

Method used

A polarizer with high bending durability was designed, and the protective layer had bending times in the MIT test to reach more than 200 times. By optimizing the resin material and laminated structure, the optical characteristics and bending performance of the polarizer were improved.

Benefits of technology

A polarizer suitable for a bendable or foldable image display device is realized, which enhances the bending durability and stability of the device, and avoids cracks and image display failures during bending.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119045106A_ABST
    Figure CN119045106A_ABST
Patent Text Reader

Abstract

The invention provides a polarizing plate which can be suitably applied to a bendable or foldable image display device, and an image display device. A polarizing plate according to an embodiment of the present invention is provided with a polarizer and a protective layer. The protective layer is disposed on at least one surface of the polarizer. The number of bends in the MIT test of the protective layer is 200 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polarizing plate and an image display device. Background Art

[0002] Image display devices represented by liquid crystal display devices and electroluminescent (EL) display devices (such as organic EL display devices and inorganic EL display devices) are rapidly becoming popular. In image display devices, a polarizing plate having a polarizer and a protective layer is typically used (see, for example, Patent Document 1).

[0003] In recent years, the use of image display devices has diversified, and research has been conducted on making image display devices more flexible and bendable. However, if the polarizing plate described in Patent Document 1 is applied to a bendable or foldable image display device, the bendability of the image display device may be insufficient.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2022-153440 Summary of the invention

[0007] Problems to be solved by the invention

[0008] The present invention has been made to solve the above-mentioned conventional problems, and a main object of the present invention is to provide a polarizing plate and an image display device that can be suitably applied to a bendable or foldable image display device.

[0009] Means for solving problems

[0010] [1] A polarizing plate according to one embodiment of the present invention comprises a polarizer and a protective layer. The protective layer is disposed on at least one side of the polarizer. The number of bending times of the protective layer in an MIT test is 200 or more.

[0011] [2] An image display device according to another aspect of the present invention includes the polarizing plate described in [1] and a flexible image display panel in this order.

[0012] [3] The image display device according to [2] above, wherein a ratio of a thickness of the protective layer to a thickness of the image display panel may be 1 to 2.

[0013] Effects of the Invention

[0014] According to the embodiments of the present invention, a polarizing plate and an image display device that can be suitably applied to a bendable or foldable image display device can be realized. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1This is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention.

[0016] Figure 2 This is a schematic cross-sectional view of a polarizing plate according to another embodiment of the present invention.

[0017] Figure 3 Yes Figure 2 Schematic cross-sectional view of an image display device including a polarizing plate.

[0018] Explanation of symbols

[0019] 1 Protective layer

[0020] 2 Polarizer

[0021] 100 Polarizer

[0022] 200 Image display device DETAILED DESCRIPTION

[0023] Hereinafter, representative embodiments of the present invention will be described, but the present invention is not limited to these embodiments. In addition, in order to make the description clearer, the accompanying drawings are sometimes schematically represented for the width, thickness, shape, etc. of each part compared with the embodiments, but it is an example and does not limit the interpretation of the present invention.

[0024] (Definition of Terms and Symbols)

[0025] The definitions of terms and symbols in this specification are as follows.

[0026] (1) Refractive index (nx, ny, nz)

[0027] “nx” is the refractive index in the direction where the refractive index in the plane is maximum (ie, the slow axis direction), “ny” is the refractive index in the direction orthogonal to the slow axis in the plane (ie, the fast axis direction), and “nz” is the refractive index in the thickness direction.

[0028] (2) In-plane phase difference (Re)

[0029] "Re(λ)" is the in-plane phase difference measured by light of wavelength λnm at 23°C. For example, "Re(550)" is the in-plane phase difference measured by light of wavelength 550nm at 23°C. When the thickness of the layer (film) is set to d(nm), Re(λ) is calculated by the formula: Re(λ) = (nx-ny)×d.

[0030] (3) Retardation in the thickness direction (Rth)

[0031] "Rth(λ)" is the phase difference in the thickness direction measured by light of wavelength λnm at 23°C. For example, "Rth(550)" is the phase difference in the thickness direction measured by light of wavelength 550nm at 23°C. When the thickness of the layer (film) is set to d(nm), Rth(λ) is calculated by the formula: Rth(λ) = (nx-nz)×d.

[0032] A. Overall composition of polarizer

[0033] Figure 1 This is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention.

[0034] like Figure 1 As shown in , the polarizing plate 100 includes a polarizer 2 and a protective layer 1. The protective layer 1 is disposed on at least one side of the polarizer 2. The protective layer 1 is typically flexible. The number of bending times in the MIT test of the protective layer 1 (hereinafter referred to as the MIT bending number) is 200 times or more. The MIT test can be measured, for example, according to JIS P 8115.

[0035] If the MIT bending number of the protective layer is 200 times or more, sufficient bending durability can be given to the polarizing plate having the protective layer and the polarizer. If it is such a polarizing plate, it can be applied to a bendable image display device (such as a liquid crystal display device, an organic EL display device, an inorganic EL display device), preferably a foldable image display device, and more preferably a foldable organic EL display device.

[0036] The MIT bending number of the protective layer 1 is preferably 500 times or more, more preferably 800 times or more, and further preferably 1000 times or more. When the MIT bending number of the protective layer is equal to or more than the above lower limit, the bending durability of the polarizing plate can be further improved.

[0037] On the other hand, the MIT bending number of the protective layer 1 is, for example, 6000 times or less, preferably 3000 times or less, and more preferably 2000 times or less.

[0038] The indentation elastic modulus of the protective layer 1 is, for example, 3.00 GPa or more, preferably 3.10 GPa or more, and more preferably 3.20 GPa or more. When the indentation elastic modulus of the protective layer is equal to or more than such a lower limit, the bending durability of the polarizing plate can be further improved.

[0039] On the other hand, the indentation elastic modulus of the protective layer 1 is, for example, 7.00 GPa or less, preferably 6.00 GPa or less, more preferably 4.00 GPa or less, and further preferably 3.50 GPa or less. If the indentation elastic modulus of the protective layer is below such an upper limit, cracking of the protective layer during bending can be suppressed. The indentation elastic modulus can be measured, for example, according to JIS Z 2255.

[0040] The elongation at break of the protective layer 1 at 25° C. is, for example, 20 mm or more, preferably 25 mm or more, and more preferably 30 mm or more. When the elongation at break of the protective layer is equal to or more than the above lower limit, the bending durability of the polarizing plate can be further improved.

[0041] On the other hand, the elongation at break of the protective layer 1 is, for example, 150 mm or less, preferably 130 mm or less, more preferably 100 mm or less, and further preferably 50 mm or less. If the elongation at break of the protective layer is below such an upper limit, deformation of the protective layer can be suppressed. The elongation at break can be measured, for example, according to JIS K 7127.

[0042] The loss tangent tanδ of the protective layer 1 at 85°C and 85%RH (relative humidity) is, for example, 15×10 -2 Below, preferably 13×10 -2 Below, more preferably 10×10 -2 Below, more preferably 7.0×10 -2 On the other hand, the lower limit of the loss tangent tanδ of the protective layer 1 at 85°C and 85%RH (relative humidity) is typically 4.0×10 -2 .

[0043] The loss tangent tanδ of the protective layer 1 at 100°C is, for example, 15×10 -2 Below, preferably 13×10 -2 Below, more preferably 10×10 -2 Below, more preferably 8.0×10 -2 Below, particularly preferably 6.0×10 -2 On the other hand, the lower limit of the loss tangent tanδ of the protective layer 1 at 100°C is typically 3.0×10 -2 Note that tan δ of the protective layer is observed, for example, by measuring dynamic viscoelasticity in a tensile mode at a measurement frequency of 5 Hz.

[0044] If the tanδ of the protective layer is above this lower limit, stress relaxation during bending can be effective, and failure modes such as cracks caused by residual stress can be improved. If the tanδ of the protective layer is below this upper limit, creases will not be generated even if it is bent multiple times, and good image display can be maintained.

[0045] The thickness of the protective layer 1 is, for example, 10 μm or more, preferably 20 μm or more. If the thickness of the protective layer is above this lower limit, excellent bending durability can be stably imparted to the polarizer. On the other hand, the thickness of the protective layer 1 is, for example, 130 μm or less, preferably 100 μm or less, more preferably 80 μm or less, further preferably 55 μm or less, particularly preferably 47 μm or less, particularly preferably 42 μm or less, and most preferably 30 μm or less. If the thickness of the protective layer is below this upper limit, excellent bending durability can be stably imparted to the polarizer, and the polarizer can be thinned.

[0046] like Figure 2 As shown in , in one embodiment, the protective layer 1 is disposed on both sides of the polarizer 2. Hereinafter, the protective layer 1 disposed on one side of the polarizer 2 is sometimes referred to as the first protective layer 1a, and the protective layer 1 disposed on the other side of the polarizer 2 is sometimes referred to as the second protective layer 1b for distinction.

[0047] Hereinafter, the components of the polarizing plate will be described in detail.

[0048] B. Polarizer

[0049] Any appropriate polarizer can be used as the polarizer 2. For example, the resin film forming the polarizer may be composed of a single-layer resin film, or may be prepared using a laminate of two or more layers.

[0050] Specific examples of polarizers composed of a single-layer resin film include polarizers obtained by dyeing and stretching hydrophilic polymer films such as polyvinyl alcohol (PVA) films, partially formalized PVA films, and partially saponified films of ethylene-vinyl acetate copolymers with dichroic substances such as iodine or dichroic dyes, and polyene-based oriented films such as dehydrated PVA films and dehydrochlorinated polyvinyl chloride films. Preferably, a polarizer obtained by dyeing a PVA film with iodine and uniaxially stretching the film is used from the perspective of excellent optical properties.

[0051] As a specific example of a polarizer obtained using a laminate, a laminate using a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a laminate using a resin substrate and a PVA-based resin layer formed by coating on the resin substrate can be cited. A polarizer obtained using a laminate using a resin substrate and a PVA-based resin layer formed by coating on the resin substrate can be made, for example, by the following method: a PVA-based resin solution is applied to a resin substrate and dried to form a PVA-based resin layer on the resin substrate, thereby obtaining a laminate of the resin substrate and the PVA-based resin layer; the laminate is stretched and dyed to make the PVA-based resin layer into a polarizer. In one embodiment of the present invention, a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is preferably formed on one side of the resin substrate. Stretching typically includes immersing the laminate in a boric acid aqueous solution for stretching. Furthermore, stretching may further include stretching the laminate in the air at a high temperature (e.g., above 95°C) before stretching in a boric acid aqueous solution as required. In addition, in one embodiment of the present invention, the laminate is preferably subjected to a drying shrinkage treatment in which the laminate shrinks by more than 2% in the width direction by heating while being conveyed in the length direction. Representatively, the manufacturing method of this embodiment includes sequentially performing an air auxiliary stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment on the laminate. By introducing auxiliary stretching, even when PVA is coated on a thermoplastic resin, it becomes possible to improve the crystallinity of PVA and achieve high optical properties. In addition, by improving the orientation of PVA in advance, when immersed in water in the subsequent dyeing process and stretching process, it is possible to prevent problems such as reduction and dissolution of the orientation of PVA, and it becomes possible to achieve high optical properties. Furthermore, when the PVA-based resin layer is immersed in a liquid, the disorder of the orientation of the polyvinyl alcohol molecules and the reduction of the orientation can be suppressed compared to the case where the PVA-based resin layer does not contain a halide. Thus, the optical properties of the polarizer obtained by the treatment process of immersing the laminate in a liquid such as a dyeing treatment and an underwater stretching treatment can be improved. Furthermore, by utilizing drying shrinkage treatment to shrink the laminate in the width direction, the optical properties can be improved. The obtained laminate of resin substrate / polarizer can be used directly (that is, the resin substrate can also be used as a protective layer of polarizer), or the resin substrate can be peeled off from the laminate of resin substrate / polarizer and any suitable protective layer corresponding to the purpose can be stacked on the peeling surface for use. The details of the manufacturing method of such a polarizer are, for example, recorded in Japanese Unexamined Patent Publication No. 2012-73580 and Japanese Patent No. 6470455. The overall records of these publications are cited in this specification as a reference.

[0052] The dyeing using iodine is performed, for example, by immersing the PVA membrane in an iodine aqueous solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching can be performed after the dyeing treatment, or it can be performed while dyeing. In addition, dyeing can also be performed after stretching. As needed, the PVA membrane is subjected to swelling treatment, cross-linking treatment, washing treatment, drying treatment, etc. For example, by immersing the PVA membrane in water for washing before dyeing, not only can the stains and anti-blocking agents on the surface of the PVA membrane be washed away, but the PVA membrane can also be swelled to prevent uneven dyeing.

[0053] The thickness of the polarizer 2 is, for example, 1 μm to 80 μm, preferably 1 μm to 15 μm, more preferably 1 μm to 12 μm, and further preferably 3 μm to 12 μm. If the thickness of the polarizer is within such a range, curling during heating can be well suppressed and good appearance durability during heating can be obtained.

[0054] The polarizer 2 typically exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The single transmittance of the polarizer 2 is, for example, 41.5% to 46.0%, preferably 43.0% to 46.0%, and more preferably 44.5% to 46.0%. The polarization degree of the polarizer 2 is preferably 97.0% or more, more preferably 99.0% or more, and further preferably 99.9% or more.

[0055] C. Protective layer

[0056] The protective layer 1 is composed of a resin film containing a resin material as a main component. As specific examples of the resin material, cycloolefin (COP) systems such as polynorbornene systems; polyester systems such as polyethylene terephthalate (PET) systems; cellulose resins such as triacetyl cellulose (TAC); polycarbonate (PC) systems; (meth) acrylic acid systems; polyvinyl alcohol systems; polyamide systems; polyimide systems; polyether sulfone systems; polysulfone systems; polystyrene systems; polyolefin systems; transparent resins such as acetate systems can be listed. In addition, thermosetting resins or ultraviolet curing resins such as (meth) acrylic acid systems, urethane systems, (meth) acrylic urethane systems, epoxy systems, and silicone systems can also be listed. It should be noted that "(meth) acrylic acid resin" refers to acrylic resins and / or methacrylic resins. In addition, glassy polymers such as siloxane polymers can also be listed, for example. In addition, polymer films described in Japanese Patent Publication No. 2001-343529 (WO01 / 37007) can also be used. As the material of the film, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group on the side chain and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group on the side chain can be used, for example, a resin composition containing an alternating copolymer formed by isobutylene and N-methylmaleimide and an acrylonitrile-styrene copolymer can be cited. The polymer film can be, for example, an extrusion molding of the above resin composition. The materials of the resin film can be used alone or in combination.

[0057] Among such resin materials, preferably, PC-based resins are used.

[0058] The PC resin is produced by reacting a dihydroxy compound containing at least a structural unit derived from a dihydroxy compound having a bonding structure represented by the following structural formula (1) and having at least one bonding structure -CH2-O- in the molecule with a carbonic acid diester in the presence of a polymerization catalyst. In other words, the PC resin contains a structural unit derived from a dihydroxy compound and a carbonate group derived from a carbonic acid diester.

[0059] [Chemical formula 1]

[0060]

[0061] Here, as the dihydroxy compound having a bonding structure represented by structural formula (1), any compound of any structure can be used as long as it has two alcoholic hydroxyl groups, contains a structure having a linking group -CH2-O- in the molecule, and can react with a carbonic acid diester in the presence of a polymerization catalyst to produce a polycarbonate, and multiple compounds can also be used in combination.

[0062] In addition, as the dihydroxy compound used in the PC-based resin, a dihydroxy compound that does not have a bonding structure represented by the above-mentioned structural formula (1) may also be used in combination. Hereinafter, a dihydroxy compound having a bonding structure represented by the structural formula (1) is sometimes abbreviated as a dihydroxy compound (A), and a dihydroxy compound that does not have a bonding structure represented by the structural formula (1) is sometimes abbreviated as a dihydroxy compound (B).

[0063] (Dihydroxy compound (A))

[0064] The "linking group -CH2-O-" in the dihydroxy compound (A) refers to a structure in which atoms other than hydrogen atoms are bonded to each other to form a molecule. In the linking group, the atom to which at least an oxygen atom can be bonded or the atom to which a carbon atom and an oxygen atom can be bonded at the same time is preferably a carbon atom. The number of "linking groups -CH2-O-" in the dihydroxy compound (A) is preferably 1 or more, and more preferably 2 to 4.

[0065] Specific examples of the dihydroxy compound (A) include 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-cyclohexylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3,5-di ...isobutylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene Compounds having an aromatic group on the side chain and an ether group bonded to the aromatic group on the main chain, such as exemplified by (4-(2-hydroxyethoxy)-3-tert-butyl-6-methylphenyl)fluorene and 9,9-bis(4-(3-hydroxy-2,2-dimethylpropoxy)phenyl)fluorene; bis[4-(2-hydroxyethoxy)phenyl]methane, bis[4-(2-hydroxyethoxy)phenyl]diphenylmethane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]ethane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]-1-phenylethane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]propane, 2,2-bis[4-(2-hydroxyethoxy)-3-methylphenyl]propane, 2,2-bis[4-(2-hydroxyethoxy)-3-methylphenyl]propane, [3,5-dimethyl-4-(2-hydroxyethoxy)phenyl]propane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]-3,3,5-trimethylcyclohexane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,4-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,3-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 2,2-bis[4-(2-hydroxyethoxy)-3-phenylphenyl]propane, 2,2-bis[(2-hydroxyethoxy)-3-isopropylphenyl]propane, 2,2-bis[3-tert-butyl-4-(2-hydroxyethoxy)phenyl]propane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]butane, 2,2-bis[3-tert-butyl-4-(2-hydroxyethoxy)phenyl]propane Bis(hydroxyalkoxyaryl)alkanes such as those exemplified by [4-(2-hydroxyethoxy)phenyl]-4-methylpentane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]octane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]decane, 2,2-bis[3-bromo-4-(2-hydroxyethoxy)phenyl]propane, and 2,2-bis[3-cyclohexyl-4-(2-hydroxyethoxy)phenyl]propane; Bis(hydroxyalkoxyaryl)cycloalkanes such as those exemplified by 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,1-bis[3-cyclohexyl-4-(2-hydroxyethoxy)phenyl]cyclohexane, and 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclopentane;Dihydroxyalkoxydiaryl ethers such as 4,4'-bis(2-hydroxyethoxy)diphenyl ether and 4,4'-bis(2-hydroxyethoxy)-3,3'-dimethyldiphenyl ether; bishydroxyalkoxyaryl sulfides such as 4,4'-bis(2-hydroxyethoxyphenyl) sulfide and 4,4'-bis[4-(2-dihydroxyethoxy)-3-methylphenyl] sulfide; bishydroxyalkoxyaryl sulfoxides such as 4,4'-bis(2-hydroxyethoxyphenyl) sulfoxide and 4,4'-bis[4-(2-dihydroxyethoxy)-3-methylphenyl] sulfoxide; 4,4'-bis(2-hydroxyethoxyphenyl) sulfone, 4,4'-bis[4-(2-dihydroxyethoxy)-3-methylphenyl] sulfoxide; Bishydroxyalkoxyaryl sulfones such as those exemplified by (2-dihydroxyethoxy)-3-methylphenyl]sulfone; Bishydroxyalkoxybenzenes such as those exemplified by 1,4-bishydroxyethoxybenzene; 1,3-bis[2-[4-(2-hydroxyethoxy)phenyl]propyl]benzene; 1,4-bis[2-[4-(2-hydroxyethoxy)phenyl]propyl]benzene; 4,4'-bis(2-hydroxyethoxy)biphenyl; 1,3-bis[4-(2-hydroxyethoxy)phenyl]-5,7-dimethyladamantane; Anhydrous sugar alcohols such as those exemplified by dihydroxy compounds represented by the following formula (2); and compounds having a cyclic ether structure such as those exemplified by spiroglycols represented by the following general formula (3). The dihydroxy compound (A) may be used alone or in combination. ;

[0066] [Chemical formula 2]

[0067]

[0068] [Chemical formula 3]

[0069]

[0070] Among these dihydroxy compounds (A), preferably, dihydroxy compounds represented by the above formula (2) can be cited. As dihydroxy compounds represented by the above formula (2), isosorbide, isomannide, and isoidide, which are stereoisomers, can be cited. They can be used alone or in combination of two or more.

[0071] Among the dihydroxy compounds (A), isosorbide obtained by dehydration condensation of sorbitol produced from various starches that are abundant and easily available as resources is most preferred from the viewpoints of availability and ease of production, optical properties, and moldability.

[0072] The proportion of the structural units derived from the dihydroxy compound (A) relative to all the structural units derived from the dihydroxy compound contained in the PC-based resin is, for example, 10 mol% or more, preferably 40 mol% or more, and more preferably 60 mol% or more. On the other hand, the proportion of the structural units derived from the dihydroxy compound (A) is, for example, 100 mol% or less, preferably 90 mol% or less, more preferably 80 mol% or less, and further preferably 70 mol% or less. If the proportion of the dihydroxy compound (A) is within the above range, the MIT bending number of the protective layer can be stably adjusted to the above range.

[0073] (Dihydroxy compound (B))

[0074] As a dihydroxy compound that becomes a structural unit of the PC-based resin, a dihydroxy compound (B) may be used together with the dihydroxy compound (A). When the dihydroxy compounds (A) and (B) are used together, the MIT bending number of the protective layer can be more stably adjusted to the above range.

[0075] The dihydroxy compound (B) is typically a dihydroxy compound other than the dihydroxy compound (A). Examples of the dihydroxy compound (B) include alicyclic dihydroxy compounds, aliphatic dihydroxy compounds, oxyalkylene glycols, aromatic dihydroxy compounds, and diols having a cyclic ether structure. The dihydroxy compound (B) may be used alone or in combination.

[0076] Among the dihydroxy compounds (B), preferably, an alicyclic dihydroxy compound is used.

[0077] The alicyclic dihydroxy compound is not particularly limited, but preferably includes a compound containing a common 5-membered ring structure or a 6-membered ring structure. In addition, the 6-membered ring structure can also be fixed in a chair shape or a boat shape by covalent bonding. When the alicyclic dihydroxy compound is a 5-membered ring or a 6-membered ring structure, the heat resistance of the obtained PC-based resin can be improved. The number of carbon atoms contained in the alicyclic dihydroxy compound is, for example, 70 or less, preferably 50 or less, and more preferably 30 or less.

[0078] Specific examples of the alicyclic dihydroxy compound containing a 5-membered ring structure or a 6-membered ring structure include alicyclic dihydroxy compounds represented by the following general formula (I) or (II).

[0079] HOCH2-R 1 -CH2OH(I)

[0080] HO-R 2 -OH(II)

[0081] (In formula (I) and (II), R 1 and R 2Each represents a cycloalkylene group having 4 to 20 carbon atoms. )

[0082] The alicyclic dihydroxy compound represented by the general formula (I), namely cyclohexanedimethanol, includes R 1 The following general formula (Ia) (wherein, R 3 represents an alkyl group having 1 to 12 carbon atoms or a hydrogen atom. ) represents various isomers. Specific examples of such compounds include 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, and 1,4-cyclohexanedimethanol.

[0083] [Chemical formula 4]

[0084]

[0085] The alicyclic dihydroxy compound represented by the general formula (I), that is, tricyclodecanedimethanol or pentacyclopentadecanedimethanol, contains R 1 Various isomers represented by the following general formula (Ib) (wherein n represents 0 or 1).

[0086] [Chemical formula 5]

[0087]

[0088] The alicyclic dihydroxy compound represented by the general formula (I), that is, decalin dimethanol or tricyclotetradecane dimethanol, contains R 1 Various isomers represented by the following general formula (Ic) (wherein m represents 0 or 1). Specific examples of such compounds include 2,6-decalinedimethanol, 1,5-decalinedimethanol, and 2,3-decalinedimethanol.

[0089] [Chemical formula 6]

[0090]

[0091] The alicyclic dihydroxy compound represented by the general formula (I), i.e., norbornane dimethanol, includes R 1 Various isomers represented by the following general formula (Id). Specific examples of such compounds include 2,3-norbornane dimethanol and 2,5-norbornane dimethanol.

[0092] [Chemical formula 7]

[0093]

[0094] The alicyclic dihydroxy compound represented by the general formula (I), namely adamantane dimethanol, includes R 1Various isomers represented by the following general formula (Ie). Specific examples of such compounds include 1,3-adamantanedimethanol.

[0095] [Chemical formula 8]

[0096]

[0097] The alicyclic dihydroxy compound represented by the general formula (II), i.e., cyclohexanediol, includes R 2 The following general formula (IIa) (wherein, R 3 represents an alkyl group having 1 to 12 carbon atoms or a hydrogen atom. ) represents various isomers. Specific examples of such compounds include 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, and 2-methyl-1,4-cyclohexanediol.

[0098] [Chemical formula 9]

[0099]

[0100] The alicyclic dihydroxy compound represented by the general formula (II), that is, tricyclodecanediol or pentacyclopentadecanediol, contains R 2 Various isomers represented by the following general formula (IIb) (wherein n represents 0 or 1).

[0101] [Chemical formula 10]

[0102]

[0103] The alicyclic dihydroxy compound represented by the general formula (II), that is, decalinediol or tricyclotetradecanediol, contains R 2 Various isomers represented by the following general formula (IIc) (wherein m represents 0 or 1). Specific examples of such compounds include 2,6-decalinediol, 1,5-decalinediol, and 2,3-decalinediol.

[0104] [Chemical formula 11]

[0105]

[0106] The alicyclic dihydroxy compound represented by the general formula (II), i.e., norbornanediol, comprises R 2 Various isomers represented by the following general formula (IId): Specific examples of such compounds include 2,3-norbornanediol and 2,5-norbornanediol.

[0107] [Chemical formula 12]

[0108]

[0109] The alicyclic dihydroxy compound represented by the general formula (II), i.e., adamantanediol, comprises R 2 Various isomers represented by the following general formula (IIe). Specific examples of such compounds include 1,3-adamantanediol.

[0110] [Chemical formula 13]

[0111]

[0112] Specific examples of the alicyclic dihydroxy compounds include preferably cyclohexanedimethanols, tricyclodecanedimethanols, adamantanediols, and pentacyclopentadecanedimethanols. From the viewpoint of easy availability and easy handling, more preferably 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,2-cyclohexanedimethanol, and tricyclodecanedimethanol. Still more preferably, tricyclodecanedimethanol is used.

[0113] The proportion of the structural units derived from the dihydroxy compound (B) relative to all the structural units derived from the dihydroxy compound contained in the PC-based resin is, for example, 0 mol% or more, preferably 10 mol% or more, more preferably 20 mol% or more, and further preferably 30 mol% or more. On the other hand, the proportion of the structural units derived from the dihydroxy compound (B) is, for example, 90 mol% or less, preferably 60 mol% or less, and more preferably 40 mol% or less.

[0114] The details of these PC-based resins are described in, for example, Japanese Patent Application Laid-Open No. 2012-31370 (Japanese Patent No. 5448264), and the description of this patent document is incorporated herein by reference.

[0115] In one embodiment, the PC-based resin comprises a structural unit derived from a dihydroxy compound (A) represented by the above formula (2), a structural unit derived from an alicyclic dihydroxy compound (B) represented by the above general formula (I), and a carbonate group connecting them. If the PC-based resin comprising these structural units is applied to a resin film, the MIT bending number of the protective layer can be further stably adjusted to the above range.

[0116] In such a PC-based resin, the molar ratio (A:B) of the structural unit derived from the dihydroxy compound (A) represented by the above formula (2) to the structural unit derived from the alicyclic dihydroxy compound (B) represented by the above general formula (I) is, for example, 5:5 to 9:1, and preferably 6:4 to 8:2.

[0117] In such a PC-based resin, the combination of the dihydroxy compound (A) represented by the above formula (2) and the alicyclic dihydroxy compound (B) represented by the above general formula (I) is preferably a combination of isosorbide and tricyclodecane dimethanol.

[0118] In addition to the above-mentioned resin material, the protective layer 1 may also contain any suitable additives. As additives, for example, antioxidants, ultraviolet absorbers, light stabilizers, nucleating agents, fillers, pigments, surfactants, and antistatic agents may be listed. On the surface of the protective layer 1 (the surface on the opposite side of the polarizer 2), any suitable surface treatment layer may also be provided. As surface treatment layers, for example, hard coatings, easy-adhesion layers, easy-slip layers, anti-adhesion layers, antistatic layers, anti-reflection layers, and oligomer prevention layers may be listed.

[0119] The protective layer 1 is typically optically isotropic. In this specification, “optically isotropic” means that the in-plane retardation Re (550) and the retardation Rth (550) in the thickness direction are within the following ranges.

[0120] The in-plane retardation Re(550) of the protective layer 1 is, for example, 10 nm or less, preferably 5 nm or less, and more preferably 3 nm or less. On the other hand, the lower limit of the in-plane retardation Re(550) of the protective layer 1 is typically 0 nm.

[0121] The retardation Rth(550) in the thickness direction of the protective layer 1 is in the range of, for example, -10 nm to +10 nm, or preferably -5 nm to +5 nm.

[0122] The total light transmittance of the protective layer 1 is, for example, 80% or more, preferably 85% or more, more preferably 90% or more, and further preferably 95% or more.

[0123] The haze value of the protective layer 1 is, for example, 2.0% or less, preferably 1.5% or less, more preferably 1.0% or less, further preferably 0.7% or less, particularly preferably 0.5% or less, and particularly preferably 0.3% or less. The lower limit of the haze value of the protective layer 1 is typically 0.05%.

[0124] If the total light transmittance and / or the haze value of the protective layer is within such a range, it is possible to suppress the protective layer from affecting the optical characteristics of the polarizer.

[0125] D. Adhesive layer (adhesive layer or adhesive layer)

[0126] Although not shown in the drawings, the protective layer 1 is typically attached to the polarizer 2 via an adhesive layer (adhesive layer or pressure-sensitive adhesive layer).

[0127] As the adhesive constituting the adhesive layer, for example, (meth) acrylic adhesives, rubber adhesives, vinyl alkyl ether adhesives, silicone adhesives, polyester adhesives, polyamide adhesives, urethane adhesives, fluorine adhesives, epoxy adhesives, and polyether adhesives can be listed. The adhesive can be used alone or in combination of two or more. Among the adhesives, preferably, a (meth) acrylic adhesive can be listed.

[0128] The thickness of the adhesive layer is typically 10 μm to 250 μm, and preferably 10 μm to 150 μm. The adhesive layer may be a single layer or may have a laminated structure.

[0129] The storage elastic modulus (G') of the adhesive layer at 25° C. is, for example, 0.01 MPa to 1.00 MPa, preferably 0.05 MPa to 0.50 MPa. If the storage elastic modulus of the adhesive layer is within such a range, a polarizing plate having very excellent bendability can be realized, and as a result, a bendable or foldable image display device (particularly an organic EL display device) can be realized.

[0130] Examples of the adhesive constituting the adhesive layer include thermosetting adhesives and active energy ray-curing adhesives, and preferably ultraviolet curing adhesives. The thickness of the adhesive layer is, for example, 0.4 μm to 3.0 μm.

[0131] Among these adhesive layers, preferably, an adhesive layer is used.

[0132] E. Image display device

[0133] In one embodiment, the polarizing plate described in the above items A to D is attached to a flexible image display panel for use.

[0134] Figure 3 Yes Figure 2 The image display device 200 of the illustrated example includes a polarizing plate 100 and a flexible image display panel 5 in this order.

[0135] The polarizing plate 100 is typically disposed on the viewing side with respect to the image display panel 5. In one embodiment, the polarizing plate 100 is attached to the image display panel 5 via any appropriate adhesive layer (adhesive layer or pressure-sensitive adhesive layer).

[0136] The flexible image display panel 5 typically includes an image display unit. As the flexible image display panel 5, for example, a liquid crystal display panel, an organic EL panel, and an inorganic EL panel can be listed, and preferably an organic EL panel can be listed. The flexible image display panel 5 is described in, for example, Japanese Patent Publication No. 2017-126061. The entire description of these publications is cited in this specification as a reference.

[0137] As the adhesive layer for bonding the polarizing plate 100 and the image display panel 5 together, preferably, the above-mentioned pressure-sensitive adhesive layer is used, and more preferably, a pressure-sensitive adhesive layer composed of an acrylic pressure-sensitive adhesive is used.

[0138] In one embodiment, the thickness of the protective layer 1 of the polarizer 100 is, for example, 0.6 to 2.2, preferably 1.0 to 2.0, relative to the thickness of the image display panel 5. When the thickness ratio of the protective layer to the image display panel is within such a range, the image display device can be stably provided with appropriate bendability.

[0139] Such an image display device 200 is bendable or foldable as described above. It should be noted that an image display device is sometimes referred to as an optical display device, an image display panel is sometimes referred to as an optical display panel, and an image display unit is sometimes referred to as an optical display unit.

[0140] Example

[0141] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to these examples. It should be noted that the measuring methods of various properties are as follows.

[0142] (1) MIT bending times of protective layer (resin film)

[0143] In the embodiments and comparative examples, the resin film to be the protective layer was subjected to the MIT test according to JIS P 8115. Specifically, the resin film was cut into pieces with a length of 15 cm and a width of 1.5 cm to serve as a test sample. The test sample was mounted on a MIT folding fatigue tester BE-202 (manufactured by TESTER SANGYO Co., Ltd.) (load 1.0 kgf, R of the clip: 0.38 mm), and repeatedly bent at a test speed of 90 cpm and a bending angle of 90°, and the number of bends when the test sample broke was taken as the test value. The results are shown in Table 1.

[0144] (2) Loss tangent tanδ of protective layer (resin film)

[0145] The loss tangent tan δ of the resin films used in Examples and Comparative Examples was measured under the following conditions using a dynamic viscoelasticity measuring apparatus (manufactured by IT KEISSUOSHI CO., LTD.).

[0146] <Measurement Conditions>

[0147] Measuring temperature: 85℃ or 100℃

[0148] Measuring humidity: 85RH% (relative humidity) *仅85℃的情况

[0149] Mode: Stretch

[0150] Frequency: 5Hz

[0151] Sample width: 5mm

[0152] Distance between chucks: 20mm

[0153] (3) Bendability of organic EL display devices

[0154] The polarizer obtained in the examples and comparative examples was used as a dummy of a flexible organic EL panel using a transparent polyimide film (manufactured by KOLON, with a thickness of 25 μm), and was attached using an acrylic adhesive (thickness of 15 μm). The ratio of the thickness of the protective layer to the thickness of the organic EL panel is shown in Table 1. Next, the obtained evaluation sample was cut into a strip of 100 mm × 20 mm with the direction of the absorption axis of the polarizer as the long side. The cut sample was fixed in a no-load U-shaped telescopic tester ("Small Desktop Durability Tester DLMD111LHA" and "U-shaped Telescopic Test Fixture" manufactured by YUASASYSTEM Machinery Co., Ltd.) in such a way that the polarizer side became the inner side of the bend, and a bending test was performed under the following conditions.

[0155] Environmental conditions: 25°C, 55% RH

[0156] Test speed: 60rpm

[0157] Bending radius: R3

[0158] Bending times: 10,000 times

[0159] Thereafter, the bendability of the organic EL display device was evaluated according to the following criteria. The results are shown in Table 1.

[0160] ○: No cracks occurred in the polarizing plate.

[0161] ×: Cracks occurred in the polarizing plate.

[0162] <<Preparation Example 1: PC-based resin film>>

[0163] Relative to 81.98 parts by mass of isosorbide (ISB), 47.19 parts by mass of tricyclodecane dimethanol (TCDDM), 175.1 parts by mass of diphenyl carbonate (DPC), and 0.979 parts by mass of 0.2% aqueous solution of cesium carbonate as a catalyst are put into a reaction vessel, and under a nitrogen atmosphere, as the first step of the reaction, the heating tank temperature is heated to 150°C, and the raw materials are dissolved (about 15 minutes) while stirring as needed. Then, the pressure is set to 13.3kPa from normal pressure, while the heating tank temperature is raised to 190°C in 1 hour, while the generated phenol is extracted out of the reaction vessel. After the reaction vessel as a whole is kept at 190°C for 15 minutes, as the second step, the pressure in the reaction vessel is set to 6.67kPa, and the heating tank temperature is raised to 230°C in 15 minutes, and the generated phenol is extracted out of the reaction vessel. Since the stirring torque of the stirrer gradually increases, the temperature is raised to 250°C in 8 minutes. In order to further remove the generated phenol, the pressure in the reaction container is made to be below 0.200 kPa. After reaching a specific stirring torque, the reaction is terminated, and the generated reactant is extruded into water to obtain pellets of PC resin. After the obtained PC resin is vacuum dried at 100°C for 12 hours, a film-making device equipped with a single screw extruder (manufactured by Toshiba Machinery Co., Ltd., roller setting temperature: 250°C), a T-die (width 1700mm, setting temperature: 250°C), a casting roll (setting temperature: 60°C) and a winder is used to prepare a PC resin film with a thickness of 25μm. The in-plane phase difference Re(550) of the PC resin film is 3.0nm.

[0164] <<Preparation Example 2: PC-based resin film>>

[0165] A PC-based resin film was produced in the same manner as in Preparation Example 1 except that the thickness was changed to 45 μm.

[0166] <<Preparation Example 3: PC-based resin film>>

[0167] A PC-based resin film was produced in the same manner as in Preparation Example 1 except that the thickness was changed to 60 μm.

[0168] [Example 1]

[0169] As the thermoplastic resin substrate, a long amorphous polyethylene terephthalate copolymer film (thickness: 100 μm) having a Tg of about 75° C. was used, and one surface of the resin substrate was subjected to a corona treatment.

[0170] 13 parts by mass of potassium iodide was added to 100 parts by mass of a PVA-based resin prepared by mixing polyvinyl alcohol (degree of polymerization 4200, degree of saponification 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name "Gohsefimer") in a ratio of 9:1, and the resulting substance was dissolved in water to prepare a PVA aqueous solution (coating solution).

[0171] The PVA aqueous solution was applied to the corona-treated surface of the resin substrate and dried at 60° C. to form a 13 μm-thick PVA-based resin layer, thereby producing a laminate.

[0172] The obtained laminate was uniaxially stretched to 2.4 times in the longitudinal direction (length direction) in an oven at 130° C. (in-air auxiliary stretching treatment).

[0173] Next, the laminate was immersed in an insolubilization bath (boric acid aqueous solution prepared by mixing 4 parts by mass of boric acid with respect to 100 parts by mass of water) at a liquid temperature of 40° C. for 30 seconds (insolubilization treatment).

[0174] Next, the film was immersed in a dyeing bath (an iodine aqueous solution prepared by mixing iodine and potassium iodide at a weight ratio of 1:7 per 100 parts by mass of water) at a liquid temperature of 30° C. for 60 seconds while adjusting the concentration so that the single body transmittance (Ts) of the polarizer finally obtained would be a desired value (dyeing treatment).

[0175] Next, the sample was immersed in a crosslinking bath (boric acid aqueous solution containing 3 parts by mass of potassium iodide and 5 parts by mass of boric acid per 100 parts by mass of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment).

[0176] Afterwards, the laminate was immersed in an aqueous boric acid solution (boric acid concentration 4 wt%, potassium iodide concentration 5 wt%) at a liquid temperature of 70°C, and was uniaxially stretched (underwater stretching treatment) in the longitudinal direction (length direction) between rollers with different peripheral speeds so that the total stretching ratio became 5.5 times.

[0177] Thereafter, the laminate was immersed in a washing bath (an aqueous solution prepared by mixing 4 parts by mass of potassium iodide with respect to 100 parts by mass of water) at a liquid temperature of 20° C. (washing treatment).

[0178] Thereafter, the sheet was brought into contact with a SUS heating roll whose surface temperature was maintained at about 75° C. while being dried in an oven maintained at about 90° C. (drying shrinkage treatment).

[0179] In this manner, a polarizer having a thickness of about 5 μm was formed on the resin substrate, thereby obtaining a laminate having a structure of resin substrate / polarizer.

[0180] The polarizer surface (the surface opposite to the resin substrate) of the obtained laminate was bonded to the PC-based resin film (first protective layer) obtained in Preparation Example 1 using an adhesive (specifically, an active energy ray-curable adhesive), and the adhesive was cured by irradiating with ultraviolet rays.

[0181] Next, the resin substrate was peeled off, and the peeled surface of the resin substrate in the polarizer was bonded to the PC-based resin film (second protective layer) obtained in Preparation Example 1 using an adhesive (specifically, an active energy ray-curable adhesive), and the adhesive was cured by irradiating with ultraviolet rays.

[0182] As described above, a polarizing plate having a structure of first protective layer / polarizer / second protective layer was obtained.

[0183] [Example 2]

[0184] A polarizing plate was obtained in the same manner as in Example 1 except that the PC-based resin film in Preparation Example 1 was changed to a COP-based resin film having a thickness of 50 μm (manufactured by ZEON CORPORATION, product number ZF16).

[0185] [Example 3]

[0186] A polarizing plate was obtained in the same manner as in Example 1 except that the PC-based resin film in Preparation Example 1 was changed to an acrylic resin film having a thickness of 25 μm (manufactured by Kaneka Corporation, product name “HTX-Z”).

[0187] [Example 4]

[0188] A polarizing plate was obtained in the same manner as in Example 1 except that the PC-based resin film in Preparation Example 1 was changed to a 40 μm-thick PET film (manufactured by Toray Industries, Inc., part number “50U48”).

[0189] [Example 5]

[0190] A polarizing plate was obtained in the same manner as in Example 1 except that the PC-based resin film of Preparation Example 1 was changed to the PC-based resin film of Preparation Example 2.

[0191] [Comparative Example 1]

[0192] A polarizing plate was obtained in the same manner as in Example 1 except that the PC-based resin film of Preparation Example 1 was changed to the PC-based resin film of Preparation Example 3.

[0193] Table 1

[0194]

[0195] [evaluate]

[0196] As shown in Table 1, it is found that when the number of bending times in the MIT test of the protective layer is 200 or more, excellent bendability can be imparted to the organic EL display device by applying a polarizing plate including the protective layer to the organic EL display device.

[0197] Industrial Applicability

[0198] The polarizing plate of the present invention can be applied to image display devices, and can be particularly suitably used in bendable or foldable organic EL display devices.

Claims

1. A polarizing plate, comprising: Polarizer, and a protective layer disposed on at least one side of the polarizer, The protective layer is bent 200 times or more in a MIT test. 2 . An image display device comprising the polarizing plate according to claim 1 and a flexible image display panel in this order.

3. The image display device according to claim 2, wherein: The ratio of the thickness of the protective layer to the thickness of the image display panel is 1-2.