Variable contact angle non-noble metal-based membrane electrode as well as preparation method and application thereof
By designing a cathode catalytic layer and a precious metal anode layer with variable contact angles in the non-precious metal base film electrode, the problem of mass transfer resistance caused by the high load of the non-precious metal oxygen reduction catalyst is solved, the performance and power density of the fuel cell are improved, and Reduced costs.
Patent Information
- Application Number
- CN202411340408.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-25
AI Technical Summary
The high loading of the non-precious metal oxygen reduction catalyst on the cathode side of the fuel cell leads to an increase in the mass transfer resistance of the gas, reducing the performance of the fuel cell. The existing hydrophobization strategy is not suitable for non-precious metal base film electrodes with a thickness much larger than the precious metal catalytic layer.
Using a variable contact angle non-precious metal base film electrode, the gas-liquid transport capability is optimized by setting three sub-layers in the cathode catalytic layer and adjusting their contact angles through ionomers of different mass, combining with the anode layer of the noble metal catalyst.
The gas-liquid transmission capacity of the membrane electrode is improved, the gas-liquid transmission resistance is reduced, the performance and power density of the fuel cell are improved, and the preparation cost is reduced.
Smart Images

Figure CN119050378A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of fuel cells, and in particular to a membrane electrode assembly with a non-precious metal catalyst layer having a variable contact angle and a preparation method thereof. Background Art
[0002] Environmental pollution and energy security issues caused by the use of traditional energy such as fossil fuels hinder the country's high-quality development. The development of clean energy has become a consensus of all mankind. Among them, hydrogen energy, as a zero-carbon energy, is an ideal energy storage medium and energy carrier. Fuel cells are the core of efficient utilization of hydrogen energy, and membrane electrodes are key components of fuel cells. The cost of catalysts in membrane electrodes accounts for about 41% of the cost of membrane electrodes, and precious metal Pt-based catalysts are often used (Journal of power source, 2018, 399: 304-313). In particular, the slow oxygen reduction reaction on the cathode side usually requires a high load of precious metal catalysts. The high cost of catalysts hinders the commercialization of proton exchange membrane fuel cells. In recent years, non-precious metal oxygen reduction catalysts have made great progress and have shown a trend of commercialization (Journal of Power Sources, 2023, 586: 233534). Therefore, the development of non-precious metal-based membrane electrodes with stable performance and lower cost is the main direction to promote the development of fuel cells.
[0003] However, due to the low intrinsic kinetic activity of non-precious metal oxygen reduction catalysts, the loading amount on the cathode side is usually higher than that of precious metal catalysts, resulting in the thickness of the non-precious metal-based catalyst layer being about 2 to 3 times thicker than that of the Pt-based catalyst layer, causing serious gas mass transfer resistance, hindering the transmission of reaction-generated water, and reducing the performance of the fuel cell. In the precious metal Pt-based cathode catalyst layer, the hydrophobic concept is often used to optimize the catalyst layer. For example, CN1167832C shows a thin layer of hydrophobic catalyst layer electrode, which is beneficial to the removal of reaction-generated water by adding polytetrafluoroethylene (PTFE), and improves the ability of the membrane electrode to resist flooding. CN106961838B shows a membrane electrode with a composite catalyst layer, in which the two catalyst layer sublayers are respectively a hydrophilic layer and a hydrophobic layer, wherein the side close to the proton exchange membrane is hydrophilic, and the hydrophobic layer uses a PTFE additive, and is tightly combined with the proton exchange membrane through the hydrophilic catalyst layer, and is not easy to fall off.
[0004] Adding a hydrophobic agent will reduce the conductivity of the cathode catalyst layer. In addition, CN1167832C mentions that the added hydrophobic agent will also increase the thickness of the catalyst layer to a certain extent. Obviously, some current hydrophobic strategies are not suitable for non-precious metal-based catalyst layers that are much thicker than precious metal catalyst layers. It is very necessary to develop a non-precious metal-based membrane electrode with excellent performance and improved gas-liquid transmission capacity. Summary of the invention
[0005] Based on the above purpose, the purpose of this application is to provide a variable contact angle non-precious metal-based membrane electrode and its preparation method and application. To this end, the first technical solution of this application discloses a variable contact angle non-precious metal-based membrane electrode, including a cathode gas diffusion layer, a cathode catalyst layer, a proton exchange membrane, an anode catalyst layer and an anode gas diffusion layer;
[0006] The cathode catalyst layer is a non-precious metal catalyst, comprising three sublayers, namely, an outer sublayer of the cathode catalyst layer, a neutron layer of the cathode catalyst layer, and an inner sublayer of the cathode catalyst layer; the outer sublayer of the cathode catalyst layer is connected to the cathode gas diffusion layer, the inner sublayer of the cathode catalyst layer is connected to the proton exchange membrane, and the neutron layer of the cathode catalyst layer is located between the outer sublayer of the cathode catalyst layer and the inner sublayer of the cathode catalyst layer; the contact angles of the three sublayers decrease successively from the outer sublayer of the cathode catalyst layer to the inner sublayer of the cathode catalyst layer.
[0007] Furthermore, the amount of non-precious metal catalyst added between the three sub-layers of the cathode catalyst layer is equal, and the change of the contact angle is adjusted by adding ionomers of different masses.
[0008] Furthermore, in terms of mass ratio, the mass ratio of the ionomer to the non-precious metal catalyst in the cathode catalyst layer sublayer is 0.8, the amount of ionomer added increases from the inner sublayer of the cathode catalyst layer to the outer sublayer of the cathode catalyst layer, and the mass ratio of two adjacent sublayers increases by 0.02 to 0.6.
[0009] Furthermore, the non-precious metal element in the non-precious metal catalyst is any one or any combination of Fe, Co, Ni, Mn, Cu, and Zn.
[0010] Furthermore, the ionomer is a proton exchange resin, including any one or any combination of long-chain perfluorosulfonic acid, short-chain perfluorosulfonic acid or long- and short-chain mixed perfluorosulfonic acid.
[0011] The second technical solution of the present application discloses a method for preparing the above-mentioned variable contact angle non-precious metal-based film electrode, comprising the following steps:
[0012] Preparation of cathode catalyst layer: non-precious metal catalyst, ionomer, deionized water and organic solvent are mixed and dispersed in ultrasonic water bath to obtain catalyst slurry of three sublayers, wherein the amount of ionomer added increases from the inner sublayer of cathode catalyst layer to the outer sublayer of cathode catalyst layer, and the mass ratio of two adjacent sublayers increases by 0.02 to 0.6.
[0013] Preparation of anode catalyst layer: mixing noble metal catalyst, ionomer, deionized water and organic solvent, and dispersing in an ultrasonic water bath to obtain catalyst slurry;
[0014] Preparation of electrodes: GDE method is used to prepare cathode gas diffusion electrode and anode gas diffusion electrode;
[0015] Preparation of membrane electrode: The cathode gas diffusion electrode, the proton exchange membrane and the anode gas diffusion electrode are combined together by hot pressing to form a variable contact angle non-precious metal-based membrane electrode.
[0016] Furthermore, when preparing the cathode gas diffusion electrode, the catalyst slurry of the outer sublayer of the cathode catalyst layer is ultrasonically sprayed on the microporous side of the gas diffusion layer, and then the catalyst slurry of the neutron layer of the cathode catalyst layer is ultrasonically sprayed on the outer sublayer of the cathode catalyst layer, and finally the catalyst slurry of the inner sublayer of the cathode catalyst layer is ultrasonically sprayed on the neutron layer of the cathode catalyst layer; when preparing the anode gas diffusion electrode, the anode catalyst slurry is ultrasonically sprayed on the microporous side of the gas diffusion layer to form the anode catalyst layer.
[0017] Furthermore, the catalyst loadings of the three sublayers in the cathode catalyst layer are equal, wherein the total non-precious metal catalyst loading is 0.5-5 mg cm -2 The loading amount of the noble metal catalyst in the anode catalyst layer is 0.05 to 0.4 mg. Pt cm -2 .
[0018] Also, a non-precious metal-based membrane electrode with a variable contact angle obtained according to the above preparation method and its application in the preparation of a fuel cell.
[0019] Beneficial effects: The present invention adopts a variable contact angle cathode catalyst layer. The ionomer content is low and the contact angle is large on the side close to the gas diffusion layer, which is conducive to the gas entering the membrane electrode for reaction and the liquid discharge; the ionomer content is high on the side close to the proton exchange membrane, and the contact angle is small while still maintaining hydrophobicity. On the one hand, it is conducive to increasing the water content of the ionomer and reducing the proton transfer resistance. On the other hand, the hydrophobicity improves the liquid transfer capacity, avoiding the decrease in mass transfer capacity of the thicker non-precious metal-based catalyst layer, thereby improving the membrane electrode performance.
[0020] The mass ratio of ionomer to catalyst used in the present invention is much larger than that in ordinary precious metal-based catalyst layers (the mass ratio of ionomer to catalyst in precious metal-based catalyst layers is usually around 0.25), and the contact angle of the formed catalyst layer has a larger range of variation, which effectively improves the water management capacity of the membrane electrode; and from the perspective of the composition of the catalyst layer, no additional hydrophobic agent is added to avoid an increase in the electron transfer impedance of the membrane electrode.
[0021] The present invention adopts a non-precious metal catalyst as a cathode oxygen reduction catalyst, has low preparation cost, simple operating conditions, and is conducive to batch production and large-scale application.
[0022] The present invention adopts the GDE method to prepare the membrane electrode, aiming to optimize the interface between the gas diffusion layer on the cathode side and the thicker non-precious metal catalyst layer, further reduce the gas-liquid transmission resistance, and improve the power density of the fuel cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] AttachedFigure 1 Schematic diagram of the variable contact angle non-precious metal-based membrane electrode structure;
[0024] Attached Figure 2 The material transfer principle diagram of the variable contact angle non-precious metal-based membrane electrode and the ordinary non-precious metal-based membrane electrode;
[0025] Attached Figure 3 This is the relationship diagram between different ionomer-to-catalyst mass ratios and the contact angle of the catalytic layer;
[0026] Attached Figure 4 This is a comparison diagram of the polarization curves of the variable contact angle non-precious metal-based membrane electrodes prepared in Examples 1, 2, and 3 and the ordinary non-precious metal-based membrane electrode in Comparative Example 4. DETAILED DESCRIPTION
[0027] The present invention is further described in detail below in conjunction with specific examples. This implementation case is implemented based on the technology of the present invention, and a detailed implementation method and specific operation process are now given to illustrate that the present invention is creative, but the protection scope of the present invention is not limited to the following examples.
[0028] The first embodiment of the present application provides a variable contact angle non-noble metal-based film electrode, such as Figure 1 As shown: it includes a cathode gas diffusion layer, a cathode catalyst layer, a proton exchange membrane, an anode catalyst layer and an anode gas diffusion layer; wherein the cathode catalyst layer is a non-precious metal catalyst, comprising three sublayers, namely a cathode catalyst layer outer sublayer, a cathode catalyst layer neutron layer, and a cathode catalyst layer inner sublayer; the cathode catalyst layer outer sublayer is connected to the cathode gas diffusion layer, the cathode catalyst layer inner sublayer is connected to the proton exchange membrane, and the cathode catalyst layer neutron layer is located between the cathode catalyst layer outer sublayer and the cathode catalyst layer inner sublayer; wherein the contact angles of the three sublayers decrease successively from the cathode catalyst layer outer sublayer to the cathode catalyst layer inner sublayer.
[0029] In this embodiment, the amount of non-precious metal catalyst added between the three sub-layers of the cathode catalyst layer is equal, and the change of the contact angle is adjusted by adding ionomers of different masses. It should be noted that in the prior art, the addition of ionomers in the catalyst layer is generally used to adhere the catalyst, form a highly active triple phase point, and play a role in proton conduction. In the embodiment, the addition of ionomers also plays a role in adjusting the contact angle of the catalyst layer, achieving the purpose of a variable contact angle cathode catalyst layer.
[0030] In a further embodiment, in order to achieve the purpose of a non-precious metal-based film with a variable contact angle, the three sub-layers can adjust the variable contact angle by adjusting the mass ratio of the ionomer to the non-precious metal catalyst when the non-precious metal catalyst content is constant. Figure 1As shown in the figure, the mass ratio of ionomer to non-precious metal catalyst increases from the inner sublayer of the cathode catalyst layer to the outer sublayer of the cathode catalyst layer, and the mass ratio of the middle sublayer of the cathode catalyst layer is 0.8. Among them, the mass ratio of the inner sublayer of the cathode catalyst layer is the highest, that is, the ionomer content is the highest, and its catalyst layer contact angle is the smallest. The ionomer content gradually decreases from the inner sublayer of the cathode catalyst layer to the outer sublayer of the cathode catalyst layer. The difference in the mass ratio of two adjacent sublayers is 0.02 to 0.6, that is, the outermost catalyst layer has the lowest ionomer content and the largest contact angle.
[0031] It should be noted that in the inner sublayer of the cathode catalyst layer, even if the contact angle of the catalyst layer is the smallest, it is still necessary to control its contact angle to be greater than 90°, and it is still hydrophobic. Therefore, the mass ratio of the ionomer to the non-precious metal catalyst needs to be controlled within the range of 0.2 to 1.4. Figure 2 Shown: From Figure 2 It can be seen that in the variable contact angle membrane electrode, the contact angle gradually increases from the inner sublayer to the outer sublayer, generating a driving force for outward drainage. Water is transported from the inner sublayer to the gas diffusion layer, and liquid water is smoothly discharged from the membrane electrode, which is conducive to the continuous entry of the reaction gas into the catalyst layer for reaction, avoiding flooding and other causes that lead to degradation of the membrane electrode performance; in ordinary membrane electrodes, compared with variable contact angle membrane electrodes, there is no additional drainage driving force provided by the change in contact angle, and the thickness of the non-precious metal catalyst layer is thicker, so water is more easily accumulated in the non-precious metal catalyst layer, affecting the reaction gas entering the catalyst layer for reaction, resulting in reduced membrane electrode performance and causing reverse polarity of the fuel cell stack.
[0032] It should be noted that the cathode catalyst layer also includes an organic solvent and deionized water, and their basic functions and addition methods are consistent with the prior art. This embodiment is not particularly described. Preferably, the mass ratio of the organic solvent to the catalyst is 150-800, but it can be understood that the catalyst loadings of the three sublayers in the cathode catalyst layer are equal, and the addition amounts of the organic solvent and deionized water are also equal. The contact angle is changed only by changing the addition amount of the ionomer, wherein the total non-precious metal catalyst loading is 0.5-5 mg cm -2 .
[0033] In a further embodiment, the non-precious metal element in the non-precious metal catalyst is any one or any combination of Fe, Co, Ni, Mn, Cu, and Zn. Wherein, the carrier of the non-precious metal catalyst is carbon nanotubes, graphene, porous carbon, carbon black, etc., and the dispersed form of the metal element is single atom, diatomic, cluster, nanoparticle, etc. The ionomer is a proton exchange resin, including any one or any combination of long-chain perfluorosulfonic acid, short-chain perfluorosulfonic acid, or long- and short-chain mixed perfluorosulfonic acid, such as Nafion, Aquivion, 3M PFSA, etc.
[0034] It should be noted that, in this embodiment, the cathode gas diffusion layer, proton exchange membrane, anode catalyst layer and anode gas diffusion layer are commonly known in the art, and this application does not specifically explain them, and only provides a preferred embodiment.
[0035] In some preferred embodiments, the proton exchange membrane is a commercial proton exchange membrane such as Nafion 211, Nafion 212, NC 700, Gore M765.08, Gore M788.12, Gore M820.15, Gore M735.18, etc.
[0036] In some preferred embodiments, the anode catalyst layer includes a precious metal catalyst, deionized water, an organic solvent and an ionomer. The metal combination of the catalyst in the precious metal catalyst includes one or any combination of Pt, PtRu, PtPd, PtPb, PtFe, PtCo, PtNi, PtMn, PtCu, etc. The precious metal catalyst can use a catalyst carrier such as carbon nanotubes, graphene, porous carbon, carbon black, etc. The dispersed form of the metal element includes but is not limited to single atoms, diatoms, clusters, nanoparticles, etc. The mass ratio of Pt in the precious metal catalyst is 0% to 70%. The loading amount of the precious metal catalyst in the anode catalyst layer is 0.05 to 0.4 mg Pt cm -2 ; The mass ratio of organic solvent to catalyst in the anode catalyst slurry is 50 to 300.
[0037] The organic solvent in the catalyst slurry of the cathode and the anode mainly plays a dispersing role, and includes one or any combination of n-propanol, isopropanol, n-butanol, ethanol, and propylene glycol.
[0038] The second embodiment of the present application provides a second technical solution of the present application, which discloses a method for preparing the above-mentioned variable contact angle non-noble metal-based film electrode, comprising the following steps:
[0039] Preparation of cathode catalyst layer: non-precious metal catalyst, ionomer, deionized water and organic solvent are mixed and dispersed in ultrasonic water bath to obtain catalyst slurry of three sublayers, wherein the amount of ionomer added increases from the inner sublayer of cathode catalyst layer to the outer sublayer of cathode catalyst layer, and the mass ratio of two adjacent sublayers increases by 0.02 to 0.6.
[0040] Preparation of anode catalyst layer: mixing noble metal catalyst, ionomer, deionized water and organic solvent, and dispersing in an ultrasonic water bath to obtain catalyst slurry;
[0041] Preparation of electrodes: GDE method is used to prepare cathode gas diffusion electrode and anode gas diffusion electrode;
[0042] Preparation of membrane electrode: The cathode gas diffusion electrode, the proton exchange membrane and the anode gas diffusion electrode are combined together by hot pressing to form a variable contact angle non-precious metal-based membrane electrode.
[0043] In this embodiment, after the components of the catalyst slurry are mixed according to the mass ratio, they need to be placed in an ultrasonic water bath at a temperature of 0 to 10° C. for dispersion, and the dispersion time is 0.5 h to 10 h.
[0044] In this embodiment, the membrane electrode components are assembled by hot pressing, the temperature range of the hot pressing operation is 90-140° C., the set pressure of the hot pressing operation is 50-1200 psi, and the set time of the hot pressing operation is 1-10 min.
[0045] In a further embodiment, when preparing the cathode gas diffusion electrode, the catalyst slurry of the outer sublayer of the cathode catalyst layer is ultrasonically sprayed on the microporous side of the gas diffusion layer, and then the catalyst slurry of the neutron layer of the cathode catalyst layer is ultrasonically sprayed on the outer sublayer of the cathode catalyst layer, and finally the catalyst slurry of the inner sublayer of the cathode catalyst layer is ultrasonically sprayed on the neutron layer of the cathode catalyst layer; when preparing the anode gas diffusion electrode, the anode catalyst slurry is ultrasonically sprayed on the microporous side of the gas diffusion layer to form the anode catalyst layer. The ultrasonic power in the ultrasonic spraying is 0.5 to 3.5 W, and the spraying liquid flow rate is 0.02 to 2 mL min -1 , the operating temperature is 25 ~ 80 ℃.
[0046] In a further embodiment, the catalyst loadings of the three sub-layers in the cathode catalyst layer are equal, wherein the total non-precious metal catalyst loading is 0.5-5 mg cm -2 The loading amount of the noble metal catalyst in the anode catalyst layer is 0.05 to 0.4 mg. Pt cm -2 .
[0047] The third embodiment of the present application discloses a non-precious metal-based membrane electrode with a variable contact angle obtained according to the above preparation method and its application in the preparation of a fuel cell.
[0048] In this embodiment, by using a variable contact angle cathode catalyst layer, the ionomer content is low and the contact angle is large on the side close to the gas diffusion layer, which is conducive to the gas entering the membrane electrode for reaction and liquid discharge; the ionomer content is high on the side close to the proton exchange membrane, and the contact angle is small while still maintaining hydrophobicity, which is conducive to increasing the water content of the ionomer and reducing the proton transmission resistance on the one hand, and on the other hand, the hydrophobicity improves the liquid transmission capacity and avoids the decrease in the mass transfer capacity of the thicker non-precious metal-based catalyst layer, thereby optimizing the interface between the cathode side gas diffusion layer and the thicker non-precious metal catalyst layer, further reducing the gas-liquid transmission resistance and improving the membrane electrode performance. Therefore, using this membrane electrode to prepare a fuel cell can effectively improve the power density of the fuel cell.
[0049] In order to make the content of the present invention easier to understand, specific examples are provided below for further explanation. It should be noted that the examples are only for illustration and cannot be interpreted as limiting the present invention in any way.
[0050] Example 1 Preparation of non-precious metal-based membrane electrodes with variable contact angles
[0051] 1. Prepare the catalyst slurry for the anode catalyst layer: take 6 mg of 60% Pt / C catalyst, add 260 μL of deionized water to wet the catalyst, then add 560 μL of isopropanol, add Nafion-D521 so that the ionomer accounts for 25% of the dry weight of the slurry, put it in a water bath and ultrasonicate for 0.5 h to make the ionomer evenly adhere to the catalyst particles, then add 1159 μL of isopropanol, continue to ultrasonicate in the water bath for 3 h to obtain the catalyst slurry for the anode catalyst layer.
[0052] 2. Prepare the anode electrode: Use a 1.8W ultrasonic nozzle to spray the anode catalyst slurry on a 5cm 2 The microporous side of the square commercial gas diffusion layer enables the anode Pt loading to be 0.3 mg cm -2 .
[0053] 3. Prepare the catalyst slurry of the cathode catalyst layer: take 10 mg of non-precious metal-based FeSNC catalyst, add 650 μL of deionized water to wet the catalyst, then add 935 μL of isopropanol, and add Nafion-D521 ionomer, wherein the mass ratio of ionomer to catalyst in the outer sublayer of the cathode catalyst layer is 0.7 (7 mg), the mass ratio of ionomer to catalyst in the middle sublayer of the cathode catalyst layer is 0.8 (8 mg), and the mass ratio of ionomer to catalyst in the inner sublayer of the cathode catalyst layer is 0.9 (9 mg); that is, the difference in the mass ratio of ionomer to catalyst in adjacent sublayers of the catalyst layer is 0.1. The mass of the ionomer is determined according to the mass ratio of ionomer to catalyst in each sublayer, and the catalyst slurry is placed in a water bath for ultrasonic treatment for 0.5 h to make the ionomer evenly adhere to the catalyst particles, and then 1832 μL of isopropanol is added, and ultrasonic treatment is continued in the water bath for 3 h.
[0054] 4. Preparation of cathode electrode: Use a 1.8W ultrasonic nozzle to spray the catalyst slurry of the outer layer of the cathode catalyst layer on a 5cm 2 The microporous side of the square commercial gas diffusion layer makes the catalyst loading of the outer layer of the cathode catalyst layer 1 mg cm -2 ; Then, the catalyst slurry of the cathode catalyst layer middle layer was sprayed on the cathode catalyst layer outer layer, so that the catalyst loading of the cathode catalyst layer middle layer was 1 mg cm -2 Finally, the catalyst slurry of the inner sublayer of the cathode catalyst layer was sprayed on the middle sublayer of the cathode catalyst layer, so that the catalyst loading of the inner sublayer of the cathode catalyst layer was 1 mg cm -2 .
[0055] 5. Preparation of membrane electrode: The cathode electrode and the anode electrode are symmetrically placed on both sides of the commercial proton exchange membrane N211 with the catalytic layer as the opposite surface, and the membrane electrode is obtained after hot pressing at a temperature of 125°C, a pressure of 500 psi, and a time of 5 minutes.
[0056] Example 2 Preparation of non-precious metal-based membrane electrodes with variable contact angles
[0057] The preparation method is the same as that in Example 1, except that the amount of ionomer added in step 3 of Example 2 is such that the mass ratio of ionomer to catalyst in the outer sublayer of the cathode catalyst layer is 0.65 (6.5 mg), the mass ratio of ionomer to catalyst in the middle sublayer of the cathode catalyst layer is 0.8 (8 mg), and the mass ratio of ionomer to catalyst in the inner sublayer of the cathode catalyst layer is 0.95 (9.5 mg); that is, the difference in the mass ratio of ionomer to catalyst in adjacent catalyst layer sublayers is 0.15.
[0058] Example 3 Preparation of non-precious metal-based membrane electrodes with variable contact angles
[0059] The preparation method is the same as that of Example 1, except that the amount of ionomer added in step 3 of Example 3 is such that the mass ratio of ionomer to catalyst in the outer sublayer of the cathode catalyst layer is 0.6 (6 mg), the mass ratio of ionomer to catalyst in the middle sublayer of the cathode catalyst layer is 0.8 (8 mg), and the mass ratio of ionomer to catalyst in the inner sublayer of the cathode catalyst layer is 1.0 (10 mg);
[0060] That is, the difference in the mass ratio of ionomer to catalyst in adjacent catalytic layer sublayers is 0.2.
[0061] Comparative Example 1 Preparation of non-precious metal-based membrane electrode
[0062] The preparation method is the same as that in Example 1, except that the amount of ionomer added in step 3 of comparative example 1 is such that the mass ratio of ionomer to catalyst in the outer sublayer of the cathode catalyst layer, the middle sublayer of the cathode catalyst layer, and the inner sublayer of the cathode catalyst layer is 0.8 (8 mg), that is, the ionomer gradient of comparative example 1 is 0, which is a cathode catalyst layer with a uniform Nafion content.
[0063] The cathode catalyst layer in the membrane electrode of the above-mentioned Example 1, Example 2, and Example 3 has an ionomer gradient, wherein the mass ratio of ionomer to catalyst in the outer sublayer of the cathode catalyst layer, the middle sublayer of the cathode catalyst layer, and the inner sublayer of the cathode catalyst layer are respectively: Example 1 (0.7 / 0.8 / 0.9), Example 2 (0.65 / 0.8 / 0.95), and Example 3 (0.6 / 0.8 / 1.0), and the contact angle gradually decreases in the catalyst layer. In the comparative example 1, there is no ionomer gradient in the cathode catalyst layer, the mass ratio of ionomer to catalyst is 0.8, and the contact angle does not change in the catalyst layer. The catalyst mass on the cathode side of the comparative membrane electrode and the membrane electrode of the example is consistent, both of which are 3 mg cm -2 .
[0064] Test Example 1 Proton Exchange Membrane Fuel Cell Test
[0065] The membrane electrodes prepared in Examples 1-3 and Comparative Example 1 were tested for proton exchange membrane fuel cells. The test conditions were: the anode gas was hydrogen, and the flow rate was 0.3 L min -1 ; The cathode gas is oxygen, and the flow rate is 0.4L min -1 ; Battery temperature 80°C, fully humidified; back pressure 1 bar; battery fixture active area 5 cm 2 .
[0066] The test results are as follows Figure 3-4 shown. Figure 3 The contact angle of the catalytic layer with different mass ratios of ionomer to catalyst is shown. When the mass ratio is 0.6, the contact angle is 138.60±0.65°. When the mass ratio increases, the contact angle decreases. For example, when the mass ratio is 1.4, the contact angle is 95.10±1.45°, which is reduced by about 43.5°. The contact angle of the catalytic layer can be significantly adjusted.
[0067] Depend on Figure 4 It can be seen that the peak power densities of Example 1, Example 2, Example 3 and Comparative Example 1 are 925 mWcm -2 、950mW cm -2 、886mW cm -2 and 846 mW cm -2, that is, the peak power density of the embodiment is higher than that of the comparative example 1, indicating that the use of a variable contact angle ionomer catalyst layer on the cathode side can significantly improve the performance of the membrane electrode; when the mass ratio of the ionomer to the catalyst of each sub-layer differs by 0.15, the power density of the membrane electrode of embodiment 2 is the highest, which is 12.29% higher than that of the membrane electrode of comparative example 1. The limiting current densities of embodiment 1, embodiment 2, embodiment 3 and comparative example 1 are 4265 mA cm -2 、4603mAcm -2 、4031mAcm -2 and 3942mAcm -2 That is, the limiting current density of the embodiments is higher than that of the comparative example 1, indicating that the use of a variable contact angle catalytic layer on the cathode side can significantly improve the operating current density range of the membrane electrode, which means that the ability of the membrane electrode to discharge liquid water at a high current density is enhanced, thereby improving the gas-liquid transmission capacity of the membrane electrode.
[0068] Finally, it should be noted that the above implementation cases are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred implementation cases, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A variable contact angle non-precious metal-based film electrode, characterized in that: It includes a cathode gas diffusion layer, a cathode catalyst layer, a proton exchange membrane, an anode catalyst layer and an anode gas diffusion layer; The cathode catalyst layer is a non-precious metal catalyst, comprising three sublayers, namely, an outer sublayer of the cathode catalyst layer, a neutron layer of the cathode catalyst layer, and an inner sublayer of the cathode catalyst layer; the outer sublayer of the cathode catalyst layer is connected to the cathode gas diffusion layer, the inner sublayer of the cathode catalyst layer is connected to the proton exchange membrane, and the neutron layer of the cathode catalyst layer is located between the outer sublayer of the cathode catalyst layer and the inner sublayer of the cathode catalyst layer; the contact angles of the three sublayers decrease successively from the outer sublayer of the cathode catalyst layer to the inner sublayer of the cathode catalyst layer.
2. The variable contact angle non-noble metal-based film electrode according to claim 1, characterized in that: The addition amount of the non-precious metal catalyst is equal between the three sub-layers of the cathode catalyst layer, and the change of the contact angle is adjusted by adding ionomers of different masses.
3. The variable contact angle non-noble metal-based film electrode according to claim 2, characterized in that: In terms of mass ratio, the mass ratio of ionomer to non-precious metal catalyst in the cathode catalyst layer is 0.8, and the amount of ionomer added increases from the inner sublayer to the outer sublayer of the cathode catalyst layer, and the mass ratio of two adjacent sublayers increases by 0.02 to 0.
6.
4. The variable contact angle non-noble metal-based film electrode according to claim 2, characterized in that: The non-precious metal element in the non-precious metal catalyst is any one or any combination of Fe, Co, Ni, Mn, Cu and Zn.
5. The variable contact angle non-noble metal-based film electrode according to claim 2, characterized in that: The ionomer is a proton exchange resin, including any one or any combination of long-chain perfluorosulfonic acid, short-chain perfluorosulfonic acid or long- and short-chain mixed perfluorosulfonic acid.
6. The method for preparing a non-precious metal-based film electrode with a variable contact angle according to any one of claims 1 to 5, characterized in that: The steps include: Preparation of cathode catalyst layer: non-precious metal catalyst, ionomer, deionized water and organic solvent are mixed and dispersed in ultrasonic water bath to obtain catalyst slurry of three sublayers, wherein the amount of ionomer added increases from the inner sublayer of cathode catalyst layer to the outer sublayer of cathode catalyst layer, and the mass ratio of two adjacent sublayers increases by 0.02 to 0.
6. Preparation of anode catalyst layer: mixing noble metal catalyst, ionomer, deionized water and organic solvent, and dispersing in an ultrasonic water bath to obtain catalyst slurry; Preparation of electrodes: GDE method is used to prepare cathode gas diffusion electrode and anode gas diffusion electrode; Preparation of membrane electrode: The cathode gas diffusion electrode, the proton exchange membrane and the anode gas diffusion electrode are combined together by hot pressing to form a variable contact angle non-precious metal-based membrane electrode.
7. The preparation method according to claim 6, characterized in that: When preparing a cathode gas diffusion electrode, the catalyst slurry of the outer sublayer of the cathode catalyst layer is ultrasonically sprayed on the microporous side of the gas diffusion layer, and then the catalyst slurry of the neutron layer of the cathode catalyst layer is ultrasonically sprayed on the outer sublayer of the cathode catalyst layer, and finally the catalyst slurry of the inner sublayer of the cathode catalyst layer is ultrasonically sprayed on the neutron layer of the cathode catalyst layer; when preparing an anode gas diffusion electrode, the anode catalyst slurry is ultrasonically sprayed on the microporous side of the gas diffusion layer to form an anode catalyst layer.
8. The preparation method according to claim 4, characterized in that: The catalyst loadings of the three sublayers in the cathode catalyst layer are equal, wherein the total non-precious metal catalyst loading is 0.5-5 mg cm -2 The loading amount of the noble metal catalyst in the anode catalyst layer is 0.05 to 0.4 mg. Pt cm -2 .
9. A non-precious metal-based film electrode with a variable contact angle obtained according to any one of the preparation methods described in claims 6-8.
10. Use of the variable contact angle non-noble metal-based membrane electrode according to any one of claims 1 to 5 and claim 9 in the preparation of a fuel cell.
Citation Information
Patent Citations
Fuel cell membrane electrode and preparation method thereof
CN112838251A
Preparation method and application of membrane electrode for improving water management of cathode catalyst layer of proton exchange membrane fuel cell
CN114420955A
Membrane electrode containing gradient cathode catalyst layer and preparation method and application thereof
CN115133043A
High-temperature proton exchange membrane fuel cell membrane electrode with hydrophobic binder gradient cathode catalyst layer and preparation method of high-temperature proton exchange membrane fuel cell membrane electrode
CN116111152A
Fuel cell membrane electrode with gradient structure and preparation method thereof
CN116364947A
Cited By
Method for constructing interface of high-performance ionic membrane and catalyst layer
CN120565744A