Activated carbon fiber impregnation modification method and activated carbon fiber impregnation modification device
Through the vacuum flash explosion principle, high-pressure impregnated steam is inserted into the micropores of activated carbon fiber, solving the problem that the modified substances cannot be filled in the impregnation modification of activated carbon fiber, improving the adsorption efficiency and firmness, suitable for air purification in nuclear power plants, and improving the purification efficiency and reliability.
Patent Information
- Application Number
- CN202411084343.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-12-03
AI Technical Summary
The existing activated carbon fiber impregnation methods cannot effectively fill the modified substances into the activated carbon fibers, resulting in easy desorption after adsorption, and the purpose of long-term retention of radioactive substances is not high, and the purification efficiency is not high, and it is easily affected by humidity.
The high-pressure impregnated steam is transported to the micropores of activated carbon fibers by using the vacuum flash explosion principle. By heating the gasified impregnated material in the first sealing chamber and forming a negative pressure in the second sealing chamber, the impregnated material is protected by inert gas to increase the impregnation amount and Adsorption efficiency.
The adsorption efficiency and firm adsorption of activated carbon fibers on radioactive substances are improved, and the modified activated carbon fibers meet the technical requirements of air purification in nuclear power plants are improved, and the purification efficiency and reliability are improved.
Smart Images

Figure CN119056427A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nuclear power plant air purification, in particular to an activated carbon fiber impregnation modification method and an activated carbon fiber impregnation modification device. Background Art
[0002] Nuclear power plants currently use iodine adsorbers based on granular coconut shells or coal-based activated carbon to purify nuclear air. Their disadvantages are: ① low purification efficiency; ② easily affected by water vapor humidity. When the humidity exceeds 80%, the purification effect drops significantly; ③ heavy weight, inconvenient to carry and install, which can easily cause purification tests to fail due to installation.
[0003] Activated carbon fiber is an activated carbon fiber that is activated by high temperature carbonization. Its surface produces nanometer-scale pores, which increases the specific surface area and changes its adsorption characteristics. Activated carbon fiber is the third generation product after powdered activated carbon and granular activated carbon. It has a large specific surface area (1000-3000m 2 / g) and abundant micropores, with the volume of micropores accounting for more than 90% of the total pore volume. Activated carbon fiber has a larger adsorption capacity and faster adsorption kinetics than granular activated carbon. It has high adsorption efficiency for organic matter and anions and cations in liquid and gas phases. It is also resistant to acid and alkali, high temperature and humidity, has strong adaptability, good conductivity and chemical stability, and is an ideal environmentally friendly purification material. However, if the activated carbon fiber produced in the factory is directly used for radioactive purification in nuclear power plants, there will be a problem of easy desorption after adsorption, that is, it cannot achieve the purpose of long-term adsorption and retention of radioactive substances. Therefore, it is necessary to impregnate and modify the activated carbon fiber, and fill the modified substance with good complexing properties for radioactive substances into the activated carbon fiber.
[0004] The existing method for impregnating granular activated carbon is to dissolve the modified substance into water to form an aqueous solution of a certain concentration, and then spray it into the activated carbon. This method cannot achieve the goal of impregnating activated carbon fibers due to the difference in the pore structure of activated carbon fibers and granular activated carbon. If the existing method is applied to activated carbon fibers, the impregnated material can only stay on the surface of the activated carbon fibers, and the impregnation amount does not meet the requirements. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide an improved activated carbon fiber impregnation modification method and activated carbon fiber impregnation modification device.
[0006] The technical solution adopted by the present invention to solve the technical problem is: to provide an activated carbon fiber impregnation modification method, comprising the following steps:
[0007] S1, placing the impregnated material in a first sealed chamber, heating and gasifying the impregnated material to form high-pressure impregnation steam;
[0008] S2, placing the activated carbon fiber in a second sealed chamber, and evacuating the second sealed chamber to form a negative pressure;
[0009] S3, conveying high-pressure impregnation steam into the second sealed chamber; in the second sealed chamber, the high-pressure impregnation steam enters into the micropores of the activated carbon fiber.
[0010] In some embodiments, the impregnant is triethylenediamine or hexamethylenetetramine.
[0011] In some embodiments, in step S1, the first sealed chamber is heated to 200°C±30°C, and the pressure reaches 1.6 bar to 2 bar.
[0012] In some embodiments, in step S2, after the second sealed chamber is evacuated, the pressure is ≤-0.99 bar.
[0013] In some embodiments, step S1 further includes: purging the first sealed chamber with an inert gas so that the impregnated object is placed in an inert gas atmosphere.
[0014] In some embodiments, in step S3, the inert gas is mixed with the high-pressure impregnation steam and enters the second sealed chamber together.
[0015] The present invention also provides an activated carbon fiber impregnation modification device, comprising a first sealed chamber for placing an impregnated object, a second sealed chamber for placing activated carbon fibers, a vacuum unit, a heating unit, and a connecting pipeline;
[0016] The heating unit is disposed in the first sealed chamber to heat the first sealed chamber so as to heat and vaporize the impregnated material in the first sealed chamber;
[0017] The vacuum unit is connected to the second sealed chamber to vacuum the second sealed chamber;
[0018] The connecting pipeline is connected between the first sealed chamber and the second sealed chamber, and is used to transport the heated and vaporized impregnated material into the second sealed chamber.
[0019] In some embodiments, the vacuum unit comprises a vacuum pump.
[0020] In some embodiments, the connecting pipeline includes a connecting pipe and a valve arranged on the connecting pipe.
[0021] In some embodiments, the activated carbon fiber impregnation and modification device further comprises an inert gas source, wherein the inert gas source is connected to the first sealed chamber and is used to fill the first sealed chamber with inert gas.
[0022] The beneficial effects of the present invention are as follows: the impregnation material is introduced into the micropores of activated carbon fibers in the form of gaseous molecules by utilizing the vacuum flash explosion principle, the activated carbon fibers are impregnated and modified, the adsorption efficiency of the activated carbon fibers for radioactive substances is improved and the firmness of the adsorption is increased, and the modified activated carbon fibers can meet the technical requirements for purifying radioactivity.
[0023] The impregnated and modified activated carbon fiber of the present invention is suitable for the field of air purification in nuclear power plants, and can replace traditional granular activated carbon, thereby bringing benefits of cost-effectiveness, reliability and safety level improvement to nuclear power plants. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The present invention will be further described below with reference to the accompanying drawings and embodiments, in which:
[0025] Figure 1 It is a schematic structural diagram of an activated carbon fiber impregnation and modification device according to an embodiment of the present invention. DETAILED DESCRIPTION
[0026] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described in detail with reference to the accompanying drawings.
[0027] The activated carbon fiber impregnation modification device of the present invention is used for impregnation modification of activated carbon fibers.
[0028] like Figure 1 As shown, an activated carbon fiber impregnation modification device according to an embodiment of the present invention may include a first sealed chamber 10 , a second sealed chamber 20 , a heating unit 30 , a vacuum unit 40 and a connecting pipeline 50 .
[0029] The first sealed chamber 10 is used to place the impregnation material 100, and the second sealed chamber 20 is used to place the activated carbon fiber 200 to be impregnated and modified. The heating unit 30 is arranged in the first sealed chamber 10, and is used to heat the first sealed chamber 10 so that the impregnation material 100 in the first sealed chamber 10 is heated and gasified. The vacuum unit 40 is connected to the second sealed chamber 20, and is used to vacuum the second sealed chamber 20 so that a negative pressure is formed inside the second sealed chamber 20. The connecting pipe 50 is connected between the first sealed chamber 10 and the second sealed chamber 20, and is used to pass the heated and gasified impregnation material 100 into the second sealed chamber 20, so as to enter the micropores of the activated carbon fiber 200 in the second sealed chamber 20.
[0030] The impregnant 100 may be, but is not limited to, triethylenediamine or hexamethylenetetramine.
[0031] Specifically. The first sealed chamber 10 can be formed by a sealed can, the top cover of which can be opened and closed, so as to facilitate the placement and removal of the impregnated object 100. The heating unit 30 may include a heating platform or a heater, which is supported below the first sealed chamber 10 to heat the first sealed chamber 10 to a predetermined temperature. Alternatively, the heating unit 30 may also be arranged on the periphery of the first sealed chamber 10, and may specifically include a heating element (such as a heating tube, etc.), which generates heat after being powered on, and heats the first sealed chamber 10 to a predetermined temperature. Alternatively, the heating unit 30 includes a plurality of heating elements, which may be arranged in the side wall of the first sealed chamber 10.
[0032] Furthermore, a first pressure gauge 11 and a first temperature measuring unit 12 may be provided on the first sealed chamber 10. The first pressure gauge 11 is used to detect the internal pressure of the first sealed chamber 10, and the first temperature measuring unit 12 is used to detect the temperature in the first sealed chamber 10. The first temperature measuring unit 12 includes but is not limited to a thermometer or a thermocouple.
[0033] The second sealed chamber 20 may be formed by a sealed can, the top cover of which may be opened and closed, so as to facilitate the taking and placing of the activated carbon fiber 200. The vacuum unit 40 may include a vacuum pump 41 and a vacuum pipe 42, the vacuum pump 41 being connected to the second sealed chamber 20 via the vacuum pipe 42, and vacuuming the second sealed chamber 20 so that the interior of the second sealed chamber 20 reaches the required vacuum degree or negative pressure requirement.
[0034] A second pressure gauge 21 may also be provided on the second sealed chamber 20 to detect the internal pressure of the second sealed chamber 20 .
[0035] The connecting pipeline 50 may specifically include a connecting pipeline 51 and a valve 52 disposed on the connecting pipeline 51. The connecting pipeline 51 is connected between the first sealed chamber 10 and the second sealed chamber 20, and is communicated with the first sealed chamber 10 and the second sealed chamber 20. The valve 52 is used on the connecting pipeline 51 to control the on-off of the connecting pipeline 51, and can also control the flow of the connecting pipeline 51 by adjusting its own opening.
[0036] In some embodiments, the activated carbon fiber impregnation and modification device further includes an inert gas source 60, which is connected to the first sealed chamber 10 and is used to fill the first sealed chamber 10 with inert gas, so that the impregnated material 100 in the first sealed chamber 10 is protected by inactive gas. In addition, the inert gas source 60 can also purge the inside of the first sealed chamber 10 by filling the inert gas to remove the air in the first sealed chamber 10.
[0037] Preferably, the inert gas is nitrogen. The inert gas source 60 includes a nitrogen bottle 61, a gas path 62 connected between the nitrogen bottle 61 and the first sealed chamber 10, and a gas path valve 63 is provided on the gas path 62. The gas path valve 63 is used to control the passage of the gas path 62 and the internal flow of the gas path 62.
[0038] By using the above-mentioned activated carbon fiber impregnation and modification device to impregnate and modify the activated carbon fiber, the impregnation amount on the activated carbon fiber can reach 5% to 15% (mass ratio).
[0039] The activated carbon fiber impregnation modification method of the present invention is implemented by using the above-mentioned activated carbon fiber impregnation modification device. Figure 1 The activated carbon fiber impregnation modification method may include the following steps:
[0040] S1. placing the impregnation object 100 in the first sealed chamber 10, heating and gasifying the impregnation object 100 to form high-pressure impregnation steam.
[0041] The impregnated substance 100 may be triethylenediamine or hexamethylenetetramine. The first sealed chamber 10 is heated by the heating unit 30 to 200°C ± 30°C and a pressure of 1.6 bar to 2 bar, so that the impregnated substance 100 in the first sealed chamber 10 is heated and vaporized to form high-pressure impregnation steam. The heating temperature is determined according to the selected impregnated substance 100.
[0042] The pressure and temperature in the first sealed chamber 10 can be detected by the first pressure gauge 11 and the first temperature measuring unit 12 respectively.
[0043] Before heating, the first sealed chamber 10 is purged with an inert gas provided by the inert gas source 60 to remove the air in the first sealed chamber 10 and simultaneously place the impregnated object 100 in an inert gas atmosphere.
[0044] The inert gas may be, but is not limited to, nitrogen.
[0045] Before step S1, the activated carbon fiber can also be (selectively) hydrophobically modified as needed to improve the humidity resistance of the activated carbon fiber. The hydrophobic modification can be carried out by pressure spraying a mixed hydrophobic solution prepared with tetraethyl orthosilicate and ethanol evenly spraying it on the surface of the activated carbon fiber. The spraying amount is preferably enough to cover the entire surface of the activated carbon fiber without flowing out. Let it stand for more than 12 hours, then rinse with deionized water, and mechanically dry it in a spin dryer.
[0046] S2. Place the activated carbon fiber 200 in the second sealed chamber 20, and evacuate the second sealed chamber 20 to form a negative pressure.
[0047] Specifically, after the activated carbon fiber 200 is placed in the second sealed chamber 20, the second sealed chamber 20 is evacuated by the vacuum unit 40 to discharge air and other impurities in the chamber to make the chamber as close to absolute vacuum as possible, or to make the pressure in the second sealed chamber 20 ≤-0.99 bar.
[0048] It is understandable that the above steps S1 and S2 do not need to be limited in order, that is, step S1 can be performed first and then step S2, or step S2 can be performed first and then step S1, or steps S1 and S2 can be performed simultaneously.
[0049] S3, passing the high-pressure impregnation steam into the second sealed chamber 20 through the connecting pipe 50; in the second sealed chamber 20, the high-pressure impregnation steam enters into the micropores of the activated carbon fiber 200.
[0050] In combination with the impregnation material 100 in the first sealed chamber 10 being in an inert gas atmosphere, when the impregnation material is heated and gasified to form high-pressure impregnation steam, the high-pressure impregnation steam is also mixed with an inert gas and transported to the second sealed chamber 20 in the form of a mixed gas. When the high-pressure impregnation steam is passed into the second sealed chamber 20, the pressure in the second sealed chamber 20 is -0.8 to -0 bar.g.
[0051] Since the second sealed chamber 20 is in a negative pressure state, the impregnant 100 entering the second sealed chamber 20 is a high-pressure impregnation steam that has been heated and gasified. The impregnant 100 enters the micropores of the activated carbon fiber 200 in the form of gaseous molecules using the vacuum flash explosion principle, and the impregnation amount can reach 5% to 15% (the mass percentage of the activated carbon fiber 200). Compared with the method of using an impregnant aqueous solution, the impregnant 100 enters the micropores of the activated carbon fiber 200 in the form of gaseous molecules, which avoids the problem that the aqueous solution cannot enter the micropores of the activated carbon fiber due to the surface tension of water.
[0052] The present invention is further described below by means of specific examples.
[0053] Example 1
[0054] In the case of a sealed pressure tank with a volume of 1 liter, 15 grams of triethylenediamine are placed, heated to 200°C ± 30°C, and the pressure reaches 1.6 bar to 2 bar. The sealed negative pressure tank is evacuated to -0.99 bar or lower, and the valve on the connecting pipeline is opened to allow the gasified triethylenediamine in the sealed pressure tank to enter the sealed negative pressure tank. When the pressure of the sealed negative pressure tank rises from -0.99 bar to -0.45 bar, the valve on the connecting pipeline is closed, and the activated carbon fiber is taken out after the sealed negative pressure tank is cooled. The obtained activated carbon fiber has an impregnation amount of 10% (triethylenediamine impregnation).
[0055] Example 2
[0056] In the case of a sealed pressure tank with a volume of 1 liter, 15 grams of triethylenediamine are placed, heated to 200°C ± 30°C, and the pressure reaches 1.6 bar to 2 bar. The sealed negative pressure tank is evacuated to -0.99 bar or lower, and the valve on the connecting pipeline is opened to allow the gasified triethylenediamine in the sealed pressure tank to enter the sealed negative pressure tank. When the pressure of the sealed negative pressure tank rises from -0.99 bar to -0.2 bar, the valve on the connecting pipeline is closed, and the activated carbon fiber is taken out after the sealed negative pressure tank is cooled. The obtained activated carbon fiber has an impregnation amount of 15% (triethylenediamine impregnation).
[0057] It can be seen from the above Examples 1 and 2 that the activated carbon fibers can be impregnated to different amounts (impregnation mass ratios) by adjusting the pressure.
[0058] Example 3
[0059] In the case of a sealed pressure tank with a volume of 1 liter, 5 grams of triethylenediamine are placed, heated to 200℃±30℃, and the pressure reaches 1.6 bar to 2 bar. After the sealed negative pressure tank is evacuated to -0.99 bar, the valve on the connecting pipeline is opened to allow the sealed pressure tank and the sealed negative pressure tank to reach a pressure balance, which is about 1 atmosphere of normal pressure, and the valve on the connecting pipeline is closed. After the sealed negative pressure tank is cooled, the activated carbon fiber is taken out, and the obtained activated carbon fiber has an impregnation amount of 10% (triethylenediamine impregnation).
[0060] Example 4
[0061] In the case of a sealed pressure tank with a volume of 1 liter, 8 grams of triethylenediamine are placed, heated to 200℃±30℃, and the pressure reaches 1.6 bar to 2 bar. After the sealed negative pressure tank is evacuated to -0.99 bar, the valve on the connecting pipeline is opened to allow the sealed pressure tank and the sealed negative pressure tank to reach a pressure balance, which is about 1 atmosphere of normal pressure, and the valve on the connecting pipeline is closed. After the sealed negative pressure tank is cooled, the activated carbon fiber is taken out, and the obtained activated carbon fiber has an impregnation amount of 15% (triethylenediamine impregnation).
[0062] It can be seen from the above Examples 3 and 4 that the activated carbon fibers can be impregnated to different amounts (impregnation mass ratios) by adjusting the initial mass of the impregnant.
[0063] Methyl iodide removal test:
[0064] The activated carbon fiber modified by the impregnation of the present invention is immersed in a potassium iodide aqueous solution for 10 minutes to 30 minutes, and then taken out and dried.
[0065] The methyl iodide removal test was conducted according to ASTM D3803-1991. Specifically, the modified activated carbon fiber was tested in the form of an adsorption bed, and the specific conditions are shown in Table 1 below.
[0066] Table 1
[0067]
[0068] Test results: adsorption efficiency 99.909% ± 0.012%;
[0069] Penetration efficiency 0.091%±0.012%.
[0070] It can be seen from the above test results that the impregnated and modified activated carbon fiber can meet the nuclear grade purification capacity requirements in application.
[0071] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for impregnating and modifying activated carbon fibers, It is characterized in that The following steps are involved: S1, placing the impregnated material in a first sealed chamber, heating and gasifying the impregnated material to form high-pressure impregnation steam; S2, placing the activated carbon fiber in a second sealed chamber, and evacuating the second sealed chamber to form a negative pressure; S3, conveying high-pressure impregnation steam into the second sealed chamber; in the second sealed chamber, the high-pressure impregnation steam enters into the micropores of the activated carbon fiber.
2. The activated carbon fiber impregnation modification method according to claim 1, It is characterized in that The impregnated material is triethylenediamine or hexamethylenetetramine.
3. The activated carbon fiber impregnation modification method according to claim 1, It is characterized in that In step S1, the first sealed chamber is heated to 200°C±30°C and the pressure reaches 1.6 bar to 2 bar.
4. The activated carbon fiber impregnation modification method according to claim 1, It is characterized in that In step S2, after the second sealed chamber is evacuated, the pressure is ≤-0.99 bar.
5. The activated carbon fiber impregnation modification method according to claim 1, It is characterized in that Step S1 also includes: purging the first sealed chamber with an inert gas so that the impregnated object is placed in an inert gas atmosphere.
6. The activated carbon fiber impregnation modification method according to claim 5, It is characterized in that In step S3, the inert gas is mixed with the high-pressure impregnation steam and enters the second sealed chamber together.
7. An activated carbon fiber impregnation modification device, It is characterized in that It includes a first sealed chamber for placing an impregnated object, a second sealed chamber for placing activated carbon fibers, a vacuum unit, a heating unit, and a connecting pipeline; The heating unit is disposed in the first sealed chamber to heat the first sealed chamber so as to heat and vaporize the impregnated material in the first sealed chamber; The vacuum unit is connected to the second sealed chamber to vacuum the second sealed chamber; The connecting pipeline is connected between the first sealed chamber and the second sealed chamber, and is used to transport the heated and vaporized impregnated material into the second sealed chamber.
8. The activated carbon fiber impregnation modification device according to claim 7, It is characterized in that The vacuum unit includes a vacuum pump.
9. The activated carbon fiber impregnation modification device according to claim 7, It is characterized in that The connecting pipeline includes a connecting pipeline and a valve arranged on the connecting pipeline.
10. The activated carbon fiber impregnation modification device according to claim 7, It is characterized in that The activated carbon fiber impregnation and modification device also includes an inert gas source, which is connected to the first sealed chamber and is used to fill the first sealed chamber with inert gas.