Composites of manganese-based oxides and zeolites useful as NH3-SCR catalysts

Through the manganese oxide, cerium oxide and zeolite composite catalyst, especially the Mn/Ce/NH4+-ZSM-5 catalyst prepared by the sol-gel method, the problems of low temperature NOx removal efficiency and N2O emission in the prior art are solved. , achieving efficient NOx conversion and low N2O generation.

CN119056488APending Publication Date: 2024-12-03BASF CORPORATON +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310619575.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing SCR catalysts have low efficiency in removing NOx at low temperatures and are not satisfied with N2O emissions. In particular, Cu-promoting zeolite catalysts lack activity at low temperatures, and V2O5/TiO2 catalysts have a risk of environmental pollution.

Method used

The composite of manganese oxide, cerium oxide and zeolite is used as the NH3-SCR catalyst and prepared by the sol-gel method to ensure that the content of molecular sieve in the catalyst is between 20-70%, and the molar ratio of manganese and cerium is between 4:1 In the range of 1:4, the ZSM-5 zeolite of the MFI skeleton is preferably at a calcination temperature of 300-500°C.

Benefits of technology

It achieves high-efficiency NOx conversion rate and low N2O emissions at low temperatures, improves the low-temperature activity and stability of the catalyst, reduces the amount of N2O generation, and is better than the performance of traditional catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056488A_ABST
    Figure CN119056488A_ABST
Patent Text Reader

Abstract

The present invention relates to an NH3-SCR catalyst comprising a complex of manganese oxide, cerium oxide and a molecular sieve, where the molecular sieve is present in an amount of from 20% to 70% by weight based on the total weight of the complex. The invention also relates to a sol-gel process for preparing the NH3-SCR catalyst, an SCR catalytic article comprising the NH3-SCR catalyst, and an exhaust gas treatment system comprising the SCR catalytic article.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a composite of a manganese-based oxide and a zeolite that can be used as a catalyst for the selective catalytic reduction (SCR) of nitrogen oxides in engine exhaust, an SCR catalytic article comprising the composite, an exhaust gas treatment system comprising the SCR catalytic article, and a method for preparing the composite of a manganese-based oxide and a zeolite. Background Art

[0002] Nitrogen oxides (NOx) are common air pollutants that are usually contained in exhaust gases from mobile sources such as cars and stationary sources such as power plants. Due to the negative environmental impact of NOx on ecosystems, humans, animals and plants, the control of NOx emissions has always been one of the most important topics in the field of automobile manufacturing, for example.

[0003] Various treatment methods have been used to treat NO x A gas mixture is prepared to reduce atmospheric pollution. One of the well-known treatment types is the selective catalytic reduction (SCR) process using ammonia or an ammonia precursor as a reducing agent, also known as the NH3-SCR process. The NH3-SCR process is considered to be advantageous because a high degree of NOx reduction can be achieved with a small amount of reducing agent. In the NH3-SCR process, NO x Catalytic reduction by a reducing agent (such as ammonia or urea) in the presence of atmospheric oxygen results in the formation of mainly nitrogen and water vapor:

[0004] 4NO+4NH3+O2→4N2+6H2O (standard SCR reaction)

[0005] 2NO2+4NH3+O2→3N2+6H2O (slow SCR reaction)

[0006] NO+NO2+2NH3→2N2+3H2O (fast SCR reaction).

[0007] A side reaction accompanying the selective catalytic reduction of NOx is the formation of low-valent nitrogen oxides, especially nitrous oxide (N2O), from the reducing agent NH3 and oxygen.

[0008] Current catalysts used in the SCR process include copper-promoted zeolites (e.g., copper-promoted CHA). However, regulations around the world require lower vehicle emissions. In general, efficient removal of NO at low temperatures (<200°C) is required. x This is an unmet need and a huge challenge for the industry. Cu-promoted zeolites are the most active catalyst type for NH3-SCR in diesel vehicles, but such SCR catalysts lack sufficient activity at low temperatures, such as below 200°C. At low temperatures, Cu-promoted zeolite catalysts also need to be saturated with ammonia (NH3) to be effective for NO xreduction, which slows down the response to reducing agents (e.g., urea injection). Vanadium oxide / titanium dioxide (V2O5 / TiO2) based catalysts represent another type of current SCR catalysts that require less NH3 to reach saturation, but are much less active at low temperatures relative to copper-promoted zeolite catalysts. Another disadvantage of vanadium-based catalysts is the environmental issues associated with the potential escape of V2O5 into the atmosphere when using such catalysts.

[0009] Manganese oxide-based catalysts are known to be useful and effective for low-temperature NH3-SCR reactions, which may be manganese oxides or Mn-based multimetallic oxides. Manganese oxides generally produce high N2O emissions, thus resulting in poor N2 selectivity. It has been found that Mn-based multimetallic oxides, such as composite oxides of manganese and cerium (also referred to as "MnCeOx"), can exhibit excellent SCR activity at low temperatures as well as reduced N2O emissions. However, in view of stringent emission regulations, the emission of N2O is still unsatisfactory.

[0010] It is desirable to provide NH3-SCR catalysts that can exhibit desirable NOx conversion levels, particularly at lower temperatures, while resulting in reduced N2O emissions, and methods for preparing NH3-SCR catalysts that exhibit such catalytic performance. Summary of the invention

[0011] It is an object of the present invention to provide an SCR catalyst that exhibits desirable NOx conversion levels and yields acceptable N2O emission levels, particularly at low temperatures (eg, 200°C or lower).

[0012] It has surprisingly been found that this object is achieved by a composite of manganese (Mn) species, cerium (Ce) species and zeolite species.

[0013] Another object of the present invention is to provide a process which is particularly useful for preparing an SCR catalyst which exhibits high NOx conversion levels combined with low N2O emissions.

[0014] This object is achieved by a process comprising preparing a composite of manganese (Mn) species, cerium (Ce) species and zeolite species by a sol-gel process.

[0015] Accordingly, in a first aspect, the present invention relates to an NH3-SCR catalyst comprising a composite of manganese oxide, cerium oxide and a molecular sieve, in particular consisting of a composite of manganese oxide, cerium oxide and a molecular sieve, wherein the molecular sieve is present in an amount of 20 wt% to 70 wt% based on the total weight of the composite.

[0016] In a second aspect, the present invention relates to a sol-gel process for preparing the NH3-SCR catalyst as described herein, comprising the steps of

[0017] (i) providing a suspension comprising a molecular sieve, a precursor of a manganese oxide and a precursor of a cerium oxide,

[0018] (ii) heating the suspension to form a gel, and

[0019] (iii) subjecting the gel to drying, grinding and calcining.

[0020] In a third aspect, the present invention relates to an NH3-SCR article comprising an NH3-SCR catalyst as described herein and preferably in the form of a shaped body or a coated structure.

[0021] In a fourth aspect, the invention relates to a method for treating exhaust gas containing nitrogen oxides by selective catalytic reduction, comprising contacting the exhaust gas with an NH3-SCR catalyst or NH3-SCR article as described herein in the presence of ammonia or an ammonia precursor as a reducing agent.

[0022] In a fifth aspect, the present invention relates to an exhaust gas treatment system for a combustion engine, comprising a reductant source, an NH3-SCR product as described herein, and optionally one or more of the following: a diesel oxidation catalyst (DOC), a three-way conversion catalyst (TWC), a four-way conversion catalyst (FWC), an uncatalyzed or catalyzed soot filter (CSF), an ammonia oxidation catalyst (AMOx), a NOx trap, a NOx absorber catalyst, a hydrocarbon trap catalyst, a sensor, and a mixer.

[0023] The inventors have discovered that composites containing manganese oxides, cerium oxides and molecular sieves are particularly useful as or in NH3-SCR catalysts to provide desirable NOx conversion levels and to obtain acceptable N2O emission levels, especially at low temperatures (eg, 200°C or less). BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Display NH4 separately + - ZSM-5, MnCeOx composites in fresh and aged states and manganese oxides, cerium oxides and NH4 according to the invention in fresh and aged states + -ZSM-5 composite (Mn / Ce / NH4 + -ZSM-5).

[0025] Figure 2a It shows that manganese oxide, cerium oxide and NH4 + -ZSM-5 composite (Mn / Ce / NH4 + -SEM-EDS image of ZSM-5) in fresh state.

[0026] Figure 2bIt shows that manganese oxide, cerium oxide and NH4 + -ZSM-5 composite (Mn / Ce / NH4 + -SEM-EDS images of ZSM-5) under aging conditions. DETAILED DESCRIPTION

[0027] The present invention is described in detail below. It is to be understood that the present invention may be embodied in many different forms and should not be construed as limited to the embodiments set forth herein.

[0028] As used herein, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. The terms "comprising," and the like are used interchangeably with "containing," and the like, and should be interpreted in a non-limiting, open-ended manner. That is, for example, there may be additional components or elements. The phrase "consisting of," or "consisting essentially of," or cognates thereof, may be encompassed by "comprising" or cognates thereof.

[0029] The term "molecular sieve" as used herein refers to framework materials, such as zeolites and other framework materials (e.g., isomorphous substitution materials), which can be used as catalysts in particulate form and in combination with one or more promoter metals. Molecular sieves are materials based on a large three-dimensional network of oxygen ions containing generally tetrahedral sites and having a substantially uniform pore distribution.

[0030] The term "zeolite" as used herein refers to a specific example of a molecular sieve. Typically, zeolite is defined as an aluminosilicate having an open three-dimensional framework structure consisting of corner-sharing TO4 tetrahedra, wherein T is, for example, Al or Si. The cations balancing the charge of the anionic framework are loosely bound to the framework oxygen. For the present disclosure, the term "aluminosilicate zeolite" does not include phosphorus or other metals that are isomorphously substituted in the framework. That is, "aluminosilicate zeolite" does not include aluminophosphate materials, such as SAPO, AlPO and MeA1PO materials, while the more general term "zeolite" includes aluminosilicates and aluminophosphates.

[0031] The term "composite" as used herein refers to a material consisting of a manganese species, a cerium species and a molecular sieve species, which are combined with each other in a uniformly dispersed manner rather than existing as discrete individuals, as determined by SEM-EDS. Physical mixtures of these species obtained by physical means, such as by mechanical mixing or blending, are not included in this term.

[0032] The term "manganese oxide" as used herein is intended to encompass manganese in any possible oxidation state, such as MnO, Mn2O3, Mn3O4, MnO2, MnO3, Mn2O7 or any combination thereof.

[0033] The term "cerium oxide" is also intended to include cerium in any possible oxidation state, such as CeO2, Ce2O3, Ce3O4 or any combination thereof.

[0034] The term "catalytic article" used herein is intended only to mean an article of a certain shape having a catalytic function, which is not necessarily a single entity. In other words, the catalytic article can be a single entity or composed of two or more separable entities.

[0035] In a first aspect, the present invention provides an NH3-SCR catalyst comprising a composite of manganese oxide, cerium oxide and a molecular sieve, in particular consisting of a composite of manganese oxide, cerium oxide and a molecular sieve, wherein the molecular sieve is present in an amount of 20 wt% to 70 wt% based on the total weight of the composite.

[0036] In some embodiments, the NH3-SCR catalyst consists of a composite of manganese oxide, cerium oxide, and a molecular sieve, wherein the molecular sieve is present in an amount of 20 wt% to 70 wt% based on the total weight of the composite.

[0037] According to the present invention, the molecular sieve is preferably present in the composite of manganese oxide, cerium oxide and molecular sieve in an amount of 20 to 50 wt%, more preferably 35 to 45 wt%, based on the total weight of the composite.

[0038] In the composite described herein, manganese oxide and cerium oxide are present in a molar ratio ranging from 4:1 to 1:4, preferably ranging from 7:3 to 3:7, more preferably ranging from 3:2 to 2:3, calculated as Mn and Ce elements.

[0039] For purposes of this invention, suitable molecular sieves may include, but are not limited to, zeolites having a skeletal type selected from the following group: ABW, ACO, AEI, AEL, AEN, AET, AFG, AFI, AFN, AFO, AFR, AFS, AFT, AFV, AFX, AFY, AHT, ANA, APC, APD, AST, ASV , ATN, ATO, ATS, ATT, ATV, AVL, AWO, AWW, BCT, BEA, BEC, BIK, BOF, BOG, BOZ, BPH, BRE, BSV, CAN, CAS, CDO, CFI, CGF, CGS, CHA, -CHI, -CLO, CON, CSV, CZP, DAC, DDR, DFO, DFT, DOH, DON, EAB, EDI, EEI, EMT, EON, EPI, ERI, ESV, ETR, EUO, *-EWT, EZT, FAR, FAU, FER, FRA, GIS, GIU, GME, GON, GOO, HEU, IFO, IFR, - IFU, IFW, IFY, IHW, IMF, IRN, IRR, -IRY, ISV, ITE, ITG, ITH, *-ITN, ITR, ITT, -ITV, ITW, IWR, IWS, IWV, IWW, JBW, JNT, JOZ, JRY, JSN, JSR, JST, JSW, KFI 、LAU、LEV、LIO、-LIT、LOS、LOV、LTA、LTF、LTJ、LTL、LTN、MAR、MAZ、MEI、MEL、MEP、MER、MFI、MFS、MON、MOR、MOZ、*MRE、MSE、MSO、MTF、MTN、MTT、MTW、MVY、 MWF、MWW、NAB、NAT、NES、NON、NPO、NPT、NSI、OBW、OFF、OKO、OSI、OSO、OWE、-PAR、PAU、PCR、PHI、PON、POS、PSI、PUN、RHO、-RON、RRO、RSN、RTE、RTH、RUT、R WR, RWY, SAF, SAO, SAS, SAT, SAV, SBE, SBN, SBS, SBT, SEW, SFE, SFF, SFG, SFH, SFN, SFO, SFS, *SFV, SFW, SGT, SIV, SOD, SOF, SOS, SSF, *-SSO, SSY, STF, S TI, *STO, STT, STW, -SVR, SVV, SZR, TER, THO, TOL, TON, TSC, TUN, UEI, UFI, UOS, UOV, UOZ, USI, UTL, UWY, VET, VFI, VNI, VSV, WEI, -WEN, YUG, ZON and any combination thereof.

[0040] In particular, suitable molecular sieves may be zeolites having a framework type selected from the group consisting of AEI, AEL, AFI, AFT, AFO, AFX, AFR, ATO, BEA, CHA, DDR, EAB, EMT, ERI, EUO, FAU, FER, GME, HEU, JSR, KFI, LEV, LTA, LTL, LTN, MAZ, MEL, MFI, MOR, MOZ, MSO, MTW, MWW, OFF, RTH, SAS, SAT, SAV, SBS, SBT, SFW, SSF, SZR, TON, TSC, WEN, and any combination thereof.

[0041] It is to be appreciated that when zeolites are referred to herein with reference to framework type codes as recognized by the International Zeolite Association (IZA), it is intended to include not only the standard material, but also any isotype framework material having SCR catalytic activity. Lists of standard materials and isotype framework materials for each framework type code can be obtained from the IZA database (http: / / www.iza-structure.org / databases / ).

[0042] There is no particular limitation on the cations that balance the charge of the anionic framework in the zeolites that can be used as molecular sieves in the composites described herein. In other words, the zeolites described above can be in their H form, NH4 + forms, metal ion exchange forms, such as copper exchange forms and / or iron exchange forms, and any other suitable forms.

[0043] In some embodiments, the molecular sieve in the composite described herein is a zeolite having a framework type selected from the group consisting of BEA (e.g. Beta), CHA (e.g. Chabazite), FAU (e.g. zeolite Y), FER (e.g. ferrierite), MFI (e.g. ZSM-5) and MOR (e.g. mordenite). The molecular sieve in the composite described herein is particularly a zeolite having an MFI framework, such as ZSM-5, preferably H-form ZSM-5 (H-ZSM-5) or NH4 + ZSM-5(NH4 + -ZSM-5), especially NH4 + form of ZSM-5.

[0044] Zeolites useful as molecular sieves in the composites described herein may have a SiO2 / Al2O3 molar ratio (SAR) in the range of 5:1 to 150:1, preferably 5:1 to 50:1.

[0045] The molecular sieve may have a molecular weight of at least 150 m2 / g, at least 250m 2 / g or at least 300m 2 / g of BET surface area.

[0046] In some exemplary embodiments, the NH3-SCR catalyst according to the present invention consists of a composite of manganese oxide, cerium oxide and a molecular sieve, wherein the molecular sieve is present in an amount of 20 wt% to 70 wt% based on the total weight of the composite, and wherein the molecular sieve is a zeolite having a framework type selected from the group consisting of BEA (e.g., Beta), CHA (e.g., chabazite), FAU (e.g., zeolite Y), FER (e.g., ferrierite), MFI (e.g., ZSM-5) and MOR (e.g., mordenite).

[0047] In these exemplary embodiments, the molecular sieve is preferably present in an amount of 20 wt % to 50 wt % based on the total weight of the composite. In these exemplary embodiments, the molecular sieve is more preferably present in an amount of 35 wt % to 45 wt % based on the total weight of the composite.

[0048] In some specific embodiments, the NH3-SCR catalyst according to the present invention is composed of a composite of manganese oxide, cerium oxide and a molecular sieve, wherein the molecular sieve is present in an amount of 20 wt% to 50 wt% based on the total weight of the composite, and wherein the molecular sieve is in the H form or NH4 + The zeolite in the form of a zeolite having a framework type selected from the group consisting of BEA (eg, Beta), CHA (eg, chabazite), FAU (eg, zeolite Y), FER (eg, ferrierite), MFI (eg, ZSM-5), and MOR (eg, mordenite).

[0049] More particularly, the NH3-SCR catalyst according to the present invention consists of a composite of manganese oxide, cerium oxide and a molecular sieve, wherein the molecular sieve is present in an amount of 35 wt % to 45 wt % based on the total weight of the composite, and wherein the molecular sieve is NH4 + A zeolite having an MFI framework type (eg ZSM-5) in the form of.

[0050] In some other exemplary embodiments, the NH3-SCR catalyst according to the present invention is composed of a composite of manganese oxide, cerium oxide and molecular sieve, wherein

[0051] - the molecular sieve is present in an amount of 20% to 70% by weight, based on the total weight of the composite,

[0052] - manganese oxide and cerium oxide are present in a molar ratio ranging from 4:1 to 1:4, and

[0053] The molecular sieve is a zeolite having a framework type selected from the group consisting of BEA (eg Beta), CHA (eg Chabazite), FAU (eg zeolite Y), FER (eg ferrierite), MFI (eg ZSM-5) and MOR (eg mordenite).

[0054] Preferably, the NH3-SCR catalyst according to the present invention is composed of a composite of manganese oxide, cerium oxide and molecular sieve, wherein

[0055] - the molecular sieve is present in an amount of 20% to 50% by weight, based on the total weight of the composite,

[0056] - manganese oxide and cerium oxide are present in a molar ratio ranging from 7:3 to 3:7, and

[0057] The molecular sieve is a zeolite having a framework type selected from the group consisting of BEA (eg Beta), CHA (eg Chabazite), FAU (eg zeolite Y), FER (eg ferrierite), MFI (eg ZSM-5) and MOR (eg mordenite).

[0058] More preferably, the NH3-SCR catalyst according to the present invention is composed of a composite of manganese oxide, cerium oxide and molecular sieve, wherein

[0059] - the molecular sieve is present in an amount of 35% to 45% by weight, based on the total weight of the composite,

[0060] - manganese oxide and cerium oxide are present in a molar ratio ranging from 3:2 to 2:3, and

[0061] The molecular sieve is a zeolite having a framework type selected from the group consisting of BEA (eg Beta), CHA (eg Chabazite), FAU (eg zeolite Y), FER (eg ferrierite), MFI (eg ZSM-5) and MOR (eg mordenite).

[0062] Most preferably, the NH3-SCR catalyst according to the present invention consists of a composite of manganese oxide, cerium oxide and molecular sieve, wherein

[0063] - the molecular sieve is present in an amount of 35% to 45% by weight, based on the total weight of the composite,

[0064] - manganese oxide and cerium oxide are present in a molar ratio ranging from 3:2 to 2:3, and

[0065] -Molecular sieve is NH4 + A zeolite having an MFI framework type (eg ZSM-5) in the form of.

[0066] In some embodiments, the composites described herein contain a CeO2 phase (

[111] ) having a crystallite size of 3.5 nm or less, e.g., 3.2 nm or less, in a fresh state, and / or having a crystallite size of 6.5 nm or less, e.g., 6.0 nm or less, after hydrothermal aging at 650° C. for 50 hours in an air atmosphere containing 10% water vapor. The crystallite size of CeO2 (

[111] ) is determined by X-ray powder diffraction (XRD) analysis.

[0067] The composites described herein may have a content of at least 100 m 2 / g, for example at least 150m 2 / g, and / or at least 50m2 after hydrothermal aging at 650°C for 50 hours in an air atmosphere containing 10% water vapor. 2 / g, for example at least 75m 2 / g or at least 100m 2 / g BET specific surface area.

[0068] The composite described herein, i.e., the composite of manganese oxide, cerium oxide and molecular sieve, can be prepared by any suitable method that can provide the composite from manganese precursor, cerium precursor and molecular sieve. Preferably, the composite of manganese oxide, cerium oxide and molecular sieve can be prepared by coprecipitation or sol-gel method, more preferably by sol-gel method.

[0069] The inventors have surprisingly found that a composite of manganese oxide, cerium oxide and molecular sieve prepared by a sol-gel process is particularly advantageous in terms of the low temperature catalytic performance of the composite when used in an NH3-SCR process.

[0070] Accordingly, in a second aspect, the present invention provides a sol-gel method for preparing the NH3-SCR catalyst as described in the first aspect, comprising the steps of:

[0071] (i) providing a suspension comprising a molecular sieve, a precursor of a manganese oxide and a precursor of a cerium oxide,

[0072] (ii) heating the suspension to form a gel, and

[0073] (iii) subjecting the gel to drying, grinding and calcining.

[0074] Suitable molecular sieves for use in the sol-gel process according to the invention are those generally described above and as being preferred in the first aspect.

[0075] As used herein, the term "precursor" refers to materials that can decompose or otherwise convert to the respective catalytically active species (ie, manganese oxide and cerium oxide, respectively) upon calcination or use of the catalyst.

[0076] Suitable manganese oxide precursors for the sol-gel method according to the present invention may be any inorganic or organic, water-soluble or water-dispersible manganese compounds, such as salts and complexes of manganese. Suitable cerium oxide precursors for the sol-gel method according to the present invention may also be any inorganic or organic, water-soluble or water-dispersible cerium compounds, such as salts and complexes of cerium.

[0077] In particular, the suspension in step (i) further comprises an aqueous medium, preferably water, more preferably deionized water (DI water) or demineralized water.

[0078] The suspension in step (i) may further comprise a complexing agent, such as citric acid.

[0079] In step (i), the suspension may be provided by preparing a mixture containing the molecular sieve, a precursor of the manganese oxide and a precursor of the cerium oxide and then dissolving the mixture in an aqueous medium, preferably DI water. The mixture may also contain a complexing agent, such as citric acid.

[0080] In step (ii), the suspension obtained from step (i) is heated, preferably under stirring, to form a gel. The heating may be carried out at a temperature of 70°C to 100°C, for example 80°C to 90°C.

[0081] In step (iii), the gel obtained from step (ii) is dried, ground and calcined. Drying, grinding and calcining can be carried out in any conventional manner and conditions known in the art. In particular, drying can be carried out at a temperature of 40 to 100° C., for example 60 to 80° C. to remove the aqueous medium. The resulting solid can be further ground into a powder having a suitable particle size. Then, the powder is calcined at a temperature of 300° C. to 500° C., for example 300° C. or 400° C. to provide a composite of manganese oxide, cerium oxide and molecular sieve.

[0082] In some exemplary embodiments, the present invention provides a sol-gel method for preparing the NH3-SCR catalyst according to the first aspect, which comprises the steps of:

[0083] (i) providing a suspension comprising a molecular sieve, a precursor of a manganese oxide, a precursor of a cerium oxide and a complexing agent in an aqueous medium, preferably water,

[0084] (ii) heating the suspension to form a gel, and

[0085] (iii) subjecting the gel to drying, grinding and calcining.

[0086] In particular, the present invention provides a sol-gel method for preparing the NH3-SCR catalyst as described in the first aspect, which comprises the steps of

[0087] (i) providing a suspension comprising a molecular sieve, a water-soluble manganese salt, a water-soluble cerium salt and citric acid in water,

[0088] (ii) heating the suspension to form a gel, and

[0089] (iii) subjecting the gel to drying, grinding and calcining.

[0090] It has been found that NH3-SCR catalysts prepared by a sol-gel method can exhibit reduced N2O generation compared to counterparts prepared by a co-precipitation method, higher low-temperature NOx conversion compared to counterparts prepared by an impregnation method, and both higher low-temperature NOx conversion and reduced N2O generation compared to counterparts prepared by mixing Mn / Ce composite oxides with molecular sieves.

[0091] The NH3-SCR catalyst according to the first aspect of the present invention or the NH3-SCR catalyst obtained from the sol-gel process according to the second aspect of the present invention can be used in any conventional form for exhaust gas treatment applications. For example, the NH3-SCR catalyst can be used as a powder or can be processed into a shaped body or coated on a substrate in a conventional manner.

[0092] Accordingly, in a third aspect, the present invention provides an NH3-SCR product comprising the NH3-SCR catalyst as described in the first aspect or the NH3-SCR catalyst obtained from the sol-gel method as described in the second aspect, and preferably in the form of a shaped body or a coated structure.

[0093] The NH3-SCR product may be in the form of a shaped body, such as an extrudate, in particular a granular extrudate or a monolithic extrudate. The granular extrudate may be in various shapes, such as pellets, beads, rings, spheres, cylinders, trilobes and quadrilobes. The monolithic extrudate may have any suitable structure that allows exhaust gas to flow through, preferably a honeycomb structure. The honeycomb structure may have flow channels as described below for the monolithic flow-through structure and the wall-flow structure. This form of NH3-SCR product may contain an NH3-SCR catalyst and optionally other conventional functional components or processing aids, such as adhesives and lubricants.

[0094] Alternatively, the NH3-SCR article may be in the form of a coated structure comprising an NH3-SCR catalyst in a coating on a substrate. The substrate generally refers to a structure suitable for withstanding the conditions encountered in the exhaust gas stream, and the NH3-SCR catalyst is supported thereon in the form of a coating, especially a washcoat.

[0095] Suitable substrates may have a monolithic flow-through type structure having a plurality of thin parallel gas flow channels extending from an inlet face to an outlet face of the substrate, the channels being open to fluid flow therethrough. The channels, which are substantially straight paths from their fluid inlet to their fluid outlet, are defined by walls to which the catalytic material is applied as a coating, particularly a washcoat, so that gases flowing through the channels contact the catalytic material.

[0096] The substrate may also have a monolithic wall-flow structure having many thin parallel gas flow channels extending from the inlet face to the outlet face of the substrate with alternating channels blocked at opposite ends. The channels are delimited by walls to which the catalytic material is applied as a coating, particularly a washcoat, so that the gas flowing through the channels contacts the catalytic material. This configuration requires the gas to flow through the porous walls of the wall-flow substrate to reach the outlet face.

[0097] The term "washcoat" has its ordinary meaning in the art and refers to a thin adherent coating of a catalytic material or other material applied to a substrate. The washcoat is typically formed by preparing a slurry containing the desired catalytic material and optional processing aids such as a binder having a certain solid content (e.g., 15 to 60 wt%), then applying the slurry to a substrate, drying and calcining to provide the washcoat.

[0098] The NH3-SCR product according to the invention can be used to treat exhaust gases from, for example, stationary combustion devices such as power plants and heating systems of buildings and private homes, as well as mobile combustion devices such as combustion engines of vehicles, in particular diesel engines. The NH3-SCR product according to the invention can particularly effectively treat exhaust gases from internal combustion engines, such as diesel engines.

[0099] The NH3-SCR article according to the present invention may be located downstream of an internal combustion engine, such as a diesel engine, in a close-in position, in a position downstream of a close-in position, or both. Preferably, the catalytic article according to the present invention is located downstream of an internal combustion engine in a close-in position.

[0100] Accordingly, in a fourth aspect, the present invention relates to a method for treating exhaust gas containing nitrogen oxides by selective catalytic reduction, which comprises contacting the exhaust gas with an NH3-SCR catalyst or NH3-SCR article as described herein in the presence of ammonia or an ammonia precursor as a reducing agent.

[0101] In addition, in a fifth aspect, the present invention provides an exhaust treatment system for a combustion engine, comprising a reductant source, the NH3-SCR product described herein and optionally one or more of the following: a diesel oxidation catalyst (DOC), a three-way conversion catalyst (TWC), a four-way conversion catalyst (FWC), an uncatalyzed or catalyzed soot filter (CSF), an ammonia oxidation catalyst (AMOx), a NOx trap, a NOx absorber catalyst, a hydrocarbon trap catalyst, a sensor and a mixer.

[0102] Preferably, the exhaust treatment system further comprises a diesel oxidation catalyst located downstream of the engine and upstream of the NH3-SCR article according to the present invention. In some embodiments, the exhaust treatment system preferably comprises a diesel oxidation catalyst and a catalyzed soot filter located upstream of the catalytic article according to the present invention.

[0103] Implementation

[0104] Various embodiments are listed below. It is to be understood that the following embodiments can be combined with all aspects and other embodiments according to the scope of the present invention.

[0105] 1. An NH3-SCR catalyst comprising a composite of manganese oxide, cerium oxide and a molecular sieve, in particular consisting of a composite of manganese oxide, cerium oxide and a molecular sieve, wherein the molecular sieve is present in an amount of 20 wt % to 70 wt % based on the total weight of the composite.

[0106] 2. The NH3-SCR catalyst according to embodiment 1, wherein the molecular sieve is present in the composite of manganese oxide, cerium oxide and molecular sieve in an amount of 20 to 50 wt%, more preferably 35 to 45 wt%, based on the total weight of the composite.

[0107] 3. The NH3-SCR catalyst according to embodiment 1 or 2, wherein the manganese oxide and the cerium oxide are present in a molar ratio in the range of 4:1 to 1:4, preferably in the range of 7:3 to 3:7, more preferably in the range of 3:2 to 2:3, calculated as Mn and Ce elements.

[0108] 4.If the NH3-SCR reactor is 1 or 3 inches thick, then ABW, ACO, AEI, AE L、AEN、AET、AFG、AFI、AFN、AFO、AFR、AFS、AFT、AFV、AFX、AFY、AHT、ANA、APC、 APD、AST、ASV、ATN、ATO、ATS、ATT、ATV、AVL、AWO、AWW、BCT、BEA、BEC、BIK、BO F、BOG、BOZ、BPH、BRE、BSV、CAN、CAS、CDO、CFI、CGF、CGS、CHA、-CHI、-CLO、CO N、CSV、CZP、DAC、DDR、DFO、DFT、DOH、DON、EAB、EDI、EEI、EMT、EON、EPI、ERI、 ESV、ETR、EUO、*-EWT、EZT、FAR、FAU、FER、FRA、GIS、GIU、GME、GON、GOO、HEU、 IFO、IFR、-IFU、IFW、IFY、IHW、IMF、IRN、IRR、-IRY、ISV、ITE、ITG、ITH、*-IT N、ITR、ITT、-ITV、ITW、IWR、IWS、IWV、IWW、JBW、JNT、JOZ、JRY、JSN、JSR、JST 、JSW、KFI、LAU、LEV、LIO、-LIT、LOS、LOV、LTA、LTF、LTJ、LTL、LTN、MAR、MAZ 、MEI、MEL、MEP、MER、MFI、MFS、MON、MOR、MOZ、*MRE、MSE、MSO、MTF、MTN、MTT、 MTW、MVY、MWF、MWW、NAB、NAT、NES、NON、NPO、NPT、NSI、OBW、OFF、OKO、OSI、OS O、OWE、-PAR、PAU、PCR、PHI、PON、POS、PSI、PUN、RHO、-RON、RRO、RSN、RTE、RT H、RUT、RWR、RWY、SAF、SAO、SAS、SAT、SAV、SBE、SBN、SBS、SBT、SEW、SFE、SFF、 SFG、SFH、SFN、SFO、SFS、*SFV、SFW、SGT、SIV、SOD、SOF、SOS、SSF、*-SSO、SSY 、STF、STI、*STO、STT、STW、-SVR、SVV、SZR、TER、THO、TOL、TON、TSC、TUN、UEI 、UFI、UOS、UOV、UOZ、USI、UTL、UWY、VET、VFI、VNI、VSV、WEI、-WEN、YUGZON。

[0109] 5. The NH3-SCR catalyst according to any one of embodiments 1 to 4, wherein the molecular sieve is selected from zeolites having the following framework types: AEI, AEL, AFI, AFT, AFO, AFX, AFR, ATO, BEA, CHA, DDR, EAB, EMT, ERI, EUO, FAU, FER, GME, HEU, JSR, KFI, LEV, LTA, LTL, LTN, MAZ, MEL, MFI, MOR, MOZ, MSO, MTW, MWW, OFF, RTH, SAS, SAT, SAV, SBS, SBT, SFW, SSF, SZR, TON, TSC and WEN.

[0110] 6. The NH3-SCR catalyst according to embodiment 4 or 5, wherein the zeolite is in the respective H form, NH4 + form or a metal ion exchange form, such as a copper exchange form and / or an iron exchange form.

[0111] 7. The NH3-SCR catalyst according to any one of embodiments 1 to 6, wherein the molecular sieve is a zeolite having a framework type selected from the group consisting of BEA (e.g. Beta), CHA (e.g. Chabazite), FAU (e.g. zeolite Y), FER (e.g. ferrierite), MFI (e.g. ZSM-5) and MOR (e.g. mordenite), preferably MFI (e.g. ZSM-5), more preferably NH4 + Form of MFI (e.g. ZSM-5).

[0112] 8. The NH3-SCR catalyst according to any one of embodiments 1 to 7, wherein the composite of manganese oxide, cerium oxide and molecular sieve is prepared by a co-precipitation method or a sol-gel method, more preferably a sol-gel method.

[0113] 9. A sol-gel method for preparing an NH3-SCR catalyst according to any one of embodiments 1 to 8, comprising the steps of

[0114] (i) providing a suspension comprising a molecular sieve, a precursor of a manganese oxide and a precursor of a cerium oxide,

[0115] (ii) heating the suspension to form a gel, and

[0116] (iii) subjecting the gel to drying, grinding and calcining.

[0117] 10. The sol-gel process according to embodiment 9, wherein the suspension in step (i) comprises an aqueous medium, preferably water.

[0118] 11. The sol-gel process according to embodiment 9 or 10, wherein the suspension in step (i) comprises a complexing agent, such as citric acid.

[0119] 12. The process according to any one of embodiments 9 to 11, wherein the heating in step (ii) is carried out at a temperature of 70°C to 100°C.

[0120] 13. The process according to any one of embodiments 9 to 12, wherein the calcination in step (iii) is carried out at a temperature of 300°C to 500°C, such as 300°C or 400°C.

[0121] 14. An NH3-SCR article comprising the NH3-SCR catalyst according to any one of embodiments 1 to 8 or the NH3-SCR catalyst obtained from the sol-gel process according to any one of embodiments 9 to 13.

[0122] 15. The NH3-SCR article according to embodiment 14, which is in the form of a shaped body, such as an extrudate or a coated structure.

[0123] 16. The NH3-SCR article according to embodiment 15, which is in the form of a pellet extrudate or a monolith extrudate.

[0124] 17. The NH3-SCR article according to embodiment 15, which is in the form of a coated structure comprising the NH3-SCR catalyst in a coating layer on a substrate.

[0125] 18. The NH3-SCR article according to embodiment 17, wherein the substrate is a monolithic flow-through structure or a monolithic wall-flow structure.

[0126] 19. A method for treating exhaust gas containing nitrogen oxides by selective catalytic reduction, comprising contacting the exhaust gas with an NH3-SCR catalyst according to any one of embodiments 1 to 8, an NH3-SCR catalyst obtained from a sol-gel process according to any one of embodiments 9 to 13, or an NH3-SCR product according to any one of embodiments 14 to 18 in the presence of ammonia or an ammonia precursor as a reducing agent.

[0127] 20. An exhaust treatment system for a combustion engine, comprising a reductant source, an NH3-SCR article according to any one of embodiments 14 to 18, and optionally one or more of the following: a diesel oxidation catalyst (DOC), a three-way conversion catalyst (TWC), a four-way conversion catalyst (FWC), an uncatalyzed or catalyzed soot filter (CSF), an ammonia oxidation catalyst (AMOx), a NOx trap, a NOx absorber catalyst, a hydrocarbon trap catalyst, a sensor, and a mixer.

[0128] 21. The exhaust gas treatment system according to embodiment 20, comprising a diesel oxidation catalyst located downstream of the engine and upstream of the NH3-SCR product.

[0129] 22. The exhaust gas treatment system according to embodiment 20 or 21, comprising a diesel oxidation catalyst and a catalyzed soot filter located downstream of the engine and upstream of the NH3-SCR article.

[0130] The invention is further illustrated by the following examples, which illustrate particularly advantageous embodiments.While the examples are provided to illustrate the invention, they are not intended to limit the invention.

[0131] Example

[0132] I. Materials

[0133] Cu-SSZ-13 SAR=27, 3.2 wt% CuO from Zeolyst H-CHA SAR=27, H form, from Zeolyst HY SAR=30, H form, from Zeolyst Ferrierite <![CDATA[SAR=20,NH4 + form, from Zeolyst]]> Mordenite <![CDATA[SAR=20,NH4 + form, from Zeolyst]]> Beta <![CDATA[SAR=25,NH4 + form, from Zeolyst]]> H-ZSM-5 <![CDATA[Calcined NH4 + -ZSM-5]]> Fe-ZSM-5 <![CDATA[SAR = 30, 0.41 wt% Fe2O3, from Zeolyst]]> <![CDATA[NH4 + -ZSM-5]]> <![CDATA[SAR=30,NH4 + form, from Zeolyst]]>

[0134] II. General Preparation Procedure

[0135] II.1 Preparation of Mn and Ce composite oxide (MnCeOx) by sol-gel method

[0136] A mixture of Mn(NO3)4·4H2O, Ce(NO3)3·6H2O and citric acid in a molar ratio of 1:1:2 was dissolved in deionized water with a mixture / water weight ratio of 1:50 under stirring and heated at 90°C until a gel was formed. The gel was dried in an oven at 80°C overnight. The resulting solid was ground into a powder with a particle size of 40-60 mesh and calcined in a muffle furnace at 300°C for 4 hours.

[0137] II.2 Preparation of Mn / Ce / zeolite composites by coprecipitation

[0138] A mixture of a certain amount of Mn(NO3)4·4H2O, Ce(NO3)3·6H2O and zeolite indicated for each composite sample was prepared. The mixture was dissolved with deionized (DI) water in a mixture / water weight ratio of 1:50. Ammonia was then added to the resulting suspension to adjust the pH to 11 and stirred at room temperature until a sediment was formed. The sediment was separated by filtration and washed, and then dried in a furnace overnight. Finally, the resulting solid was ground into a powder with a particle size of 40-60 mesh and calcined in a muffle furnace at 300°C for 4 hours. Composites of manganese oxide, cerium oxide and zeolite, referred to as Mn / Ce / zeolite, such as Mn / Ce / NH4 are provided. + -ZSM-5.

[0139] II.3 Preparation of Mn / Ce / zeolite composites by sol-gel method

[0140] A mixture of Mn(NO3)4·4H2O, Ce(NO3)3·6H2O and citric acid at a (Mn+Ce) / citric acid molar ratio of 1:2 is prepared, and a certain amount of zeolite is added to the mixture. The mixture is dissolved with deionized (DI) water at a mixture / water weight ratio of 1:50 under stirring and heated at 90°C until a gel is formed. The gel is dried in a furnace at 80°C overnight. The resulting solid is ground into a powder having a particle size of 40-60 mesh and calcined in a muffle furnace at 300°C or 400°C for 4 hours. A composite of manganese oxide, cerium oxide and zeolite, referred to as Mn / Ce / zeolite, such as Mn / Ce / NH4 is provided. + -ZSM-5.

[0141] II.4 By grinding MnCeO x Preparation of MnCeO from a mixture of zeolite and x Composite mixture with zeolite (grinding method)

[0142] A mixture of Mn(NO3)4·4H2O, Ce(NO3)3·6H2O and citric acid at a (Mn+Ce) / citric acid molar ratio of 1:2 was prepared, and then dissolved with deionized water at a mixture / water weight ratio of 1:0.3 under stirring and heated at 90°C until a colloid was formed. The gel was dried in a furnace at 80°C overnight. The obtained solid was ground into powder and calcined in a muffle furnace at 300°C for 4 hours to obtain a Mn / Ce composite oxide (i.e., MnCeO x ). A certain amount of MnCeO x Mixed with zeolite and ground into powder with a particle size of 40-60 mesh. A composite mixture of MnCeOx and zeolite is provided, referred to as MnCeO x / zeolite, such as MnCeO x / NH4 + -ZSM-5.

[0143] II.5 Preparation of MnCeO by water mixing method x Composite mixture of zeolite

[0144] A mixture of Mn(NO3)4·4H2O, Ce(NO3)3·6H2O and citric acid in a molar ratio of 1:1:2 was prepared, and then dissolved with deionized water in a mixture / water weight ratio of 1:50 under stirring and heated at 90°C until a gel was formed. The gel was dried in a furnace at 80°C overnight. The obtained solid was ground into powder and calcined in a muffle furnace at 300°C for 4 hours to obtain a Mn / Ce composite oxide (i.e., MnCeO x ). Then a certain amount of MnCeO x and zeolite were mixed with an appropriate amount of deionized water to make MnCeO xThe precipitate was filtered, washed and dried in a furnace at 80°C overnight. The solid was ground into a powder with a particle size of 40-60 mesh and calcined in a muffle furnace at 300°C for 4 hours. x and zeolite, designated as MnCeO x / zeolites, such as MnCeO x / NH4 + -ZSM-5.

[0145] II.6 Preparation of Mn / Ce / zeolite composites by impregnation method

[0146] A mixture of Mn(NO3)4·4H2O and Ce(NO3)3·6H2O in a 1:1 molar ratio was dissolved with deionized water in a mixture / water weight ratio of 1:0.3. A certain amount of zeolite was added to the resulting solution and kept stirring for 2 hours. The resulting sediment was then filtered, washed and dried in a furnace at 80°C overnight. The resulting solid was ground into a powder with a particle size of 40-60 mesh and calcined in a muffle furnace at 300°C for 4 hours. A composite of manganese oxide, cerium oxide and zeolite, referred to as Mn / Ce / zeolite, such as Mn / Ce / NH4 is provided. + -ZSM-5.

[0147] III. Characterization Methods

[0148] X-ray diffraction (XRD) experiments were performed on a Rigaku D / MAS-RB X-ray diffractometer using CuKα (40 kV, 40 mA) radiation, and XRD patterns were recorded in the 2θ range of 10° to 90° at a scan rate of 8° / min.

[0149] SEM-EDS characterization was performed on a field emission69 scanning electron microscope (FE-SEM, SIGMA-3000). Energy dispersive spectroscopy (EDS)70 mapping of the catalysts was done on an Oxford Instruments EDS.

[0150] Nitrogen adsorption-desorption experiments were conducted using a US Quantachrome ASAP 2020M nitrogen adsorption instrument at 77 K, and the specific surface area was calculated using the Brunaue-Emmett-Teller (BET) method. The samples were degassed at 200 °C for 10 h before the experiment.

[0151] IV. SCR Performance Measurement

[0152] The SCR performance measurements were performed using a fixed bed quartz flow reactor (inner diameter = 4 mm) and 0.15 g of 40-60 mesh catalyst. The SCR activity measurements were performed in the temperature range of 90 to 480°C.

[0153] The gas stream used consisted of 500 vppm NO, 500 vppm NH3, 10 volume % O2, 5 volume % H2O, 5 volume % CO2 and N2 as the balance gas. The total flow rate was controlled at 475 mL min -1 , corresponding to 200,000 mL g -1 ·h -1 Gas hourly space velocity (GHSV, weight), 150,000h -1 The GHSV (volume) of cordierite was the same for all catalysts.

[0154] To measure the aged samples, the prepared fresh samples were hydrothermally treated at 650°C for 50 h in an air atmosphere containing 10% H2O before measurement.

[0155] The gas concentrations of NO, NO2, NH3, H2O and N2O were monitored simultaneously by FTIR spectrometer (Thermo Fisher). The SCR catalytic activity was recorded after the reaction system reached a steady state. The NOx conversion rate was calculated by referring to the following equation:

[0156]

[0157] The test results are summarized in the following table.

[0158] Table 1

[0159]

[0160] The composites of manganese oxide, cerium oxide and zeolite shown in Table 1 all have a mass ratio of the sum of manganese oxide and cerium oxide to zeolite of 1.5:1, a molar ratio of Mn:Ce of 1:1, and are prepared by a gel-sol method according to the general procedure as described under II.3 above and a calcination temperature of 300°C. Composite Mn / Co / NH4 + -ZSM-5 and Mn / Sm / NH4 + - ZSM-5 was prepared according to the same procedure and had a mass ratio of the sum of manganese oxide and cobalt oxide (or the sum of manganese oxide and samarium oxide) to zeolite of 1.5:1, a molar ratio of Mn:Co (or Sm) of 1:1.

[0161] From the test results shown in Table 1, it can be seen that the composite of manganese oxide, cerium oxide and zeolite according to the present invention exhibits a much higher low-temperature NOx conversion rate than conventional Cu-SSZ-13. The low-temperature NOx conversion rate of the composite of manganese oxide, cerium oxide and zeolite according to the present invention is comparable to that of conventional MnCeO x The N2O generation is equivalent to or slightly lower than that of conventional MnCeO x Much lower.

[0162] It can also be seen that the fresh composite Mn / Ce / NH4 according to the present invention + -ZSM-5 shows better performance than fresh composite Mn / Sm / NH4 + -ZSM-5 has much higher low temperature NOx conversion and better performance than Mn / Co / NH4 + -The fresh composite of ZSM-5 has much lower N2O generation. In addition, the aged composite Mn / Ce / NH4 according to the present invention + -ZSM-5 exhibits a better performance than the aged composite Mn / Co / NH4 + -ZSM-5 and Mn / Sm / NH4 + -ZSM-5 has much higher low temperature NOx conversion and less N2O generation. Therefore, as a catalyst for SCR applications, the composite Mn / Ce / NH4 + -ZSM-5 is superior to Mn / Co / NH4 + -ZSM-5 and Mn / Sm / NH4 + -ZSM-5.

[0163] Table 2

[0164]

[0165]

[0166] The composites of manganese oxide, cerium oxide and zeolite shown in Table 2 all have a mass ratio of the sum of manganese oxide and cerium oxide to zeolite of 1.5:1, a molar ratio of Mn:Ce of 1:1, are prepared by a gel-sol method according to the general procedure as described under II.3 above and a calcination temperature of 400°C.

[0167] It can be seen from the test results shown in Table 2 that the composite of manganese oxide, cerium oxide and zeolite prepared according to the present invention at a higher calcination temperature still exhibits the same performance as conventional MnCeO x Equivalent or slightly lower low-temperature NOx conversion rate, while N2O generation is less than conventional MnCeO x Much lower.

[0168] Table 3

[0169]

[0170]

[0171] The composites of manganese oxide, cerium oxide and zeolite shown in Table 3 all have the mass ratio of the sum of manganese oxide and cerium oxide to zeolite shown in brackets and have a molar ratio of Mn:Ce of 1:1, and are prepared by the gel-sol method according to the general procedure described under II.3 above and the calcination temperature is 300°C.

[0172] From the results shown in Table 3, it can be seen that the composites of manganese oxide, cerium oxide and various forms of ZSM-5 according to the present invention can show good low-temperature NOx conversion and better performance than MnCeO x Low N2O generation, including composite Mn / Ce / NH4 + -ZSM-5 is better for SCR applications.

[0173] Table 4

[0174]

[0175] Mn / Ce / NH4 shown in Table 4 + -ZSM-5 composites all had the indicated mass ratio of the sum of manganese oxide and cerium oxide to zeolite and had a molar ratio of Mn:Ce of 1:1, were prepared by the gel-sol method according to the general procedure as described under II.3 above and the calcination temperature was 300°C.

[0176] From the results shown in Table 4, it can be seen that the manganese oxide, cerium oxide and NH4 + -ZSM-5 composites can show good low-temperature NOx conversion and better performance than MnCeO x Low N2O generation, wherein the mass ratio of the sum of manganese oxide and cerium oxide to zeolite is 1.5:1, a composite Mn / Ce / NH4 + -ZSM-5 is the best.

[0177] Table 5

[0178]

[0179] MnCe+NH4 shown in Table 5 + -ZSM-5 composites all had a mass ratio of the sum of manganese oxide and cerium oxide to zeolite of 1.5:1 and had the indicated molar ratios of Mn:Ce, were prepared by the gel-sol method according to the general procedure as described under II.3 above and had a calcination temperature of 300°C.

[0180] From the results shown in Table 5, it can be seen that the MnCe / NH4 +-ZSM-5 composites can show good low-temperature NOx conversion and better performance than MnCeO x Low N2O generation, where the molar ratio of Mn:Ce is 1:1 composite Mn / Ce / NH4 + -ZSM-5 is the best.

[0181] Table 6

[0182]

[0183] The composites or composite mixtures shown in Table 6 all have a mass ratio of the sum of manganese oxide and cerium oxide to zeolite of 1.5:1 and a molar ratio of Mn:Ce of 1:1, are prepared by the respective methods shown and have a calcination temperature of 300°C.

[0184] From the results shown in Table 6, it can be seen that the Mn / Ce / NH4 prepared by the sol-gel method + - ZSM-5 composite showed the lowest N2O generation among all samples. The sol-gel method is the best way to prepare the composite of manganese oxide, cerium oxide and zeolite according to the present invention.

[0185] V. Characterization Results

[0186] N2 adsorption and desorption

[0187] Composite Mn / Ce / NH4 for characterization of N2 adsorption and desorption + -ZSM-5 has a 1.5:1 ratio of the sum of manganese oxide and cerium oxide to NH4 + -ZSM-5 mass ratio and 1:1 Mn:Ce molar ratio, which was prepared by gel-sol method and calcined at 300°C. MnCeO x The quartz crystals were prepared by a gel-sol method with a molar ratio of Mn:Ce of 1:1.

[0188] The results are summarized in Table 7.

[0189] Table 7

[0190]

[0191] According to the analysis of N2 adsorption and desorption, MnCeO x Specific surface area (80m 2 g -1 ) after aging, it dropped significantly to 35m 2 g -1 For comparison, Mn / Ce / NH4 + -The specific surface area of ​​ZSM-5 (174m 2 g -1 ) after aging only dropped to 147m2 g -1 It should be noted that the composite Mn / Ce / NH4 + -ZSM-5 can maintain a high specific surface area after aging.

[0192] XRD analysis and SEM-EDS analysis

[0193] Composite Mn / Ce / NH4 for XRD analysis and SEM-EDS + -ZSM-5 has a 1.5:1 ratio of the sum of manganese oxide and cerium oxide to NH4 + -ZSM-5 mass ratio and 1:1 Mn:Ce molar ratio, which was prepared by gel-sol method and calcined at 300°C. MnCeO x The quartz crystals were prepared by a gel-sol method with a molar ratio of Mn:Ce of 1:1.

[0194] The XRD results are shown in Table 8 and Figure 1 In; SEM-EDS images are shown in Figure 2a and Figure 2b middle.

[0195] Table 8 CeO2

[111] grain size of fresh and aged samples

[0196]

[0197] Although the present invention has been described herein with reference to specific embodiments, it is to be understood that these embodiments are merely illustrative of the principles and applications of the present invention. It will be apparent to those skilled in the art that various modifications and variations may be made to the methods and apparatus of the present invention without departing from the spirit and scope of the present invention. Therefore, the present invention is intended to include modifications and variations within the scope of the appended claims and their equivalents.

Claims

1. An NH3-SCR catalyst comprising a composite of manganese oxide, cerium oxide and a molecular sieve, in particular consisting of a composite of manganese oxide, cerium oxide and a molecular sieve, wherein the molecular sieve is present in an amount of 20 wt % to 70 wt % based on the total weight of the composite.

2. The NH3-SCR catalyst according to claim 1, wherein the molecular sieve is present in the composite of manganese oxide, cerium oxide and molecular sieve in an amount of 20 to 50 wt%, more preferably 35 to 45 wt%, based on the total weight of the composite.

3. The NH3-SCR catalyst according to claim 1 or 2, wherein the manganese oxide and the cerium oxide are present in a molar ratio in the range of 4:1 to 1:4, preferably in the range of 7:3 to 3:7, more preferably in the range of 3:2 to 2:3, calculated as Mn and Ce elements. 4.The NH3-SCR 1 or 3-inch NH3-SCR system ABW, ACO, AEI, AE L、AEN、AET、AFG、AFI、AFN、AFO、AFR、AFS、AFT、AFV、AFX、AFY、AHT、ANA、APC、 APD、AST、ASV、ATN、ATO、ATS、ATT、ATV、AVL、AWO、AWW、BCT、BEA、BEC、BIK、BO F、BOG、BOZ、BPH、BRE、BSV、CAN、CAS、CDO、CFI、CGF、CGS、CHA、-CHI、-CLO、CO N、CSV、CZP、DAC、DDR、DFO、DFT、DOH、DON、EAB、EDI、EEI、EMT、EON、EPI、ERI、 ESV、ETR、EUO、*-EWT、EZT、FAR、FAU、FER、FRA、GIS、GIU、GME、GON、GOO、HEU、 IFO、IFR、-IFU、IFW、IFY、IHW、IMF、IRN、IRR、-IRY、ISV、ITE、ITG、ITH、*-IT N、ITR、ITT、-ITV、ITW、IWR、IWS、IWV、IWW、JBW、JNT、JOZ、JRY、JSN、JSR、JST 、JSW、KFI、LAU、LEV、LIO、-LIT、LOS、LOV、LTA、LTF、LTJ、LTL、LTN、MAR、MAZ 、MEI、MEL、MEP、MER、MFI、MFS、MON、MOR、MOZ、*MRE、MSE、MSO、MTF、MTN、MTT、 MTW、MVY、MWF、MWW、NAB、NAT、NES、NON、NPO、NPT、NSI、OBW、OFF、OKO、OSI、OS O、OWE、-PAR、PAU、PCR、PHI、PON、POS、PSI、PUN、RHO、-RON、RRO、RSN、RTE、RT H、RUT、RWR、RWY、SAF、SAO、SAS、SAT、SAV、SBE、SBN、SBS、SBT、SEW、SFE、SFF、 SFG、SFH、SFN、SFO、SFS、*SFV、SFW、SGT、SIV、SOD、SOF、SOS、SSF、*-SSO、SSY 、STF、STI、*STO、STT、STW、-SVR、SVV、SZR、TER、THO、TOL、TON、TSC、TUN、UEI 、UFI、UOS、UOV、UOZ、USI、UTL、UWY、VET、VFI、VNI、VSV、WEI、-WEN、YUGZON。 5. The NH3-SCR catalyst according to any one of claims 1 to 4, wherein the molecular sieve is selected from zeolites having the following framework types: AEI, AEL, AFI, AFT, AFO, AFX, AFR, ATO, BEA, CHA, DDR, EAB, EMT, ERI, EUO, FAU, FER, GME, HEU, JSR, KFI, LEV, LTA, LTL, LTN, MAZ, MEL, MFI, MOR, MOZ, MSO, MTW, MWW, OFF, RTH, SAS, SAT, SAV, SBS, SBT, SFW, SSF, SZR, TON, TSC and WEN.

6. The NH3-SCR catalyst according to claim 4 or 5, wherein the zeolite is in the respective H form, NH4 + form or a metal ion exchange form, such as a copper exchange form and / or an iron exchange form.

7. The NH3-SCR catalyst according to any one of claims 1 to 6, wherein the molecular sieve is a zeolite having a framework type selected from the group consisting of BEA (e.g. Beta), CHA (e.g. Chabazite), FAU (e.g. zeolite Y), FER (e.g. ferrierite), MFI (e.g. ZSM-5) and MOR (e.g. mordenite), preferably MFI (e.g. ZSM-5), more preferably NH4 + Form of MFI (e.g. ZSM-5).

8. The NH3-SCR catalyst according to any one of claims 1 to 7, wherein the composite of manganese oxide, cerium oxide and molecular sieve is prepared by a co-precipitation method or a sol-gel method, more preferably a sol-gel method.

9. A sol-gel process for preparing an NH3-SCR catalyst according to any one of claims 1 to 8, comprising the steps of (i) providing a suspension comprising a molecular sieve, a precursor of a manganese oxide and a precursor of a cerium oxide, (ii) heating the suspension to form a gel, and (iii) subjecting the gel to drying, grinding and calcining.

10. The sol-gel process according to claim 9, wherein the suspension in step (i) comprises an aqueous medium, preferably water.

11. A sol-gel process according to claim 9 or 10, wherein the suspension in step (i) comprises a complexing agent, such as citric acid.

12. The sol-gel process according to any one of claims 9 to 11, wherein the heating in step (ii) is carried out at a temperature of 70°C to 100°C.

13. The sol-gel process according to any one of claims 9 to 12, wherein the calcination in step (iii) is carried out at a temperature of 300°C to 500°C, such as 300°C or 400°C.

14. An NH3-SCR article comprising the NH3-SCR catalyst according to any one of claims 1 to 8 or the NH3-SCR catalyst obtained from the sol-gel process according to any one of claims 9 to 13.

15. The NH3-SCR article according to claim 14, which is in the form of a shaped body, such as an extrudate or a coated structure.

16. The NH3-SCR article according to claim 15, which is in the form of a pellet extrudate or a monolith extrudate.

17. The NH3-SCR article according to claim 15, which is in the form of a coated structure comprising the NH3-SCR catalyst in a coating layer on a substrate.

18. The NH3-SCR article according to claim 17, wherein the substrate is a monolithic flow-through structure or a monolithic wall-flow structure.

19. A method for treating exhaust gases containing nitrogen oxides by selective catalytic reduction, comprising contacting the exhaust gases with an NH3-SCR catalyst according to any one of claims 1 to 8, an NH3-SCR catalyst obtained from a sol-gel process according to any one of claims 9 to 13 or an NH3-SCR preparation according to any one of claims 14 to 18 in the presence of ammonia or an ammonia precursor as reducing agent.

20. An exhaust gas treatment system for a combustion engine, comprising a reductant source, an NH3-SCR article according to any one of claims 14 to 18 and optionally one or more of the following: a diesel oxidation catalyst (DOC), a three-way conversion catalyst (TWC), a four-way conversion catalyst (FWC), an uncatalyzed or catalyzed soot filter (CSF), an ammonia oxidation catalyst (AMOx), a NOx trap, a NOx absorber catalyst, a hydrocarbon trap catalyst, a sensor and a mixer.

21. The exhaust gas treatment system of claim 20, comprising a diesel oxidation catalyst located downstream of the engine and upstream of the NH3-SCR product.

22. An exhaust gas treatment system according to claim 20 or 21, comprising a diesel oxidation catalyst and a catalyzed soot filter located downstream of the engine and upstream of the NH3-SCR article.