Composite ferrous manganese sodium sulfate positive electrode material, preparation method thereof and sodium ion battery
Through the preparation method of composite ferrous manganese sodium sulfate positive electrode material, co-precipitation reaction and step-by-step calcination technology, the problem of low conductivity and density of the positive electrode material of sodium ion battery is solved, and the capacity and rate performance of the battery are significantly improved.
Patent Information
- Application Number
- CN202411188995.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
The ionic conductivity and compaction density of existing sodium ion battery cathode materials are low, which affects its capacity and rate performance.
The preparation method of composite ferrous manganese sodium sulfate positive electrode material is adopted, and the sulfate ions are introduced through co-precipitation reaction and step-by-step calcination technology and carbon coating is achieved using a carbon source to enhance the ionic conductivity and compaction density of the material.
The ionic conductivity and compaction density of the composite ferrous manganese sulfate positive electrode material are significantly improved, and the capacity and rate performance of sodium ion batteries are improved.
Smart Images

Figure CN119059568A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sodium ion batteries, and in particular to a composite sodium ferrous manganese sulfate positive electrode material and a preparation method thereof, and a sodium ion battery. Background Art
[0002] At present, the research on positive electrode materials of sodium ion batteries mainly focuses on polyanionic materials. Among the many polyanionic compounds, SO4 2- With higher electronegativity and stronger inductive effect, the prepared sulfate materials have higher working voltage and thus receive more extensive attention. For example, Na2Fe2(SO4)3 material has a higher charge and discharge platform (3.8V) than LiFePO4 material. However, Na2Fe2(SO4)3 material has the defects of low sodium ion diffusion coefficient and low electronic conductivity. Low sodium ion diffusion coefficient leads to low ion conductivity of positive electrode material, which affects the migration and diffusion ability of sodium ions in positive electrode material, and then leads to low capacity and rate performance of positive electrode material. Low electronic conductivity leads to low transmission efficiency of electrons during charge and discharge.
[0003] In the prior art, carbon coating is usually used to improve the electronic conductivity of the positive electrode material, and metal or transition metal is doped to improve the sodium ion diffusion coefficient of the positive electrode material. Among them, the conventional doping method cannot obtain sodium ferrous sulfate positive electrode material in order to avoid the decomposition of sulfate ions. The sintering temperature of sodium ferrous sulfate positive electrode material is relatively low, resulting in a very low degree of mutual migration and fusion between metal ions. Therefore, the ionic conductivity of the positive electrode material is limited after doping. At the same time, the low sintering temperature will also lead to a low compaction density of the positive electrode material, thereby affecting the capacity and rate performance of the positive electrode material.
[0004] Therefore, there is an urgent need to provide a method for preparing a sodium ferrous sulfate positive electrode material to simultaneously improve the ionic conductivity and compaction density of the prepared sodium ferrous sulfate positive electrode material. Summary of the invention
[0005] In view of the technical problems existing in the background technology, the present application provides a composite sodium manganese ferrous sulfate positive electrode material and a preparation method thereof and a sodium ion battery, aiming to solve the problem of how to simultaneously improve the ionic conductivity and compaction density of the sodium manganese ferrous sulfate positive electrode material.
[0006] In the first aspect, the embodiment of the present application provides a method for preparing a composite sodium ferrous manganese sulfate positive electrode material, comprising the following steps: using manganese salt, ferrous salt, and dopant as raw materials, adding a reducing agent and an oxalic acid compound in sequence, and obtaining doped manganese iron oxalate through reaction; mixing the doped manganese iron oxalate with a sodium salt, and obtaining doped sodium ferromanganate after a first dispersion and a first calcination; adding a carbon source and a solvent to the doped sodium ferromanganate and performing a second dispersion, and then adding a sulfate-containing compound and a flux, and obtaining a spray-dried material through spray drying; calcining the spray-dried material for a second time, and then adding a sodium supplement, and after crushing and impurity removal, obtaining a composite sodium ferrous manganese sulfate positive electrode material; wherein the temperature of the first calcination is 750-900°C.
[0007] In the technical solution of the embodiment of the present application, iron, manganese, sodium metal ions and dopants are first melted together by coprecipitation reaction and primary calcination treatment to obtain doped sodium ferromanganate, and then sulfate ions are introduced by secondary calcination. At the same time, carbon coating of the positive electrode material is achieved by using a carbon source to prepare a composite sodium ferrous manganese sulfate positive electrode material. In the present application, the composite sodium ferrous manganese sulfate positive electrode material prepared by the above preparation method can simultaneously achieve the improvement of the ionic conductivity and compaction density of the positive electrode material.
[0008] In some embodiments, the dopant includes one or more of a soluble magnesium salt, an aluminum salt, a nickel salt, or a cobalt salt.
[0009] In this embodiment, the selected dopant is uniformly doped into the ferromanganese oxalate generated by the coprecipitation reaction to obtain doped ferromanganese oxalate, which is beneficial to improving the ionic conductivity of the prepared composite sodium manganese ferrous sulfate positive electrode material.
[0010] In some embodiments, the reducing agent includes one or more of ascorbic acid, sodium thiosulfate, sodium metabisulfite.
[0011] In this embodiment, the selected reducing agent is helpful to prevent the oxidation of ferrous salt and manganese salt, ensuring that the iron and manganese in the ferrous salt and manganese salt maintain a +2 valence, so as to achieve charge balance in the doped ferromanganese oxalate.
[0012] In some embodiments, the oxalate compound includes one or more of ammonium oxalate, oxalic acid, and sodium oxalate.
[0013] In this embodiment, the oxalic acid compound is selected as a precipitant, and the provided oxalate ions are co-precipitated with metal ions to obtain doped manganese ferrooxalate.
[0014] In some embodiments, the molar ratio of manganese ions in the manganese salt, ferrous ions in the ferrous salt, and metal ions in the dopant is 1:(2-4):(0.1-0.2).
[0015] In this embodiment, within the above range, the raw materials react more fully without causing waste of raw materials.
[0016] In some embodiments, the molar ratio of the reducing agent to the ferrous ions in the ferrous salt is (0.05-0.1):1.
[0017] In this embodiment, if the reducing agent is too little, it is insufficient to provide an anti-oxidation environment for the ferrous salt and the manganese salt, and if the reducing agent is too much, the raw materials are wasted.
[0018] In some embodiments, the ratio of the molar amount of the oxalic acid compound to the total molar amount of the manganese ions in the manganese salt, the ferrous ions in the ferrous salt, and the metal ions in the dopant is (1.1-1.25):1.
[0019] In this embodiment, if the amount of the oxalic acid compound used is too little, it will not be enough to precipitate all the metal ions, and if the amount of the oxalic acid compound used is too much, the raw materials will be wasted.
[0020] In some embodiments, the primary calcination is performed in an atmosphere with an oxygen volume concentration of ≥ 19%.
[0021] In this embodiment, sufficient oxygen is provided in the first calcination so that the divalent manganese ions and the divalent iron ions are fully oxidized to trivalent oxidation states, thereby causing the metal ions in sodium, manganese, iron and the dopant to co-melt in an oxidized state to form doped sodium ferromanganate. If the oxygen content is insufficient, the divalent manganese ions and the divalent iron ions cannot be completely oxidized. Understandably, since the thermal decomposition of oxalate produces reducing gases such as carbon monoxide, it is difficult for the metal ions in sodium, manganese, iron and the dopant to co-melt in an oxidized state to form doped sodium ferromanganate, resulting in excessive impurities in the product.
[0022] In some embodiments, the ratio of the total molar amount of metal ions in the doped ferromanganese oxalate to the molar amount of sodium ions in the sodium salt is 1:(1.03-1.1).
[0023] In this embodiment, if the amount of sodium salt used is too small, the reaction is incomplete, and the prepared doped sodium ferromanganate is less, which in turn leads to a low yield of the prepared composite sodium ferrous manganese sulfate positive electrode material; and if the amount of sodium salt used is too large, the raw materials are wasted and the process cost is increased.
[0024] In some embodiments, the sodium salt includes at least one of sodium acetate, sodium nitrate, sodium citrate, and sodium chloride.
[0025] In this embodiment, the sodium salt selected has a wide range of sources, which is beneficial to cost control.
[0026] In some embodiments, the mass ratio of doped sodium ferromanganate, solvent, and carbon source is 1:(3-5):(0.1-0.15).
[0027] In this embodiment, under the above-mentioned dosage limit, uniform coating of the carbon source can be achieved, which is beneficial to improve the conductivity of the prepared composite sodium manganese ferrous sulfate positive electrode material.
[0028] In some embodiments, the sulfate-containing compound is a mixture of ammonium sulfate and sodium sulfite, and the flux is sodium borate, wherein the molar ratio of ammonium sulfate, sodium sulfite, sodium borate and doped sodium ferromanganate is (4.5-5.5):(0.9-1.1):(0.05-0.1):1.
[0029] In this embodiment, the sulfate compound selected provides sulfate for anion conversion to improve the ionic conductivity of the product. In addition, sulfite can also play a reducing role to reduce the oxidized iron and manganese to +2 valence; the flux can lower the melting point of the material to improve the density and compaction density of the product. The use of sodium borate as a flux in this application is more conducive to improving the ionic conductivity of the product than using only cation doping. At the same time, the molar mass of borate is lower than that of sulfate, which is also beneficial to improving the capacity of the positive electrode material.
[0030] In some embodiments, manganese salt, ferrous salt, and dopant are used as raw materials, and a reducing agent and an oxalic acid compound are added in sequence to obtain doped manganese ferrooxalate through reaction. The pH value during the reaction is 4-4.5, the temperature is 40-60°C, the addition time of the oxalic acid compound and the reducing agent is 30-60min, and the reaction time is 30-60min.
[0031] In this embodiment, the pH value of the coprecipitation reaction is adjusted by ammonium bicarbonate and / or sodium bicarbonate.
[0032] In some embodiments, the spray drying temperature is 120-180°C.
[0033] In this embodiment, under the definition of the present application, the solvent is completely evaporated to achieve uniform mixing of the materials. If the temperature is lower than this, the solvent will not evaporate completely, and if the temperature is higher than this, energy will be wasted.
[0034] In some embodiments, the secondary calcination temperature is 300-350°C.
[0035] In this embodiment, if the secondary calcination temperature is too low, it is not conducive to the formation of the carbon layer, and it is also difficult to achieve complete conversion of anions. If the secondary calcination temperature is too high, it will lead to the decomposition of sulfate during the sintering process.
[0036] In some embodiments, the mass ratio of the calcined material obtained by the secondary calcination to the sodium supplement is 1:(0.02-0.03).
[0037] In this embodiment, the sodium supplementer plays a role in replenishing sodium ions during the first charge and discharge process of the positive electrode material, because during the first charging process, sodium ions will form an SEI film at the negative electrode, thereby consuming sodium ions, resulting in insufficient sodium ions during discharge and low coulomb efficiency. The sodium supplementer can supplement the sodium capacity loss of the positive electrode material. If the amount of the sodium supplementer is too much, because the sodium supplementer has no cycle performance, if the amount of the sodium supplementer is too much, the excess sodium cannot be completely returned to the positive electrode, and the sodium supplementer will account for the mass of the positive electrode material, resulting in low cycle performance, low capacity and excessive residual sodium supplementer. The influence of other performances of the battery, and if the amount of the sodium supplementer is too little, the capacity of the battery will decrease.
[0038] In some embodiments, the sodium supplement comprises sodium oxalate.
[0039] In this embodiment, sodium oxalate is selected as the sodium supplement because of its high stability and ease of storage and transportation.
[0040] In the second aspect, the embodiment of the present application provides a composite sodium ferrous manganese sulfate positive electrode material, and the ionic conductivity of the composite sodium ferrous manganese sulfate positive electrode material is 3.0×10 -6 -10.0×10 -6 S / cm, and the compaction density of the composite sodium ferrous manganese sulfate positive electrode material is 2.30-2.45g / mL.
[0041] In the technical solution of the embodiment of the present application, the composite sodium manganese ferrous sulfate positive electrode material has high ionic conductivity and large compaction density, which is beneficial to improving the capacity and rate performance of the sodium ion battery prepared using the positive electrode material.
[0042] In a third aspect, an embodiment of the present application provides a sodium ion battery comprising a composite sodium ferrous manganese sulfate positive electrode material.
[0043] In this embodiment, the sodium ion battery contains the above-mentioned composite sodium manganese ferrous sulfate positive electrode material, and thus has the advantages of high capacity and good rate performance.
[0044] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] In order to more clearly illustrate the technical solution of the present application, the following is a brief introduction to the drawings used in the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0046] Figure 1 A schematic diagram of the process for preparing the composite sodium manganese ferrous sulfate positive electrode material provided in this application;
[0047] Figure 2 This is a SEM image of the doped ferromanganese oxalate in Example 1;
[0048] Figure 3 This is a SEM image of the doped sodium ferromanganate in Example 1;
[0049] Figure 4 This is the SEM image of the spray-dried material in Example 1;
[0050] Figure 5 This is a SEM image of the composite sodium manganese ferrous sulfate positive electrode material in Example 1;
[0051] Figure 6 The charge and discharge curve of the secondary battery prepared with the positive electrode material of Example 1;
[0052] Figure 7 The charge and discharge curves of the secondary battery prepared with the positive electrode material of Example 2. DETAILED DESCRIPTION
[0053] The following embodiments of the technical solution of the present application will be described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0054] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.
[0055] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0056] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0057] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0058] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0059] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.
[0060] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.
[0061] At present, Na2Fe2(SO4)3 material has the defects of low ionic conductivity and electronic conductivity. In order to improve the above defects of Na2Fe2(SO4)3 material, relevant technicians improve electronic conductivity by carbon coating and improve ionic conductivity by doping metals or transition metals. Among them, in the conventional doping method, the doped metal salt and iron salt are generally mixed and ground first, and then the mixture is sintered. In order to prevent the decomposition of the necessary raw material sulfate, the sintering temperature cannot exceed 350°C. However, when the sintering temperature is lower than 350°C, the mutual migration and fusion degree between metal ions is very low. Therefore, the ionic conductivity of the material is limited after doping. At the same time, the low sintering temperature will also lead to low compaction density of the prepared positive electrode material, which will affect the capacity and rate performance of the secondary battery prepared using the positive electrode material.
[0062] In view of the above technical problems, the present application provides a composite sodium ferrous manganese sulfate positive electrode material and a preparation method thereof and a sodium ion battery, aiming to solve the problem of how to simultaneously improve the ionic conductivity and compaction density of the sodium ferrous sulfate positive electrode material.
[0063] First, as Figure 1 As shown, the present application embodiment provides a method for preparing a composite sodium ferrous manganese sulfate positive electrode material, comprising the following steps:
[0064] S1. Using manganese salt, ferrous salt and doping agent as raw materials, adding reducing agent and oxalic acid compound in sequence, and obtaining doped manganese ferrooxalate through reaction;
[0065] S2, mixing the doped ferromanganese oxalate with sodium salt, dispersing once and calcining once to obtain doped sodium ferromanganate;
[0066] S3, adding a carbon source and a solvent to the doped sodium ferromanganate and performing secondary dispersion, then adding a sulfate-containing compound and a flux, and spray drying to obtain a spray-dried material;
[0067] S4, calcining the spray-dried material twice, then adding a sodium supplement, and crushing and removing impurities to obtain a composite sodium ferrous manganese sulfate positive electrode material;
[0068] The primary calcination temperature is 750-900°C.
[0069] In the technical solution of the embodiment of the present application, a coprecipitation reaction and a primary calcination are first used to co-melt iron, manganese, sodium metal ions and a dopant to obtain doped sodium ferromanganate, and then a secondary calcination is performed to convert anions to introduce sulfate ions, and at the same time, a carbon source is used to achieve carbon coating of the positive electrode material to obtain a composite sodium ferrous manganese sulfate positive electrode material.
[0070] Specifically, the process and principle of the present application are as follows: first, through a coprecipitation reaction, the metal ions of manganese, iron, and dopant are formed into a uniform doped ferromanganese oxalate; secondly, at a high temperature of 750-900°C, the doped ferromanganese oxalate is mixed with a sodium salt, and after a dispersion and a calcination, a doped sodium ferromanganate is obtained, that is, a eutectic of sodium manganese iron oxide is formed, thereby effectively improving the ionic conductivity of the material. In this process, if the temperature of the first calcination is too low, a eutectic cannot be formed; further, a carbon source, a sulfate-containing compound, and a flux are added to the prepared doped sodium ferromanganate, and a spray-dried material is obtained by spray drying; finally, a secondary calcination is performed at a lower temperature to achieve anion conversion of the positive electrode material and form a carbon coating layer, so as to obtain a composite sodium ferrous manganese sulfate positive electrode material.
[0071] The above process has the following advantages: (1) by calcining in steps, a eutectic is formed first and then sulfate is introduced, which solves the contradiction between the high eutectic temperature of the doped metal and the low decomposition temperature of the sulfate, ensures that the sulfate is not decomposed, and at the same time improves the co-doping effect of the prepared composite sodium ferrous manganese sulfate positive electrode material, and the mutual migration and fusion degree between the metal ions are high, which is beneficial to improve the ion conductivity of the prepared composite sodium ferrous manganese sulfate positive electrode material; (2) the first calcination (750-900°C) is a high-temperature calcination, which is beneficial to the formation of a metal ion eutectic and the improvement of the compaction density of the prepared composite sodium ferrous manganese sulfate positive electrode material; (3) by spray drying, carbon coating is also achieved while mixing, which is beneficial to the improvement of the electronic conductivity of the prepared composite sodium ferrous manganese sulfate positive electrode material.
[0072] Further, in some embodiments, the dopant includes one or more of soluble magnesium salts, aluminum salts, nickel salts or cobalt salts; for example, one or more of magnesium sulfate, aluminum sulfate, nickel sulfate, and cobalt sulfate.
[0073] In this embodiment, the selected dopant is uniformly doped in the ferromanganese oxalate generated by the coprecipitation reaction to obtain doped ferromanganese oxalate, which is beneficial to improve the ionic conductivity of the prepared composite sodium ferrous manganese sulfate positive electrode material, and further helps to improve the sodium ion deintercalation rate in the prepared composite sodium ferrous manganese sulfate positive electrode material, thereby achieving an improvement in the capacity and rate performance of the positive electrode material.
[0074] Further, in some embodiments, the reducing agent includes one or more of ascorbic acid, sodium thiosulfate, and sodium metabisulfite.
[0075] In this embodiment, the selected reducing agent is helpful to prevent the oxidation of ferrous salt and manganese salt, ensuring that the iron and manganese in the ferrous salt and manganese salt maintain a +2 valence, so as to achieve charge balance in the doped ferromanganese oxalate.
[0076] Furthermore, in some embodiments, the oxalate compound includes one or more of ammonium oxalate, oxalic acid, and sodium oxalate.
[0077] In this embodiment, the oxalic acid compound is selected as a precipitant, and the provided oxalate ions are co-precipitated with metal ions to obtain doped manganese ferrooxalate.
[0078] Further, in some embodiments, the molar ratio of manganese ions in the manganese salt, ferrous ions in the ferrous salt, and metal ions in the dopant is 1:(2-4):(0.1-0.2).
[0079] Specifically, the molar ratio of manganese ions in the manganese salt, ferrous ions in the ferrous salt, and metal ions in the dopant can be any value between 1:2:0.1, 1:2:0.2, 1:4:0.1, 1:4:0.2, 1:3:0.1, 1:3:0.2, 1:2:0.15 or 1:(2-4):(0.1-0.2). In this embodiment, within the above range, the raw materials react more fully without causing waste of raw materials.
[0080] Further, in some embodiments, the molar ratio of the reducing agent to the ferrous ions in the ferrous salt is (0.05-0.1):1.
[0081] Specifically, the molar ratio of the reducing agent to the ferrous ions in the ferrous salt can be any value between 0.05:1, 0.08:1, 0.1:1 or (0.05-0.1): 1. In this embodiment, if the reducing agent is too little, it is insufficient to provide an antioxidant environment for the ferrous salt and the manganese salt, and if the reducing agent is too much, the raw materials are wasted.
[0082] Furthermore, in some embodiments, the ratio of the molar amount of the oxalic acid compound to the total molar amount of the manganese ions in the manganese salt, the ferrous ions in the ferrous salt, and the metal ions in the dopant is (1.1-1.25):1.
[0083] Specifically, the ratio of the molar amount of the oxalic acid compound to the total molar amount of the manganese ions in the manganese salt, the ferrous ions in the ferrous salt, and the metal ions in the dopant can be 1.1:1, 1.2:1, 1.25:1, or any value between (1.1-1.25): 1. In this embodiment, if the amount of the oxalic acid compound is too small, it is insufficient to precipitate all the metal ions, and if the amount of the oxalic acid compound is too large, the raw material is wasted.
[0084] Furthermore, in some embodiments, the primary calcination is performed in an atmosphere with an oxygen volume concentration of ≥19%.
[0085] Specifically, the primary calcination can be carried out in an atmosphere with an oxygen volume concentration of 19%, 30%, 50% or 100%. In this embodiment, sufficient oxygen is provided in the primary calcination so that the divalent manganese ions and the divalent iron ions are fully oxidized to trivalent oxidation states, thereby allowing the metal ions in sodium, manganese, iron and the dopant to be eutectic in an oxidized state to form doped sodium ferromanganate. If the oxygen content is insufficient, the manganese iron cannot be completely oxidized. Understandably, the oxalate decomposes under heat to produce reducing gases such as carbon monoxide, which makes it difficult for the metal ions in sodium, manganese, iron and the dopant to be eutectic in an oxidized state to form doped sodium ferromanganate, thereby causing excessive impurities in the product.
[0086] Furthermore, in some embodiments, the ratio of the total molar amount of metal ions in the doped ferromanganese oxalate to the molar amount of sodium ions in the sodium salt is 1:(1.03-1.1).
[0087] Specifically, the ratio of the total molar amount of metal ions in the doped ferromanganese oxalate to the molar amount of sodium ions in the sodium salt can be 1:1.03, 1:1.05, 1:1.1 or any value between 1:(1.03-1.1). In this embodiment, if the amount of sodium salt is too little, the reaction is incomplete, the prepared doped sodium ferromanganate is less, and the yield of the prepared composite sodium ferromanganese sulfate positive electrode material is low; if the amount of sodium salt is too much, the raw materials are wasted and the process cost is increased.
[0088] Further, in some embodiments, the sodium salt includes at least one of sodium acetate, sodium nitrate, sodium citrate, and sodium chloride.
[0089] In this embodiment, the sodium salt selected has a wide range of sources, which is beneficial to cost control.
[0090] Furthermore, in some embodiments, the mass ratio of doped sodium ferromanganate, solvent and carbon source is 1:(3-5):(0.1-0.15).
[0091] Specifically, the mass ratio of doped sodium ferromanganate, solvent and carbon source can be any value between 1:3:0.1, 1:3:0.15, 1:5:0.1, 1:5:0.15, 1:4:0.12, 1:4:0.1 or 1:(3-5):(0.1-0.15). In this embodiment, under the above-mentioned dosage limit, uniform coating of the carbon source can be achieved. If the carbon source is too little, the coating degree is low. If the carbon source is too much, the coating layer is too thick, causing ion diffusion to be blocked, which is not conducive to the improvement of the ionic conductivity of the prepared composite sodium ferromanganese sulfate positive electrode material.
[0092] Further, in some embodiments, the sulfate-containing compound is a mixture of ammonium sulfate and sodium sulfite, and the flux is sodium borate, wherein the molar ratio of ammonium sulfate, sodium sulfite, sodium borate and doped sodium ferromanganate is (4.5-5.5): (0.9-1.1): (0.05-0.1): 1;
[0093] Specifically, the molar ratio of ammonium sulfate, sodium sulfite, sodium borate and doped sodium ferromanganate is 4.5:0.9:0.05:1, 5.5:0.9:0.05:1, 4.5:1.1:0.05:1, 4.5:0.9:0.1:1 or any value between (4.5-5.5):(0.9-1.1):(0.05-0.1):1.
[0094] In this embodiment, the sulfate compound selected provides sulfate for anion conversion to improve the ionic conductivity of the product. In addition, sulfite can also play a reducing role, reducing trivalent iron and trivalent manganese to divalent. It is understandable that if only sulfate is selected, trivalent iron and trivalent manganese cannot be reduced to divalent values. If only sulfite is selected, the amount of sulfate provided for anion conversion is insufficient. Further, the flux can reduce the melting point of the material to improve the density and compaction density of the product. The present application uses sodium borate as a flux, which is more conducive to improving the ionic conductivity of the product compared to using only cation doping. At the same time, the molar mass of borate is lower than that of sulfate, which is also conducive to improving the capacity of the positive electrode material.
[0095] Furthermore, in some embodiments, manganese salt, ferrous salt, and dopant are used as raw materials, and a reducing agent and an oxalic acid compound are added in sequence to obtain doped manganese ferrooxalate through reaction. The pH value during the reaction is 4-4.5, the temperature is 40-60°C, the addition time of the oxalic acid compound and the reducing agent is 30-60min, and the reaction time is 30-60min.
[0096] Specifically, the pH value during the reaction can be 4, 4.1, 4.2, 4.3, 4.4, 4.5 or any value between 4-4.5, the temperature during the reaction can be 40°C, 45°C, 50°C, 55°C, 60°C or any value between 40-60°C, the addition time of the oxalic acid compound and the reducing agent can be 30min, 40min, 50min, 60min or any value between 30-60min, and the reaction time can be 30min, 40min, 50min, 60min or any value between 30-60min. The pH value of the coprecipitation reaction is adjusted by ammonium bicarbonate and / or sodium bicarbonate.
[0097] Further, in some embodiments, the spray drying temperature is 120-180°C.
[0098] Specifically, the spray drying temperature can be 120° C., 130° C., 150° C., 180° C. or any value between 120-180° C. Under the definition of the present application, complete evaporation of the solvent can achieve uniform mixing of the dried materials. If the temperature is lower than this, the solvent will not evaporate completely, and if the temperature is higher than this, energy will be wasted.
[0099] Furthermore, in the process of spray drying, hot nitrogen is used as a heat source, the temperature of the hot nitrogen is 200-300°C, and at the same time, the speed of the atomizing wheel is controlled so that the particle size of the spray-dried material is 3-10μm, and the discharge temperature is controlled to be ≤80°C, and the material is sent to a subsequent calcining furnace through a pipeline conveyor for secondary calcination treatment.
[0100] Furthermore, in some embodiments, the secondary calcination temperature is 300-350°C.
[0101] Specifically, the temperature of the secondary calcination can be 300° C., 310° C., 320° C., 330° C., 340° C., 350° C. or any value between 300-350° C. In this embodiment, if the secondary calcination temperature is too low, it is not conducive to the coating of the carbon layer, and it is difficult to achieve complete conversion of anions. If the secondary calcination temperature is too high, it will lead to the decomposition of sulfate during the sintering process.
[0102] Furthermore, in some embodiments, the mass ratio of the calcined material to the sodium supplement is 1:(0.02-0.03).
[0103] Specifically, the mass ratio of the calcined material to the sodium supplement agent can be 1:0.02, 1:0.025, 1:0.03 or any value between 1:(0.02-0.03).
[0104] In this embodiment, the sodium supplementer plays a role in replenishing sodium ions during the first charge and discharge process of the positive electrode material. During the first charging process, sodium ions will form an SEI film at the negative electrode, thereby consuming sodium ions, resulting in insufficient sodium ions during discharge and low coulomb efficiency. The sodium supplementer can supplement the sodium capacity loss of the positive electrode material. If the amount of the sodium supplementer is too much, because the sodium supplementer has no cycle performance, if the amount of the sodium supplementer is too much, the excess sodium cannot be completely returned to the positive electrode, and the sodium supplementer will account for the mass of the positive electrode material, resulting in low cycle performance, low capacity and excessive residual sodium supplementer. The influence of other performances of the battery, and if the amount of the sodium supplementer is too little, the capacity of the battery will decrease.
[0105] Furthermore, in some embodiments, the sodium supplement includes sodium oxalate.
[0106] In this embodiment, sodium oxalate is selected as the sodium supplement because of its high stability and ease of storage and transportation.
[0107] In the second aspect, the embodiment of the present application provides a composite sodium ferrous manganese sulfate positive electrode material, and the ionic conductivity of the composite sodium ferrous manganese sulfate positive electrode material is 3.0×10 -6 -10.0×10 -6 S / cm, and the compacted density is 2.30-2.45 g / mL.
[0108] In the technical solution of the embodiment of the present application, the composite sodium manganese ferrous sulfate positive electrode material has high ionic conductivity and high compaction density, which is beneficial to improving the capacity and rate performance of the battery.
[0109] In a third aspect, an embodiment of the present application provides a sodium battery comprising a composite sodium ferrous manganese sulfate positive electrode material.
[0110] In this embodiment, the sodium battery includes the above-mentioned composite sodium manganese ferrous sulfate positive electrode material, and thus has the advantages of high capacity and good rate performance.
[0111] Some specific embodiments are listed below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be obtained commercially.
[0112] 1. Preparation method
[0113] Example 1
[0114] A method for preparing a composite sodium ferrous manganese sulfate positive electrode material comprises the following steps:
[0115] (1) Manganese sulfate, ferrous sulfate and nickel sulfate are used as raw materials and mixed in a molar ratio of 1:3:0.15, and pure water is added to dissolve to obtain a salt solution with a mass concentration of 23%, and then ascorbic acid with a molar amount of 0.08 times that of ferrous sulfate is added to the salt solution, and then 1.2 mol / L ammonium oxalate is added to carry out a coprecipitation reaction; wherein the molar amount of ammonium oxalate is 1.2 times the total molar amount of manganese sulfate, ferrous sulfate and nickel sulfate. During the coprecipitation process, the pH of the reaction solution is stabilized at 4.2 by adding ammonium bicarbonate, the temperature is 50°C, and the ammonium oxalate addition time is 45 minutes. After the ammonium oxalate solution is added, the reaction is stirred for 50 minutes, and then filtered, washed and dried to obtain doped manganese ferrooxalate. Specifically, the SEM image of doped manganese ferrooxalate is as follows: Figure 2 The performance test data of doped ferromanganese oxalate are shown in Table 1.
[0116] (2) Sodium acetate is added to the doped ferromanganese oxalate in an amount such that the ratio of the total molar amount of metal ions in the doped ferromanganese oxalate to the molar amount of sodium ions in the sodium salt is 1:1.06, and after ball milling to a particle size of 2.7 μm, the material is placed in a rotary kiln and calcined once at 820°C for 8 hours. At the same time, air is introduced into the rotary kiln to maintain the oxygen volume concentration in the atmosphere in the rotary kiln at 19.8%, and then the material is cooled to a temperature of ≤80°C by a cooling screw conveyor and then conveyed out to obtain doped sodium ferromanganate. Specifically, the SEM image of doped sodium ferromanganate is as follows: Figure 3 The performance test data of doped sodium ferromanganate are shown in Table 2.
[0117] (3) Add doped sodium ferromanganate to pure water and nanographite sheets, and the mass ratio of doped sodium ferromanganate, pure water and nanographite is 1:4:0.12. Put the above mixture into a sand mill and sand grind it to a particle size of 146nm. Then add ammonium sulfate and sodium sulfite to the sand-milled slurry. The molar ratio of the added ammonium sulfate, sodium sulfite, sodium borate and sodium ferromanganate is 5:1:0.07:1. After stirring and dissolving and mixing evenly, spray drying is performed. Hot nitrogen is used as a heat source in the spray drying process. The temperature of the hot nitrogen is 250°C. The speed of the atomizing wheel is controlled so that the particle size of the final spray-dried material is 7.5μm. The discharge temperature is controlled to be ≤80°C to obtain a spray-dried material. Specifically, the SEM image of the spray-dried material is as follows: Figure 4 shown.
[0118] (4) The spray-dried material is conveyed to a calcining furnace through a pipeline conveyor. The secondary calcination is carried out in a roller furnace with nitrogen as the protective atmosphere. The heating rate in the heating stage is 1.5°C / min, and the temperature in the insulation stage is 330°C for 18 hours. The cooling rate is then 1.5°C / min. The material is discharged after cooling to a temperature ≤70°C. The material is then mixed with sodium oxalate and crushed in a pulverizer. The mass ratio of the calcined material to the mixed sodium oxalate is 1:0.025. The material is crushed in an air flow pulverizer until the particle size of the material is 1.8 μm. The material is then screened, iron removed, and vacuum packaged in a packaging room. The temperature in the packaging room is 25±5°C and the humidity is ≤10%. The composite sodium ferrous manganese sulfate positive electrode material is obtained. The SEM image of the composite sodium ferrous manganese sulfate positive electrode material is as shown in FIG. Figure 4 As shown, the performance test data of the composite sodium ferrous manganese sulfate positive electrode material is shown in Table 3.
[0119] Table 1 Performance test data of doped ferromanganese oxalate
[0120]
[0121] Table 2 Performance test data of doped sodium ferromanganate
[0122]
[0123] Table 3 Performance test data of composite sodium ferrous manganese sulfate positive electrode material
[0124]
[0125] Example 2
[0126] A method for preparing a composite sodium ferrous manganese sulfate positive electrode material comprises the following steps:
[0127] (1) manganese chloride, ferrous chloride and nickel sulfate are mixed as raw materials in a molar ratio of 1:4:0.1, and pure water is added to dissolve them to obtain a salt solution with a mass concentration of 23%, and then ascorbic acid with a molar amount of 0.05 times that of ferrous chloride is added to the salt solution, and then 1.25 mol / L of ammonium oxalate is added to carry out a coprecipitation reaction; wherein the molar amount of ammonium oxalate is 1.2 times the total molar amount of manganese chloride, ferrous chloride and nickel sulfate. During the coprecipitation process, the pH of the reaction solution is stabilized at 4 by adding ammonium bicarbonate, the temperature is 40°C, the ammonium oxalate addition time is 60 minutes, and after the ammonium oxalate solution is added, the stirring reaction is continued for 30 minutes, and then filtered, washed and dried to obtain doped manganese iron oxalate;
[0128] (2) Sodium acetate is added to the doped ferromanganese oxalate in an amount such that the total molar amount of metal ions in the doped ferromanganese oxalate is 1:1.03 to the molar amount of sodium ions in the sodium salt, and the material is ball-milled to a particle size of 2.75 μm, and then placed in a rotary kiln for calcination at 900° C. for 6 hours, while air is introduced into the rotary kiln to maintain the oxygen volume concentration in the atmosphere in the rotary kiln at 19.8%, and then cooled to a material temperature of ≤80° C. by a cooling screw conveyor and then conveyed out to obtain doped sodium ferromanganate.
[0129] (3) adding doped sodium ferromanganate to pure water and nanographite sheets, wherein the mass ratio of doped sodium ferromanganate, pure water and nanographite is 1:5:0.15, placing the mixture into a sand mill, sand grinding the mixture to a particle size of 198 nm, and then adding ammonium sulfate and sodium sulfite to the sand-milled slurry, wherein the molar ratio of the added ammonium sulfate, sodium sulfite, sodium borate and sodium ferromanganate is 5.5:1.1:0.1:1, stirring and dissolving the mixture evenly, and then spray drying. In the spray drying process, hot nitrogen is used as a heat source, the temperature of the hot nitrogen is 300° C., the speed of the atomizing wheel is controlled so that the particle size of the final spray-dried material is 10 μm, and the discharge temperature is controlled to be ≤80° C. to obtain a spray-dried material;
[0130] (4) The spray-dried material is conveyed to a calcining furnace through a pipeline conveyor. The secondary calcination is carried out in a roller furnace with nitrogen as the protective atmosphere. The heating rate of the heating section is 2°C / min, and then the temperature of the insulation section is 300°C for 20 hours. Then the cooling rate is 2°C / min. After cooling to a temperature ≤70°C, the material is discharged and then mixed with sodium oxalate and crushed in a pulverizer. The mass ratio of the calcined material to the mixed sodium oxalate is 1:0.03. The pulverization is carried out by a jet mill. The material is crushed to a particle size of 2.4 μm and then stopped. Then, the material is screened, iron removed, and vacuum packaged in a packaging room. The temperature of the packaging room is 25±5°C and the humidity is ≤10%. The composite sodium ferrous manganese sulfate positive electrode material is obtained. The performance test data of the composite sodium ferrous manganese sulfate positive electrode material in Example 2 are shown in Table 4.
[0131] Table 4 Performance test data of composite sodium ferrous manganese sulfate positive electrode material
[0132]
[0133] Example 3
[0134] A method for preparing a composite sodium ferrous manganese sulfate positive electrode material comprises the following steps:
[0135] (1) manganese chloride, ferrous chloride and nickel sulfate are mixed as raw materials in a molar ratio of 1:2:0.2, and pure water is added to dissolve them to obtain a salt solution with a mass concentration of 23%, and then ascorbic acid with a molar amount of 0.1 times that of ferrous chloride is added to the salt solution, and then 1.25 mol / L of ammonium oxalate is added to carry out a coprecipitation reaction; wherein the molar amount of ammonium oxalate is 1.1 times the total molar amount of manganese chloride, ferrous chloride and nickel sulfate. During the coprecipitation process, the pH of the reaction solution is stabilized at 4 by adding ammonium bicarbonate, the temperature is 40°C, the ammonium oxalate addition time is 60 minutes, and after the ammonium oxalate solution is added, the stirring reaction is continued for 30 minutes, and then filtered, washed and dried to obtain doped manganese iron oxalate;
[0136] (2) Sodium acetate is added to the doped ferromanganese oxalate in an amount such that the total molar amount of metal ions in the doped ferromanganese oxalate is 1:1.1 to the molar amount of sodium ions in the sodium salt, and the material is ball-milled to a particle size of 2.75 μm, and then placed in a rotary kiln for calcination at 750° C. for 6 hours, while air is introduced into the rotary kiln to maintain the oxygen volume concentration in the atmosphere in the rotary kiln at 19.8%, and then cooled to a material temperature of ≤80° C. by a cooling screw conveyor and then conveyed out to obtain doped sodium ferromanganate.
[0137] (3) adding doped sodium ferromanganate to pure water and nanographite sheets, wherein the mass ratio of doped sodium ferromanganate, pure water and nanographite is 1:3:0.1, placing the mixture into a sand mill, sand grinding the mixture to a particle size of 198 nm, and then adding ammonium sulfate and sodium sulfite to the sand-milled slurry, wherein the molar ratio of the added ammonium sulfate, sodium sulfite, sodium borate and sodium ferromanganate is 4.5:0.9:0.05:1, stirring and dissolving the mixture evenly, and then spray drying. In the spray drying process, hot nitrogen is used as a heat source, the temperature of the hot nitrogen is 200° C., the speed of the atomizing wheel is controlled so that the particle size of the final spray-dried material is 10 μm, and the discharge temperature is controlled to be ≤80° C. to obtain a spray-dried material;
[0138] (4) The spray-dried material is conveyed to a calcining furnace through a pipeline conveyor. The secondary calcination is carried out in a roller furnace with nitrogen as the protective atmosphere. The heating rate in the heating stage is 2°C / h. The temperature in the insulation stage is 350°C for 20 hours. The cooling rate is then 2°C / h. The material is discharged after cooling to a temperature ≤70°C. The material is then mixed with sodium oxalate and crushed in a pulverizer. The mass ratio of the calcined material to the mixed sodium oxalate is 1:0.02. The pulverization is carried out in a jet mill until the particle size of the material is 2.4 μm. The material is then sieved, iron removed, and vacuum packaged in a packaging room. The temperature in the packaging room is 25±5°C and the humidity is ≤10%. The composite sodium ferrous manganese sulfate positive electrode material is obtained. The performance test data of the composite sodium ferrous manganese sulfate positive electrode material in Example 2 are shown in Table 5.
[0139] Table 5 Performance test data of composite sodium ferrous manganese sulfate positive electrode material
[0140]
[0141] Example 4
[0142] A method for preparing a composite sodium manganese ferrous sulfate positive electrode material, the other contents are the same as those of Example 1, except that the temperature of the first calcination is 700°C.
[0143] Example 5
[0144] A method for preparing a composite sodium ferrous manganese sulfate positive electrode material, the other contents are the same as those in Example 1, and the primary calcination temperature is 1000°C
[0145] Example 6
[0146] A method for preparing a composite sodium manganese ferrous sulfate positive electrode material, the other contents of which are the same as those of Example 1, except that the temperature of the insulation section of the secondary calcination is 400°C.
[0147] Example 7
[0148] A method for preparing a composite sodium manganese ferrous sulfate positive electrode material, the other contents of which are the same as those of Example 1, except that the temperature of the insulation section of the secondary calcination is 200°C.
[0149] Example 8
[0150] A method for preparing a composite sodium ferrous manganese sulfate positive electrode material, the other contents of which are the same as those of Example 1. During the coprecipitation process, ammonium bicarbonate is added to stabilize the pH of the reaction solution at 3.0.
[0151] Example 9
[0152] A method for preparing a composite sodium manganese ferrous sulfate positive electrode material, the other contents of which are the same as those of Example 1. During the coprecipitation process, ammonium bicarbonate is added to stabilize the pH of the reaction solution at 5.0.
[0153] Comparative Example 1
[0154] The sodium ferrous manganese sulfate positive electrode material is prepared by adopting the existing low-temperature sintering method.
[0155] 2. Test Method
[0156] 1. Property test of composite sodium ferrous manganese sulfate positive electrode material: the compaction density is tested in accordance with "GB / T24533-2019", the tap density is tested in accordance with "GB / T 21354-2008", and the ionic conductivity is tested in accordance with "GB / T 30835-2014". The results are shown in Table 6.
[0157] 2. Test of the properties of secondary batteries: According to the positive electrode material: SP: PVDF mass ratio of 90:5:5, the materials were coated on aluminum foil, the electrolyte was sodium perchlorate with a concentration of 1 mol / L, the negative electrode was a sodium sheet, and a sodium ion button was prepared and tested at a temperature of 25±1°C. The test rates were 0.1C / 1C / 2C / 4C / 5C and 10C. The results are shown in Table 7.
[0158] III. Analysis of test results of various embodiments and comparative examples
[0159] Depend on Figure 2 As shown in Figure 1, the SEM of doped ferromanganese oxalate is a massive precipitate with a relatively smooth surface. Figure 3 As shown in Figure 1, the morphology of doped sodium ferromanganate is a block structure with fine particles distributed on the surface; Figure 4 As shown, the spray-dried material includes block material (sodium ferromanganate), granular material (sodium sulfite, ammonium sulfate), and flake material (nanographite), and the obtained spray-dried material is spherical particles; Figure 5 As shown, a coated composite sodium manganese ferrous sulfate positive electrode material is formed; Figure 2-Figure 5The forming process of the composite sodium ferrous manganese sulfate positive electrode material of the present application is shown, indicating that the product is successfully prepared; Figure 6 The charge and discharge curve of the secondary battery prepared by the positive electrode material of Example 1, Figure 7 0.1C charge and discharge curve of a secondary battery prepared with the positive electrode material of Example 2.
[0160] Table 6 Test results of properties of positive electrode materials
[0161]
[0162] As shown in Table 1, since the primary calcination temperature (900°C) in Example 2 is higher than the primary calcination temperature (820°C) in Example 1 and the primary calcination temperature (750°C) in Example 3, the compaction density of the positive electrode material prepared in Example 2 is the best, followed by Example 1, and the worst is Example 3. This result is consistent with the aforementioned lower calcination temperature, the lower the compaction density of the prepared positive electrode material. Further, in Example 4, the primary calcination temperature is reduced to 700°C, and the compaction density of the positive electrode material prepared in Example 4 is lower than the compaction density of the positive electrode material prepared in Example 3. At the same time, in Example 5, the primary calcination temperature is increased to 1000°C, and the compaction density of the positive electrode material prepared in Example 5 is higher than the compaction density of the positive electrode material prepared in Example 2. Since the primary calcination temperature is greatly increased, the compaction density of the prepared positive electrode material is also increased. However, combined with the data of ionic conductivity, the ionic conductivity of the positive electrode material prepared in Example 5 is much lower than that of the positive electrode material prepared in Examples 1 to 3. Therefore, too high a primary calcination temperature will significantly affect the ionic conductivity of the prepared positive electrode material. In the present application, by setting the primary calcination temperature to 750-900°C, the compaction density and ionic conductivity of the positive electrode material can be effectively improved at the same time.
[0163] Further, in Example 6, the temperature of the insulation section of the secondary calcination is adjusted to 400°C. Since the temperature of the insulation section of the secondary calcination in Example 6 is higher than the temperature of the insulation section of the secondary calcination in Example 1 (330°C), the compact density of the positive electrode material prepared in Example 6 is higher than the compact density of the positive electrode material prepared in Example 1 due to the influence of temperature. However, the ion conductivity of the positive electrode material prepared in Example 6 is affected and is significantly lower than the ion conductivity of the positive electrode material prepared in Example 1. Meanwhile, in Example 7, the temperature of the insulation section of the secondary calcination is adjusted to 200°C. Since the temperature of the insulation section of the secondary calcination in Example 7 is lower than the temperature of the insulation section of the secondary calcination in Example 1 (330°C), the compact density of the positive electrode material prepared in Example 7 is lower than the compact density of the positive electrode material prepared in Example 1 due to the influence of temperature. The ion conductivity of the positive electrode material prepared in Example 7 is also lower than the ion conductivity of the positive electrode material prepared in Example 1.
[0164] Furthermore, in Example 8, ammonium bicarbonate was added during the co-precipitation process to stabilize the pH of the reaction solution at 3.0, and in Example 9, ammonium bicarbonate was added during the co-precipitation process to stabilize the pH of the reaction solution at 5.0. From the data in Table 1, it can be seen that the comprehensive performance of the compaction density and ion conductivity of the positive electrode materials prepared in Examples 8 and 9 is inferior to the comprehensive performance of the compaction density and ion conductivity of the positive electrode material prepared in Example 1. Therefore, if the pH of the reaction solution in the co-precipitation process is too high or too low, it will also have a significant effect on the performance of the prepared positive electrode material.
[0165] Table 7 Test results of secondary battery properties
[0166]
[0167]
[0168] It can be seen from Table 7 that when the positive electrode materials prepared in Examples 1 to 9 and Comparative Example 1 are used to prepare sodium ion batteries, the electrochemical performance of the sodium ion batteries prepared using the positive electrode materials prepared in Examples 1 to 3 is significantly better than the electrochemical performance of the sodium ion batteries prepared using the positive electrode materials prepared in Examples 4 to 9 and Comparative Example 1.
[0169] The above results indicate that the composite sodium manganese ferrous sulfate prepared by the present application has high ionic conductivity and high compaction density, and the corresponding sodium ion battery has good electrochemical performance.
[0170] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A method for preparing a composite sodium ferrous manganese sulfate positive electrode material, characterized in that: The following steps are involved: Manganese salt, ferrous salt and doping agent are used as raw materials, and reducing agent and oxalic acid compound are added in sequence to obtain doped manganese ferrooxalate through reaction; The doped ferromanganese oxalate is mixed with sodium salt, and after a dispersion and a calcination, a doped sodium ferromanganate is obtained; Adding a carbon source and a solvent to the doped sodium ferromanganate and performing secondary dispersion, then adding a sulfate-containing compound and a flux, and spray drying to obtain a spray-dried material; The spray-dried material is subjected to secondary calcination, and then a sodium supplement is added, and after crushing and impurity removal, the composite sodium ferrous manganese sulfate positive electrode material is obtained; Wherein, the temperature of the primary calcination is 750-900°C.
2. The method for preparing the composite sodium ferrous manganese sulfate positive electrode material according to claim 1, characterized in that: The dopant comprises one or more of a soluble magnesium salt, an aluminum salt, a nickel salt or a cobalt salt; and / or The reducing agent includes one or more of ascorbic acid, sodium thiosulfate, and sodium pyrosulfite; and / or The oxalate compound includes one or more of ammonium oxalate, oxalic acid and sodium oxalate.
3. The method for preparing the composite sodium ferrous manganese sulfate positive electrode material according to claim 1, characterized in that: The molar ratio of the manganese ions in the manganese salt, the ferrous ions in the ferrous salt and the metal ions in the dopant is 1:(2-4):(0.1-0.2); and / or The molar ratio of the reducing agent to the ferrous ions in the ferrous salt is (0.05-0.1):1; and / or The ratio of the molar amount of the oxalic acid compound to the total molar amount of the manganese ions in the manganese salt, the ferrous ions in the ferrous salt and the metal ions in the dopant is (1.1-1.25):
1.
4. The method for preparing the composite sodium ferrous manganese sulfate positive electrode material according to claim 1, characterized in that: The primary calcination is carried out in an atmosphere with an oxygen volume concentration of ≥19%.
5. The method for preparing the composite sodium ferrous manganese sulfate positive electrode material according to claim 1, characterized in that: The ratio of the total molar amount of metal ions in the doped ferromanganese oxalate to the molar amount of sodium ions in the sodium salt is 1:(1.03-1.1); and / or The sodium salt includes at least one of sodium acetate, sodium nitrate, sodium citrate and sodium chloride.
6. The method for preparing the composite sodium ferrous manganese sulfate positive electrode material according to claim 1, characterized in that: The mass ratio of the doped sodium ferromanganate, the solvent and the carbon source is 1:(3-5):(0.1-0.15); and / or The sulfate-containing compound is a mixture of ammonium sulfate and sodium sulfite, and the flux is sodium borate, wherein the molar ratio of the ammonium sulfate, the sodium sulfite, the sodium borate and the doped sodium ferromanganate is (4.5-5.5):(0.9-1.1):(0.05-0.1):
1.
7. The method for preparing the composite sodium ferrous manganese sulfate positive electrode material according to claim 1, characterized in that: In the step of using manganese salt, ferrous salt and dopant as raw materials, adding reducing agent and oxalic acid compound in sequence, and obtaining doped manganese ferrooxalate through reaction, the pH value during the reaction is 4-4.5, the temperature is 40-60°C, the addition time of oxalic acid compound and reducing agent is 30-60min, and the reaction time is 30-60min.
8. The method for preparing the composite sodium ferrous manganese sulfate positive electrode material according to claim 1, characterized in that: The spray drying temperature is 120-180°C; and / or The secondary calcination temperature is 300-350°C; and / or The sodium supplement comprises sodium oxalate; and / or The mass ratio of the calcined material obtained by the secondary calcination to the sodium supplement agent is 1:(0.02-0.03).
9. A composite sodium ferrous manganese sulfate positive electrode material obtained by the preparation method according to any one of claims 1 to 8, characterized in that: The ionic conductivity of the composite sodium manganese ferrous sulfate positive electrode material is 3.0×10 -6 -10.0×10 -6 S / cm, and the compaction density of the composite sodium ferrous manganese sulfate positive electrode material is 2.30-2.45g / mL.
10. A sodium ion battery, characterized in that: It contains the composite sodium ferrous manganese sulfate positive electrode material as claimed in claim 9.