Alloy powder and method for preparing carbon nanotube reinforced high-strength steel composite member

Through ball milling process and heat treatment technology, the problem of insufficient bonding strength between carbon nanotubes and iron-based high-strength alloy materials is solved, and the preparation of high-strength and high-strength steel composites with high strength and high toughness is realized, simplifying the process and reducing costs .

WO2024250401A1PCT designated stage expired Publication Date: 2024-12-12CHANGZHOU GIAN TECH +1

Patent Information

Application Number
PCT/CN2023/109492
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-07
Filing Date
2023-07-27
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

The insufficient bonding strength of carbon nanotubes and iron-based high-strength alloy materials has limited applications in improving mechanical properties, and the existing modification methods are complex and not suitable for mass production.

Method used

The carbon nanotubes are mixed with high-strength steel alloy powder by ball milling. The carbon nanotubes are evenly dispersed through ultrasonic cleaning and ball milling. Combined with the heat treatment process to improve the interface bonding force, a carbon nanotube with high strength and high toughness is prepared. Steel composite parts.

Benefits of technology

The uniform distribution and efficient combination of carbon nanotubes in high-strength steel alloy powder was achieved, and composite parts with yield strength exceeding 2000MPa were prepared, which simplified the process flow and reduced costs, making it suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023109492_12122024_PF_FP_ABST
    Figure CN2023109492_12122024_PF_FP_ABST
Patent Text Reader

Abstract

A method for preparing a carbon nanotube reinforced high-strength steel composite member, comprising the following steps: S1, placing a carbon nanotube in a dispersion liquid, using ultrasonic waves for cleaning, and then carrying out drying treatment; S2, adding the dried carbon nanotube into a high-strength steel alloy powder, adding a process control agent for ball milling, and then washing and filtering to obtain a composite powder; S3, carrying out closed mixing granulation on the composite powder and a binder to prepare a feeding material, and carrying out injection molding in an injection molding machine to obtain a green body; S4, degreasing the green body in a nitric acid or oxalic acid catalytic degreasing furnace to obtain a degreased blank; S5, sintering the degreased blank in a single-unit furnace to obtain a sintered body; and S6, carrying out heat treatment on the sintered body in a vacuum furnace to obtain a composite member. Also provided is an alloy powder for preparing a carbon nanotube reinforced high-strength steel composite member. According to the preparation method, the problems of the carbon nanotubes having very large van der Waals force, being easy to gather and entangle and being difficult to uniformly disperse in a metal matrix due to very large length-diameter ratio, specific surface area and specific surface energy are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Alloy powder for preparing carbon nanotube reinforced high-strength steel composite parts and preparation method Technical Field

[0001] The present invention relates to the field of high-strength steel material preparation, and in particular to alloy powder for preparing carbon nanotube-reinforced high-strength steel composite parts and a preparation method thereof. Background Art

[0002] With the rapid development of the consumer electronics industry, high-strength steel, combined with metal powder injection molding technology, has gained widespread application in the manufacture of electronic components such as hinges, brackets, housings, and cams for foldable smartphones. High-strength steel, due to its ultra-high strength, excellent ductility, and superior overall performance, has entered a period of rapid material development. Current research on high-strength steel includes adjusting elemental composition, developing high-Ni alloys, and developing multi-component alloys by adding elements such as Cr, Co, Mo, and Nb, all of which have made significant progress. Chinese Patent Publication No. CN 114480943A, entitled "An Ultra-Low Carbon, Low-Cobalt Martensitic Steel and Its Preparation Method," describes the preparation of ultra-low carbon, low-cobalt martensitic powder metallurgy steel with a tensile strength exceeding 2000 MPa and an elongation exceeding 5%. This patent incorporates cryogenic heat treatment and hot isostatic pressing (HIP) processes into the preparation process. However, there have been no reports of alloy steels with yield strength exceeding 2000 MPa using only a "solutionization + aging" process.

[0003] Since their discovery, carbon nanotubes (CNTs) have shown promising application prospects in a wide range of fields, including nanoelectronics, precision machinery, and medical devices, thanks to their exceptional mechanical, thermal, magnetic, and electrical properties. With tensile strengths of 50 to 200 gp, over 100 times that of steel, and a density of only 1.35 g / cm³, and an elastic modulus of 1 TPa, approximately five times that of steel, CNTs are considered a promising reinforcement for ceramics, polymers, and metal-matrix composites. However, numerous challenges remain in reinforcing metal-matrix composites. The primary obstacle lies in the large aspect ratio, specific surface area, and specific surface energy of CNTs, resulting in strong van der Waals forces and prone to aggregation and entanglement, making uniform dispersion in metal matrices difficult. Furthermore, CNTs have low surface activity and poor wettability with metal matrices, resulting in poor interfacial bonding. These factors can significantly impact the density, mechanical, electrical, and friction and wear properties of metal-matrix composites.

[0004] Therefore, currently, methods such as surface modification of carbon nanotubes, polymer coating of metal substrates followed by adsorption of carbon nanotubes, preparation of micro-nanosheets from alloy powders and subsequent ball milling of the composite with carbon nanotubes, or densification and molding have become important approaches to improve the interfacial bonding between carbon nanotubes and metal substrates. The carbon nanotubes obtained by these methods have good dispersion and excellent interfacial bonding with the substrate, but the processes are relatively complex and are not ideal for controlling costs during mass production. Therefore, this application considers the use of ball milling, which utilizes the shearing effect of the moving balls through the rotation of the ball mill to disperse the carbon nanotubes and improve the interfacial bonding with the metal substrate.

[0005] Due to quantum confinement of electrons within carbon nanotubes, electrons can only move along the axial direction of the carbon nanotube within the graphite sheet. This gives carbon nanotubes unique electrical properties, leading to numerous reports on their use to enhance the electrical conductivity of copper-based metals. However, there are fewer reports on iron-based materials, with only a limited amount of research on their magnetic properties. Composite nanomagnetic materials made from carbon nanotubes and iron can achieve directional alignment of the carbon nanotubes under the influence of a magnetic field, significantly improving the material's magnetic sensitivity and enabling widespread application in fields such as microwave absorbing materials, wastewater treatment, and sensor development. However, carbon nanotubes have yet to be used in the field of iron-based high-strength alloys, primarily to enhance mechanical properties such as high strength and hardness.

[0006] The current difficulty in applying carbon nanotube-reinforced iron-based materials is primarily due to the insufficient bonding strength between the carbon nanotubes and the iron substrate. Whether using surface activation methods (adding surfactants to create polymer chains and functional groups on the surface to improve interfacial compatibility) or chemical modification methods (creating hyperconjugated π-electron systems on the surface to enhance chemical activity), both efforts aim to enhance the interfacial wetting and bonding between the carbon nanotubes and the iron substrate, thereby promoting a more uniform distribution of the carbon nanotubes within the iron substrate. However, the results in actual preparation remain suboptimal.

[0007] Summary of the Invention

[0008] The first object of the present invention is to provide a method for preparing carbon nanotube-reinforced high-strength steel composite parts, which can effectively solve the problem that carbon nanotubes have a large aspect ratio, specific surface area and specific surface energy, resulting in large van der Waals forces, easy aggregation and entanglement, and difficulty in uniform dispersion in the metal matrix.

[0009] The technical solution for achieving the first object of the present invention is: the method for preparing a carbon nanotube reinforced high-strength steel composite member in the present invention comprises the following steps:

[0010] S1, placing the carbon nanotubes in a dispersion and cleaning them using ultrasound, followed by drying;

[0011] S2. Adding the dried carbon nanotubes to the high-strength steel alloy powder and adding a process control agent to perform ball milling to obtain a ball milling product, removing the ball milling product, drying it, and then filtering it to obtain a composite powder;

[0012] S3, kneading the composite powder and the binder into granules to obtain feed, and then injection molding the feed in an injection molding machine to obtain a green body;

[0013] S4, degreasing the green body in a nitric acid or oxalic acid catalytic degreasing furnace to obtain a degreased body;

[0014] S5, sintering the degreased blank in a single furnace to obtain a sintered body;

[0015] S6. Heat-treating the sintered body in a vacuum furnace to obtain a composite part.

[0016] The impact on the carbon nanotubes during the ball milling process causes a small amount of carbon nanotubes to be broken and embedded in the metal matrix, making it easier to evenly distribute the carbon nanotubes in the matrix during subsequent sintering.

[0017] Furthermore, the mass percentages of the composite powder are: carbon nanotubes 0.5% to 5%, high-strength steel alloy powder 0.5% to 5%, high-strength steel alloy powder 93% to 98.5%, and process control agent 1% to 2%.

[0018] The process control agent is incorporated into the composite powder because it accounts for a significant portion of the powder mass. However, its addition has no other impact on the subsequent preparation process; it will be burned and volatilized along with the binder during sintering. The primary function of the process control agent is to prevent powder agglomeration and adhesion to the milling chamber walls during ball milling.

[0019] Furthermore, the high-strength steel alloy powder has the following mass percentages: C < 0.1%, Cr: 7-12%, Ni: 6-11%, Mo: 5-10%, Co: 8-13%, Nb: ≤ 0.5%, and the rest is Fe; the average particle size of the high-strength alloy powder is 15 μm to 25 μm.

[0020] The present invention eliminates the addition of trace alloying elements, reducing costs while simplifying the atomization and pulverization processes for the raw material high-strength alloy powder, ensuring the stability of the raw material. Using only base metal elements to formulate the high-strength alloy powder increases process feasibility, facilitates product preparation, and offers market advantages.

[0021] The high-strength alloy powder has a relatively short average particle size range. This is primarily to ensure uniformity in the composite powder. A uniform raw material particle size contributes to the stability of the composite powder. Secondly, while both single-walled and multi-walled carbon nanotubes can be grown, their typical lengths range from 1 to 30 μm. We strive to keep the particle size of the high-strength alloy powder similar to that of the carbon nanotubes to ensure uniform microstructure and promote better mixing during ball milling.

[0022] Furthermore, the carbon nanotubes are any one of single-walled carbon nanotubes and multi-walled carbon nanotubes, or a combination of two or more thereof; the aspect ratio is greater than 100, and the tube diameter is 0.4 nm to 100 nm.

[0023] The mechanical properties of single-walled carbon nanotubes are superior to those of multi-walled carbon nanotubes. The tensile strength of single-walled carbon nanotubes can exceed 100 GPa, while the tensile strength of multi-walled carbon nanotubes is mostly between 50 and 100 GPa. Because multi-walled carbon nanotubes have a layered structure, trap centers easily form on the tube walls, capturing some defects. However, it is precisely because of this characteristic that during the ball milling process, active defect sites are easily formed on the tube walls of partially broken multi-walled carbon nanotubes, creating more openings that are more likely to attract alloy atoms to gather here, thereby enhancing the bonding between the carbon nanotubes and metal particles during the ball milling process. Therefore, the advantages of combining single-walled and multi-walled carbon nanotubes can not only ensure high mechanical properties, but also promote the bonding between high-strength alloy powder and carbon nanotubes during the ball milling process.

[0024] The aspect ratio of single-walled carbon nanotubes can be as high as 10,000, while that of multi-walled carbon nanotubes is typically between 50 and 4,000. This high aspect ratio is the primary reason for carbon nanotubes' excellent mechanical properties. The impact and shearing effects of ball milling shorten the actual length of carbon nanotubes, so appropriately increasing the aspect ratio of carbon nanotubes ensures that after ball milling, multi-walled carbon nanotubes retain a high aspect ratio and maintain high mechanical properties. Chopped carbon nanotubes are less prone to entanglement and agglomeration, making them easier to disperse during ball milling and embed into the metal matrix, achieving uniform dispersion.

[0025] Typically, the diameter of single-walled carbon nanotubes is 0.4 to 6 nm, and the diameter of multi-walled carbon nanotubes is 2 to 100 nm. The diameters of the present invention basically cover the main ranges of single-walled and multi-walled carbon nanotubes, and also demonstrate the advantage of the ball milling process being applicable to single-walled, multi-walled, and a combination of single-walled and multi-walled carbon nanotubes, i.e., it has strong applicability to carbon nanotubes.

[0026] Furthermore, during the ball milling in step S2, the mass ratio of the mixture of high-strength alloy powder, carbon nanotubes, and process control agent to stainless steel balls with a diameter of 2 to 5 mm is 1 / 1 to 1 / 20, the rotation speed is 100 to 500 rpm, and the ball milling time is 30 to 6 hours. The ball milling medium is stainless steel balls. The process control agent is one or more of stearic acid, lithium stearate, zinc stearate, paraffin, methanol, ethanol, silicone oil, oleic acid, and cellulose. The ball milling process can be selected from planetary ball milling, stirred ball milling, and high-energy ball milling. The process control agent is selected to prevent cold welding of the carbon nanotubes and high-strength steel alloy powder during the ball milling process.

[0027] Preferably, the binder can be a plastic binder, which includes POM, a skeleton agent, a dispersant, a lubricant, a toughening agent, and a stabilizer. The volume ratio of the binder to the composite powder is 6:4.

[0028] Furthermore, the injection conditions in the above step S5 include: mold temperature of 130° C. to 140° C., injection pressure of 1000 bar, and barrel temperature of ≤210° C.

[0029] Furthermore, the degreasing conditions in the above step S6 include: a nitric acid flow rate of 2-5 ml / min, a catalytic temperature of 80-120° C., and a degreasing time t≥300 min.

[0030] Furthermore, the sintering conditions in the above step S7 are: sintering is performed in a single furnace under an Ar atmosphere, the sintering temperature is 1360-1380° C., and the heating time is 4 h to 5 h.

[0031] The reasons for choosing this sintering temperature are: on the one hand, high-temperature sintering and appropriately extending the holding time are conducive to improving the densification of the matrix. The denser the sintering, the lower the porosity inside the material, and the better the overall performance. If the porosity of the material is too high, during the plastic deformation process, micropores are likely to aggregate and become the origin of microcracks, causing the cracks to expand, thereby reducing the mechanical properties. At the same time, the sintering temperature cannot be too high, otherwise the grains will grow and coarsen, and the material's fracture resistance will drop sharply. On the other hand, during high-temperature sintering, the carbon atoms of the carbon nanotubes are more likely to diffuse in the matrix. The higher the temperature, the faster the diffusion rate of the carbon atoms, and the easier it is to form Fe-C groups that link with the matrix metal. Therefore, at the above temperature, while ensuring dense sintering and no grain coarsening, the bonding effect of the carbon nanotubes and the metal interface can be improved.

[0032] Furthermore, the heat treatment process in the above step S8 includes solution treatment at 1085° C., holding temperature for 1 to 1.5 hours, and aging at 520° C., holding temperature for 3 to 3.5 hours.

[0033] The mechanism of solid solution and aging treatment: When solid solution is carried out at a high temperature of 1085℃, more alloying elements can be dissolved, and then they are allowed to dissolve and precipitate during the aging process, and are distributed on the matrix in the form of fine dispersed intermetallic compounds, which plays a role of precipitation strengthening. The combined effect of solid solution strengthening and precipitation strengthening can ensure that the strength exceeds 2000MPa and is maintained at a high level. At the same time, in order to achieve a comprehensive matching effect of strength and elongation, the aging temperature is appropriately increased. When aging is carried out at 520℃, a small amount of residual austenite can be retained. Austenite, as a toughness phase, can improve the elongation of high-strength steel. Therefore, the combination of solid solution and aging is an important reason for achieving a match between high strength and high toughness.

[0034] The second purpose of the present invention is to provide an alloy powder for preparing carbon nanotube-reinforced high-strength steel composite parts. Please provide additional description of the technical purpose of designing the alloy powder (i.e., what are the advantages of combining the powder system with carbon nanotubes).

[0035] The technical solution for achieving the second object of the present invention is: the alloy powder in the present invention is the above-mentioned high-strength steel alloy powder.

[0036] After combining this high-strength steel alloy powder with carbon nanotubes, the carbon nanotubes maintain their hollow structure, with metal particles growing and connecting at their tips. This is because the five metal elements—Cr, Co, Mo, Ni, and Fe—do not disrupt the tubular structure of the carbon nanotubes, preserving their overall microscopic morphology. The transition metal elements Co and Ni reduce the specific surface area of ​​the carbon nanotubes, diminishing van der Waals forces and enhancing the bonding strength between the carbon nanotubes and the metal interface.

[0037] The present invention has positive effects: (1) The present invention realizes uniform distribution of carbon nanotubes in high-strength steel alloy powder through ultrasonic dispersion treatment, ball milling mixing of composite powder composed of carbon nanotubes and high-strength steel powder, and injection molding process, and can prepare carbon nanotube-reinforced high-strength steel composite parts with excellent comprehensive performance.

[0038] (2) In the present invention, the impact on the carbon nanotubes during the ball milling process causes a small amount of carbon nanotubes to be broken and embedded in the metal matrix, making it easier to evenly distribute the carbon nanotubes in the matrix during subsequent sintering.

[0039] (3) The process control agent is incorporated into the powder in this invention because it accounts for a significant portion of the powder mass. However, its addition has no other impact on the subsequent preparation process. During the sintering process, it will be burned and volatilized along with the binder. The main function of the process control agent is to prevent powder agglomeration and adhesion to the tank wall during the ball milling process.

[0040] (4) The average particle size range of the high-strength alloy powder in the present invention is relatively short. The first purpose is to ensure the uniformity of the composite powder. Raw materials with uniform particle size are conducive to the stability of the composite powder. The second purpose is that although both single-walled and multi-walled carbon nanotubes can be grown, their conventional length range is 1 to 30 μm. We try to make the particle size of the high-strength alloy powder similar to that of the carbon nanotubes to ensure uniform microstructure and promote better mixing of the two during ball milling.

[0041] (5) The present invention simplifies the preparation process of composite powders containing carbon nanotubes, and also maintains the dispersibility of carbon nanotubes in high-strength steel alloy powders and a good interface bonding effect with the high-strength steel alloy powders.

[0042] (6) The present invention applies carbon nanotubes to the metal injection molding process, which can meet the demand for ultra-high strength mechanical properties of electronic products, especially micro-complex parts.

[0043] (7) The present invention adopts a conventional heat treatment process and only performs solid solution and aging treatment on the material to obtain a composite part with a yield strength exceeding 2000 MPa; at the same time, it effectively controls the cost of mass production and improves production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below based on specific embodiments and in conjunction with the accompanying drawings, wherein

[0045] FIG1 is a process flow chart of the present invention. DETAILED DESCRIPTION

[0046] The present invention is further described below with reference to specific examples. It should be noted that the following examples are only used to illustrate the specific implementation methods of the present invention and cannot limit the scope of protection of the present invention.

[0047] The following examples were all carried out according to the process shown in FIG1 . The room temperature mechanical properties of the materials in all examples were determined with reference to GB / T 228.1-2010, and the tensile rate was 0.5 mm / min.

[0048] (Example 1)

[0049] The method for preparing a carbon nanotube-reinforced high-strength steel composite member of the present invention comprises the following steps:

[0050] S1. Place 100g of multi-walled carbon nanotubes (40nm in diameter) in a dispersion solution consisting of 95% by volume alcohol and 5% by volume hydrochloric acid (1-5 mol / L hydrochloric acid concentration) and use ultrasonic cleaning. The ultrasonic cleaning is performed at a power of 100W for 5 minutes at a temperature of 20-25°C. After ultrasonic cleaning, the mixture is washed and filtered multiple times with deionized water and vacuum dried at 50°C for 12 hours to produce relatively pure carbon nanotubes. This disperses the carbon nanotubes and prevents them from agglomerating.

[0051] S2. Place 10 kg of high-strength steel alloy powder with a particle size of 20 μm in a stirred ball mill, add the pure carbon nanotubes dried in step S1, and add 150 g of stearic acid as a process control agent. Use stainless steel balls as ball milling media, and the mass ratio of the mixture of stainless steel balls, carbon nanotubes, high-strength alloy powder and process control agent is 20:1. Ball milling is carried out at a speed of 300 r / min for 4 hours under argon protection to obtain a ball milling product. The ball milling product is removed, dried, and then filtered to obtain a composite powder of carbon nanotube-reinforced high-strength steel with a carbon nanotube content of 1 wt.%.

[0052] S3. The prepared composite powder is mixed with a binder and kneaded for 4 hours. The feed is then extruded and granulated using a single-screw extruder to obtain a feed to be injection molded. The feed is a cylinder with a diameter of 3 mm to 4 mm and a height of 5 mm to 6 mm.

[0053] S4. Inject the feed material into a green body of a set shape on an injection molding machine; wherein the mold temperature is 130°C, the holding pressure is 1000 bar, the holding time is 4 seconds, and the barrel temperature is ≤210°C.

[0054] S6. Using catalytic degreasing to remove the binder to obtain a degreased blank; wherein the degreasing temperature is 100° C., the nitric acid concentration is ≥99%, the degreasing time is 6 hours, nitrogen is filled as a protective gas, and the oxygen content is ≤5%.

[0055] S7, placing the degreased blank into a monomer sintering furnace for sintering to obtain a sintered body; the sintering is a stepwise heating process, and the temperatures are kept at 400°C, 600°C, 900°C, and 1200°C for 1 hour respectively, the sintering temperature is 1370°C, and the sintering time is 5 hours; after the sintering is completed, the blank is cooled with the furnace to obtain a sintered body;

[0056] S8. Place the sintered body in a vacuum furnace for heat treatment to obtain a carbon nanotube-reinforced high-strength steel composite. The heat treatment includes: solution heat treatment at a temperature of 1085° C. for 1.5 hours; and aging heat treatment at a temperature of 520° C. for 3 hours.

[0057] The binder can be a plastic binder, which includes POM, a skeleton agent, a dispersant, a lubricant, a toughening agent and a stabilizer.

[0058] The composite prepared in Example 1 had a yield strength of 2216 MPa, a tensile strength of 2380 MPa, and an elongation of 5.14%.

[0059] (Example 2)

[0060] This embodiment differs from embodiment 1 in that the weight percentage of carbon nanotubes in step S2 is 0.5 wt.%. The yield strength of the prepared carbon nanotube-reinforced high-strength steel composite is 2190 MPa, the tensile strength is 2361 MPa, and the elongation is 5.01%.

[0061] (Example 3)

[0062] This embodiment differs from embodiment 1 in that the weight percentage of carbon nanotubes in step S2 is 2 wt.%. The yield strength of the prepared carbon nanotube-reinforced high-strength steel composite is 2178 MPa, the tensile strength is 2342 MPa, and the elongation is 4.93%.

[0063] (Example 4)

[0064] This embodiment differs from embodiment 1 in that the ball mill speed in step S2 is 400 r / min and the ball milling time is 3 h. The yield strength of the prepared carbon nanotube-reinforced high-strength steel composite is 2221 MPa, the tensile strength is 2393 MPa, and the elongation is 5.02%.

[0065] (Example 5)

[0066] The difference between this embodiment and embodiment 1 is that the ball mill speed in step S2 is 200 r / min and the ball milling time is 5 hours. The yield strength of the prepared carbon nanotube-reinforced high-strength steel composite is 2183 MPa, the tensile strength is 2354 MPa, and the elongation is 4.88%.

[0067] The mechanical properties of the carbon nanotube-reinforced high-strength steel composites obtained in Examples 1 to 5 can be referred to the following table:

[0068] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a carbon nanotube reinforced high-strength steel composite, characterized in that The following steps are involved: S1, placing the carbon nanotubes in a dispersion and cleaning them using ultrasound, and then drying them; S2, adding the dried carbon nanotubes to the high-strength steel alloy powder, and adding a process control agent to perform ball milling to obtain a ball milling product, removing the ball milling product, drying it, and then filtering it to obtain a composite powder; S3, kneading the composite powder and the binder into granules to obtain feed material, and injection molding the feed material in an injection molding machine to obtain a green body; S4, degreasing the green body in a nitric acid or oxalic acid catalytic degreasing furnace to obtain a degreased body; S5, sintering the degreased blank in a monomer furnace to obtain a sintered body; S6. Heat-treating the sintered body in a vacuum furnace to obtain a composite part.

2. The method for preparing a carbon nanotube reinforced high-strength steel composite according to claim 1, characterized in that: The mass percentages of the composite powder are: 0.5% to 5% carbon nanotubes, 0.5% to 5% high-strength steel alloy powder, 93% to 98.5% process control agent, and 1% to 2%.

3. The method for preparing a carbon nanotube reinforced high-strength steel composite according to claim 1, characterized in that: The high-strength steel alloy powder has the following mass percentages: C<0.1%, Cr: 7-12%, Ni: 6-11%, Mo: 5-10%, Co: 8-13%, Nb: ≤0.5%, and the rest is Fe; the average particle size of the high-strength alloy powder is 15μm-25μm.

4. The method for preparing a carbon nanotube reinforced high-strength steel composite according to claim 1, 2 or 3, characterized in that: The carbon nanotubes are any one of single-walled carbon nanotubes and multi-walled carbon nanotubes, or a combination of two or more thereof; the aspect ratio is greater than 100, and the tube diameter is 0.4 nm to 100 nm.

5. The method for preparing a carbon nanotube reinforced high-strength steel composite according to claim 1, characterized in that: During the ball milling in step S2, the mass ratio of the mixture of high-strength alloy powder, carbon nanotubes and process control agent to stainless steel balls with a diameter of 2 to 5 mm is 1 / 1 to 1 / 20, the rotation speed is 100 r / min to 500 r / min, and the ball milling time is 30 min to 6 h; the ball milling medium is stainless steel balls; the process control agent is one or more of stearic acid, lithium stearate, zinc stearate, paraffin, methanol, ethanol, silicone oil, oleic acid, and cellulose; the ball milling can be selected from planetary ball milling, stirred ball milling, and high-energy ball milling processes.

6. The method for preparing a carbon nanotube reinforced high-strength steel composite according to claim 1, characterized in that: The sintering conditions in step S4 are: sintering is performed in a monomer furnace under an Ar atmosphere, the sintering temperature is 1360-1380° C., and the heating time is 4 h-5 h.

7. The method for preparing a carbon nanotube reinforced high-strength steel composite according to claim 1, characterized in that: The heat treatment process in step S5 includes solution treatment at 1085° C., insulation for 1 to 1.5 hours, and aging at 520° C., insulation for 3 to 3.5 hours.

8. An alloy powder for preparing a carbon nanotube-reinforced high-strength steel composite, characterized in that: The alloy powder is the high-strength steel alloy powder as claimed in claim 3.

Citation Information

Patent Citations

  • Method for manufacturing CNT (carbon nanotube) composite transmission conductor

    CN101948988A

  • Carbon material forming process and formed part

    CN104326747A

  • Carbon fiber reinforced copper-based composite material and preparation method thereof

    CN104388847A

  • Sintered compact and manufacturing method therefor

    JP2007217742A

  • Sintered body and method for producing the same

    US20080226489A1

Cited By

  • Method for preparing high-strength high-toughness wear-resistant PcBN cutter from B4C reinforced TiNbZrTa

    CN119703062A

  • A method for preparing high-strength, high-toughness and wear-resistant PcBN cutting tools by B4C-reinforced TiNbZrTa

    CN119703062B