High-fluidity early-strength cementing material as well as preparation method and application thereof
By regulating the proportion of aluminate cement, quicklime, gypsum and retarder, synergistic effects are formed, and the problem of low strength of gelled materials in the early stage is solved, and a gelled materials with high fluidity and controllable settling time are achieved. They are suitable for a variety of Application areas and reduce costs.
Patent Information
- Application Number
- CN202310634224.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
The existing cement cementitious materials have problems that contradict the fluidity and settling time, which leads to low early strength and is difficult to achieve the effect of fast settling and early strength.
By controlling the ratio of aluminate cement, quicklime, gypsum and retarder, a ternary or quaternary synergistic effect is formed, the setting time is regulated and early strength is improved, while adding a water reducer to improve fluidity and early strength.
It has achieved high fluidity, controlled settling time and early high strength gelling materials, which are suitable for mine backfill, grouting and reinforcement, reducing material costs and solving solid waste accumulation problems.
Smart Images

Figure BDA0004259364910000051 
Figure BDA0004259364910000061
Abstract
Description
Technical Field
[0001] The invention belongs to the field of cementitious materials, and relates to a high-fluidity early-strength cementitious material and a preparation method and application thereof. Background Art
[0002] CN113698160A discloses a fast-hardening high-performance bridge deck paving material, which is made by mixing aluminate cement, gypsum, redispersible latex powder, setting regulator, strengthening agent, composite additive, aggregate, steel fiber, etc. in a certain proportion. The strengthening agent is added to make the prepared material have a 2h compressive strength, but the use of the strengthening agent will result in higher costs.
[0003] CN108484062A discloses a self-leveling mortar made from coal-to-oil gasification furnace slag, which is prepared by mixing silicate cement-aluminate cement, adding slag, gypsum, lime, silica fume, water retaining agent, etc. in a certain proportion. The self-leveling mortar disclosed in the document does not have early strength.
[0004] At present, cementitious materials generally have the problem of contradiction between fluidity and setting time. The higher the fluidity, the longer the setting time, which leads to the disadvantage of low early strength. Therefore, it is an urgent problem to seek a cementitious material that can set quickly and achieve early strength while maintaining high fluidity. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a cementitious material that has fast setting and early strength while maintaining high fluidity. The cementitious material can be used in the fields of mine backfilling, grouting reinforcement, mine water blocking and concrete 3D printing.
[0006] By controlling the ratio of quicklime, gypsum and aluminate cement, a certain synergistic effect can be achieved, so that the cementitious material exhibits excellent properties such as rapid setting and early strength, which can promote the hydration of aluminate cement, shorten the setting time, and improve the early strength. However, the setting time is uncontrollable and cannot meet different construction requirements. The present invention finds that by compounding a certain proportion of a retarder (such as a retarder containing a carboxylate group) on the basis of the above-mentioned aluminate cement-quicklime-gypsum ternary system, the setting time can be controlled and the early strength can be significantly improved.
[0007] In addition, quicklime, aluminate cement and retarder also have a ternary synergistic effect. The present invention finds that by compounding a certain proportion of gypsum on the basis of the above-mentioned aluminate cement, quicklime and retarder, the setting time can be controlled and the early strength can be significantly improved.
[0008] As is known to all, adding a retarder alone to aluminate cement will prolong the setting time and greatly reduce the early strength. At the same time, gypsum, due to its retarding effect, will also delay the hydration reaction when acting alone in aluminate cement, resulting in reduced early strength. The present invention prepares a cementitious material by combining aluminate cement with quicklime, gypsum and retarder in a certain proportion, which not only makes the setting time adjustable, but also solves the problem that the slow setting caused by the retarder usually leads to reduced early strength, and unexpectedly has the effect of improving early strength. The present invention shows that there is a quaternary synergistic effect between aluminate cement, quicklime, gypsum and retarder.
[0009] Furthermore, the present invention finds that after quicklime, gypsum and retarder are mixed with aluminate cement in a certain proportion, further adding a water reducer can significantly improve the fluidity of the slurry, reduce the water consumption, and further improve the early strength.
[0010] Therefore, in a first aspect, the present invention provides a method for preparing a high-fluidity early-strength gelling material, comprising the following steps:
[0011] 100 parts by weight of aluminate cement, 2-20 parts by weight of quicklime, and 0.1-20 parts by weight of gypsum are uniformly mixed, and then 0.01-0.6 parts by weight of a retarder, 0.01-0.5 parts by weight of a water reducer, and an appropriate amount of water are added so that the water-cement ratio is 0.12-0.6, and the mixture is uniformly mixed to obtain a cementitious material;
[0012] For example, 100 parts by weight of aluminate cement, 2-20 parts by weight of quicklime and 2-20 parts by weight of gypsum are uniformly mixed, and then 0.2-0.6 parts by weight of retarder, 0.1-0.5 parts by weight of water reducer and appropriate amount of water are added so that the water-cement ratio is 0.36, and the mixture is uniformly mixed to obtain a cementitious material.
[0013] In some embodiments, in the above method, the gypsum is desulfurized gypsum.
[0014] In some embodiments, in any of the above methods, the retarder is an organic acid containing a carboxylate group, preferably tartaric acid.
[0015] In some embodiments, in any of the above methods, the water reducer is one or more of a naphthalene-based water reducer, a polycarboxylate water reducer, and a lignin-based water reducer, preferably a polycarboxylate water reducer.
[0016] In some embodiments, in any of the above methods, the initial setting time of the cementitious material is ≤10 min, the final setting time is ≤30 min, and the 2h compressive strength is ≥1 MPa.
[0017] In some embodiments, in any of the above methods, the expansion of the cementitious material is ≥ 290 mm.
[0018] In some embodiments, in any of the above methods, the quicklime can be replaced by a high-calcium mineral, wherein the high-calcium mineral is a mineral with a free calcium oxide content of 2-40wt%, preferably high-calcium fly ash. It should be noted that the high-calcium mineral described in this scheme refers to a mineral with a high free calcium oxide content. For example, high-calcium fly ash with a calcium content of more than 5wt% or even more than 10wt% in pulverized coal furnace fly ash cannot achieve such a synergistic effect with aluminate cement, because the calcium oxide in pulverized coal furnace fly ash is mainly inert calcium oxide, while the calcium oxide in circulating fluidized bed fly ash mainly exists as free calcium oxide.
[0019] In some embodiments, in the above method, the mass ratio of the aluminate cement to the high-calcium mineral is (0.2-4):1.
[0020] In a second aspect, the present invention also provides a high-fluidity early-strength gelling material prepared by any of the above methods.
[0021] In a third aspect, the present invention also provides the use of the high-fluidity early-strength gelling material as a mine backfill material, a grouting reinforcement material, a mine water plugging material, and a concrete 3D printing material.
[0022] In the present invention, early strength refers to the compressive strength of the hydration reaction 2 hours after stirring and molding; setting time refers to the initial setting and final setting time, the initial setting refers to the time when the cement paste begins to lose plasticity; the final setting time refers to the time when the cement paste completely loses plasticity and begins to generate strength.
[0023] The present invention has the following beneficial effects:
[0024] (1) The cementitious material prepared by the present invention is an early-strength cementitious material with high fluidity and controllable setting time. The compressive strength after hydration and curing for 2 hours is as high as 25.43 MPa, and can be used as mine backfill material, grouting reinforcement material, mine water plugging material, etc.;
[0025] (2) The amount of solid waste in the cementitious material of the present invention is large, which can effectively reduce the material cost and solve the problem of solid waste accumulation;
[0026] (3) The preparation process of the cementitious material of the present invention is simple and has practicality and industrial feasibility. DETAILED DESCRIPTION
[0027] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0028] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0029] The present invention will be further described below in conjunction with specific examples. It should be understood that the following examples are only used to illustrate the present invention and are not used to limit the scope of the present invention.
[0030] The aluminate cement is aluminate cement CA50-A600, a product of Zhengzhou Jianai Special Aluminate Co., Ltd.
[0031] Quicklime is a product of Hebei Hongzhuang Environmental Protection Technology Co., Ltd.
[0032] The gypsum is desulfurized gypsum.
[0033] The retarder is tartaric acid, a product of Nanjing Stabiao Trading Co., Ltd.
[0034] The water reducer is polycarboxylate water reducer, a product of Nanjing Stabo Trading Co., Ltd.
[0035] The initial setting time and final setting time are determined according to the method specified in GB / T 1346-2011 "Test method for water consumption and setting time of cement standard consistency".
[0036] The expansion degree is measured according to the method specified in GB / T 50448-2015 "Technical Specifications for Application of Cement-based Grouting Materials".
[0037] The 2h compressive strength is measured after curing for 2h according to the method specified in GB / T 50448-2015 "Technical Specifications for Application of Cement-based Grouting Materials".
[0038] Example 1
[0039] 100 parts by weight of aluminate cement, 10 parts by weight of quicklime and 10 parts by weight of gypsum were uniformly mixed, and then 0.4 parts by weight of retarder, 0.2 parts by weight of water reducer and 43 parts by weight of water were added, and the mixture was slowly stirred at 62±5 r / min for 20-30 s and then quickly stirred at 125±10 r / min for 60-90 s in a mixer to obtain cementitious material 1.
[0040] The initial setting time, final setting time, expansion and 2h compressive strength of the cementitious material are shown in Table 1.
[0041] Example 2
[0042] 100 parts by weight of aluminate cement, 10 parts by weight of quicklime and 5 parts by weight of gypsum were uniformly mixed, and then 0.4 parts by weight of retarder, 0.3 parts by weight of water reducer and 41 parts by weight of water were added, and the mixture was slowly stirred at 62±5 r / min for 20-30 s and then quickly stirred at 125±10 r / min for 60-90 s in a mixer to obtain cementitious material 2.
[0043] The initial setting time, final setting time, expansion and 2h compressive strength of the cementitious material are shown in Table 1.
[0044] Example 3
[0045] 100 parts by weight of aluminate cement, 2 parts by weight of quicklime and 20 parts by weight of gypsum were uniformly mixed, and then 0.2 parts by weight of retarder, 0.1 parts by weight of water reducer and 44 parts by weight of water were added, and the mixture was slowly stirred at 62±5 r / min for 20-30 s and then quickly stirred at 125±10 r / min for 60-90 s in a mixer to obtain cementitious material 3.
[0046] The initial setting time, final setting time, expansion and 2h compressive strength of the cementitious material are shown in Table 1.
[0047] Example 4
[0048] 100 parts by weight of aluminate cement, 20 parts by weight of quicklime and 2 parts by weight of gypsum were uniformly mixed, and then 0.6 parts by weight of retarder, 0.5 parts by weight of water reducer and 44 parts by weight of water were added, and the mixture was slowly stirred at 62±5 r / min for 20-30 s and then quickly stirred at 125±10 r / min for 60-90 s in a mixer to obtain cementitious material 4.
[0049] The initial setting time, final setting time, expansion and 2h compressive strength of the cementitious material are shown in Table 1.
[0050] Comparative Example 1
[0051] A comparative cementitious material 1 was prepared according to the method of Example 2, except that gypsum was not added and the amount of water added was adjusted so that the water-cement ratio was 0.36.
[0052] The initial setting time, final setting time, expansion and 2h compressive strength of the cementitious material are shown in Table 1.
[0053] Comparative Example 2
[0054] A comparative cementitious material 2 was prepared according to the method of Example 2 except that no retarder was added.
[0055] The initial setting time, final setting time, expansion and 2h compressive strength of the cementitious material are shown in Table 1.
[0056] Comparative Example 3
[0057] Comparative cementitious material 3 was prepared according to the method of Example 2, except that no water reducing agent was added and the amount of water added was adjusted so that the water-cement ratio was 0.6.
[0058] The initial setting time, final setting time, expansion and 2h compressive strength of the cementitious material are shown in Table 1.
[0059] Comparative Example 4
[0060] A comparative cementitious material 4 was prepared according to the method of Example 2, except that quicklime was not added and the amount of water added was adjusted so that the water-cement ratio was 0.36.
[0061] The initial setting time, final setting time, expansion and 2h compressive strength of the cementitious material are shown in Table 1.
[0062] Comparative Example 5
[0063] A comparative cementitious material 5 was prepared according to the method of Example 2, except that quicklime, gypsum and water reducing agent were not added and the amount of water added was adjusted so that the water-cement ratio was 0.6.
[0064] The initial setting time, final setting time, expansion and 2h compressive strength of the cementitious material are shown in Table 1.
[0065] Comparative Example 6
[0066] A comparative cementitious material 6 was prepared according to the method of Example 2, except that quicklime and retarder were not added and the amount of water added was adjusted so that the water-cement ratio was 0.36.
[0067] The initial setting time, final setting time, expansion and 2h compressive strength of the cementitious material are shown in Table 1.
[0068] Comparative Example 7
[0069] A comparative cementitious material 7 was prepared according to the method of Example 2, except that no retarder and water reducing agent were added and the amount of water added was adjusted so that the water-cement ratio was 0.6.
[0070] The initial setting time, final setting time, expansion and 2h compressive strength of the cementitious material are shown in Table 1.
[0071] Comparative Example 8
[0072] A comparative cementitious material 8 was prepared according to the method of Example 2, except that the weight of gypsum was adjusted to 30 and the amount of water added was adjusted so that the water-cement ratio was 0.36.
[0073] The initial setting time, final setting time, expansion and 2h compressive strength of the cementitious material are shown in Table 1.
[0074] Comparative Example 9
[0075] A comparative cementitious material 9 was prepared according to the method of Example 2, except that the weight of quicklime was adjusted to 1 and the amount of water added was adjusted so that the water-cement ratio was 0.36.
[0076] The initial setting time, final setting time, expansion and 2h compressive strength of the cementitious material are shown in Table 1.
[0077] Comparative Example 10
[0078] A comparative cementitious material 10 was prepared according to the method of Example 2, except that the weight of quicklime was adjusted to 30 and the amount of water added was adjusted so that the water-cement ratio was 0.36.
[0079] The initial setting time, final setting time, expansion and 2h compressive strength of the cementitious material are shown in Table 1.
[0080] Comparative Example 11
[0081] A comparative cementitious material 11 was prepared according to the method of Example 2 except that the weight portion of the retarder was adjusted to 0.7.
[0082] The initial setting time, final setting time, expansion and 2h compressive strength of the cementitious material are shown in Table 1.
[0083] Comparative Example 12
[0084] A comparative cementitious material 12 was prepared according to the method of Example 2 except that the weight portion of the water reducing agent was adjusted to 0.6.
[0085] The initial setting time, final setting time, expansion and 2h compressive strength of the cementitious material are shown in Table 1.
[0086] Table 1 Properties of cementitious materials prepared with different proportions of quicklime, gypsum, retarder, water reducer and aluminate cement
[0087]
[0088]
[0089] Note: Water-cement ratio refers to the mass ratio of water to cement + gypsum + quicklime.
[0090] It can be seen from Table 1 that the 2h compressive strength of the cementitious materials prepared in Examples 1-4 is greater than 1 MPa, and can reach up to 25.43 MPa. The initial setting time is 5-10 min, and the final setting time is 7-29 min. At the same time, the expansion is above 290 mm, and has high fluidity.
[0091] Compared with Example 2, Comparative Example 1 does not add gypsum, and the initial setting time of the comparative cementitious material 1 obtained is 2 minutes, and the final setting time is 5 minutes, which are significantly lower than the initial setting time and final setting time of Example 2. At the same time, the 2h compressive strength of the comparative cementitious material 1 is only 17.73MPa, which is significantly lower than 25.43MPa of Example 2. It is well known that gypsum as a retarder can usually prolong the initial setting time and final setting time of the cementitious material, and the 2h compressive strength will also decrease accordingly. However, by comparing Example 2 and Comparative Example 1, it can be found that in the present invention, due to the unexpected synergistic effect between gypsum and aluminate cement, quicklime and retarder, while the initial setting time and final setting time of the cementitious material are prolonged, the 2h compressive strength does not decrease, but is improved.
[0092] Compared with Example 2, Comparative Example 2 does not add a retarder, so that the initial setting time and final setting time of the comparative cementitious material 2 are greatly shortened, and the 2h compressive strength of the comparative cementitious material 2 is only 15.53MPa, which is significantly lower than 25.43MPa of Example 2. As mentioned above, a retarder can usually extend the initial setting time and final setting time of a cementitious material, and the 2h compressive strength will also decrease accordingly. However, by comparing Example 2 and Comparative Example 2, it can be found that in the present invention, due to the unexpected synergistic effect between the retarder and aluminate cement, quicklime and gypsum, while the initial setting time and final setting time of the cementitious material are extended, the 2h compressive strength does not decrease, but is improved.
[0093] Compared with Example 2, Comparative Example 3 does not add a water-reducing agent, so that the initial setting time and final setting time of the comparative cementitious material 3 are greatly prolonged. At the same time, the 2h compressive strength of the comparative cementitious material 3 is only 10.35 MPa, which is significantly lower than 25.43 MPa of Example 2.
[0094] The initial setting time and final setting time of the comparative cementitious materials prepared in Comparative Examples 4-9 and 11-12 are both greater than 120 min, and they do not have early strength.
[0095] The initial setting time and final setting time of the comparative cementitious material prepared in Comparative Example 10 were extremely short, and there was no time to test the expansion and 2h compressive strength.
[0096] The present invention has been described with reference to the embodiments and examples. However, the present invention is not limited to the aspects described in the above embodiments and examples, and various modifications may be made. However, it should be understood that it is possible for those skilled in the art to make various modifications and equivalent substitutions to the present invention without departing from the spirit and scope of the present invention. Therefore, the present invention is not limited to the specific embodiments described herein. More specifically, the scope of protection of the present invention is defined by the appended claims.
Claims
1. A method for preparing a high-fluidity early-strength gelling material, comprising the following steps: 100 parts by weight of aluminate cement, 2-20 parts by weight of quicklime and 0.1-20 parts by weight of gypsum are uniformly mixed, and then 0.01-0.6 parts by weight of retarder, 0.01-0.5 parts by weight of water reducer and appropriate amount of water are added to make the water-cement ratio 0.12-0.6, and the mixture is uniformly mixed to obtain a cementitious material.
2. The method according to claim 1, characterized in that: The gypsum is desulfurized gypsum.
3. The method according to claim 1 or 2, characterized in that: The retarder is an organic acid containing a carboxylate group, preferably tartaric acid.
4. The method according to any one of claims 1 to 3, characterized in that: The water reducer is one or more of a naphthalene-based water reducer, a polycarboxylate-based water reducer, and a lignin-based water reducer, preferably a polycarboxylate-based water reducer.
5. The method according to any one of claims 1 to 4, characterized in that: The initial setting time of the cementitious material is ≤10min, the final setting time is ≤30min, and the 2h compressive strength is ≥1MPa.
6. The method according to any one of claims 1 to 5, characterized in that: The expansion degree of the cementitious material is ≥290 mm.
7. The method according to any one of claims 1 to 6, characterized in that: The quicklime can be replaced by a high-calcium mineral, which is a mineral with a free calcium oxide content of 2-40 wt%, preferably high-calcium fly ash.
8. The method according to claim 7, characterized in that: The mass ratio of the aluminate cement to the high calcium mineral is (0.2-4):
1.
9. A high-fluidity early-strength gelling material prepared by the method according to any one of claims 1 to 8.
10. Application of the high-fluidity early-strength gelling material according to claim 9 as mine backfill material, grouting reinforcement material, mine water blocking material, and concrete 3D printing material.